Low-Raman-background coffee-ring-free aggregated nano-silver test chip and manufacturing method thereof

By using a combined structure of glass slides, metal base film layer and strong hydrophobic layer of fluorinated silica nanofilm on the Raman spectroscopy test chip, the problem of uneven distribution after drying of nano-silver film is solved, and efficient Raman spectroscopic signal enhancement and interference reduction significantly improves test speed and signal quality.

CN119044142APending Publication Date: 2024-11-29HAINING CHENYING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144247.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The spectral intensity of conventional Raman spectroscopy tests is weak, the test time is long, and the nano-silver film is unevenly distributed after drying, forming a coffee ring, resulting in serious spectral interference.

Method used

Design a low Raman background coffee-free ring-aggregated nanosilver test chip, using glass slides, metal base film layer and fluoride silica nanofilm strong hydrophobic layer, and preparing aluminum through vacuum evaporation and plasma sputtering technology The nano-silver colloid is aggregated by laser marking to avoid the coffee ring effect.

Benefits of technology

The Raman spectral signal intensity is improved, the test time is reduced, the spectral interference is reduced, and the high-quality Raman spectral signal is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044142A_ABST
    Figure CN119044142A_ABST
Patent Text Reader

Abstract

The invention provides a low-Raman-background coffee-ring-free aggregated nano-silver test chip and a manufacturing method thereof. The low-Raman-background coffee-ring-free aggregated nano-silver test chip comprises a glass slide, a metal bottom film layer and a fluorinated silicon dioxide nano-film strong hydrophobic layer, and the metal bottom film layer is located below the fluorinated silicon dioxide nano-film strong hydrophobic layer; the glass slide is positioned below the metal bottom film layer; when nano-silver colloid is dripped into the fluorinated silicon dioxide nano-film strong hydrophobic layer, a hydrophobic angle generated by the fluorinated silicon dioxide nano-film strong hydrophobic layer needs to be not less than 137 degrees, the coffee ring effect after the nano-silver colloid is dried is avoided by adopting the structure of the composite metal film and the strong hydrophobic layer, and the nano-silver colloid is gathered at a laser marking point. The chip is low in Raman background signal, improves the Raman spectrum signal intensity, accelerates the sample test speed, saves the characterization time, and provides a new thought for the spectrum test chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of optical technology, and in particular to a low Raman background coffee ring-free nanosilver aggregation test chip and a manufacturing method thereof. Background Art

[0002] For conventional Raman spectroscopy, the spectral intensity is weak, the test time is long, and a long time of spectral characterization is required. The existing technology uses nanosilver film technology for enhancement, but for conventional surface enhanced Raman chips, the nanosilver film is unevenly distributed after drying, often forming coffee rings, which cause serious spectral interference. This problem has always been a thorny issue in spectral testing. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a low Raman background coffee ring-free aggregated nanosilver test chip and a manufacturing method. Through a special structural design combined with an original use method, the nanosilver film is aggregated, the Raman spectrum signal intensity of the material is improved, the test speed is accelerated, the material characterization time is saved, and a high-quality Raman spectrum signal without coffee ring interference is obtained.

[0004] A low Raman background coffee ring-free nanosilver aggregation test chip and a manufacturing method, wherein:

[0005] A low Raman background and coffee ring-free nanosilver aggregation test chip, comprising:

[0006] A glass slide, a metal bottom film layer and a fluorinated silicon dioxide nanofilm strong hydrophobic layer, wherein the metal bottom film layer is located below the fluorinated silicon dioxide nanofilm strong hydrophobic layer; the glass slide is located below the metal bottom film layer; when nanosilver colloid is dripped into the fluorinated silicon dioxide nanofilm strong hydrophobic layer, the hydrophobic angle generated by the layer should be no less than 137 degrees.

[0007] As an example, after the nanosilver is dropped onto the chip, due to the presence of the strong hydrophobic layer of the fluorinated silica nanofilm, the nanosilver will not form a coffee ring after drying, but will gather at one point, which can further enhance its spectral characterization intensity.

[0008] As an example, the metal base film layer is: aluminum film.

[0009] As an example, the hydrophobic angle refers to the obtuse angle formed between the tangent line of the circle at the contact edge point on one side and the horizontal line of the point after the droplet contacts the strong hydrophobic layer of the fluorinated silica nanofilm when the nanosilver colloid is added.

[0010] A method for manufacturing a low Raman background coffee ring-free nanosilver aggregation test chip, comprising:

[0011] Step 1: Place the glass slide in anhydrous ethanol and perform ultrasonic treatment for five minutes, then take out the glass slide and place it in deionized water and perform ultrasonic treatment for five minutes; after taking it out again, use stable gas to blow dry for later use;

[0012] As an example, anhydrous ethanol and deionized water can be used to effectively remove organic matter and impurities on the surface of a glass slide through ultrasonic treatment.

[0013] As an example, the stabilizing gas is nitrogen.

[0014] As an example, the stabilizing gas may also be: an inert gas.

[0015] Step 2: Using vacuum evaporation method, a layer of aluminum film is spread on the surface of the glass slide;

[0016] As an example, the use of the aluminum film can ensure that when the Raman signal of the sample is detected, the Raman enhancement structure formed by the reflective structure of the aluminum film not only enables the excitation light to pass through the sample twice and generate two excitations, but also the Raman signal in the direction of the transmitted sample can also be reflected back to the Raman collection system through the aluminum film. These three Raman signals greatly improve the Raman signal-to-noise ratio of the system.

[0017] As an example, the thickness of the aluminum film is 25 nm.

[0018] As an example, the three Raman signals are:

[0019] ① The excitation light directly irradiates the sample, and the Raman signal is generated on the sample surface;

[0020] ② The excitation light penetrates the sample, and the excitation light that penetrates the sample is reflected by the aluminum film, irradiating the Raman signal generated on the sample surface;

[0021] ③The excitation light passes through the sample, and the Raman signal generated inside the sample is collected after reflection from the aluminum film.

[0022] Step 3: using a high-yield reaction method to prepare a fluorinated silicon dioxide nanofilm;

[0023] ① First, place 20nm silica particles in an appropriate amount of anhydrous ethanol solvent and place it in a sealed reactor;

[0024] ② Then, the sealed reactor is placed on a heated stirring table, and at the same time, hydrogen fluoride gas is slowly delivered to the sealed reactor through a gas delivery system, and the reaction temperature and pressure are gradually increased to promote the reaction rate and yield;

[0025] As an example, the reaction time is set to 2 hours.

[0026] As an example, the flow rate of the hydrogen fluoride gas is controlled to ensure the uniformity and safety of the reaction.

[0027] As an example, during the reaction, the reaction mixture is continuously stirred using a stirrer to ensure that the silicon dioxide is fully contacted with the hydrogen fluoride gas;

[0028] The reaction equations of the two are as follows:

[0029] SiO2+2HF→SiO2F2+H2O.

[0030] ③ After the reaction is completed, stop introducing hydrogen fluoride gas and cool the reactor to room temperature; filter the reaction mixture to separate the generated fluorinated silicon dioxide; and place the fluorinated silicon dioxide in anhydrous ethanol solvent to form a fluorinated silicon dioxide ethanol solvent, which is sealed and stored;

[0031] Step 4: Treat the aluminum film with a plasma sputtering method for a certain period of time to hydroxylate the surface of the aluminum film to form a hydrophilic state, and then put the fluorinated silica ethanol solvent into a nano-spray plating machine. Under a nitrogen atmosphere, set the nano-spray plating machine to have a consistent jet airflow direction to ensure uniform spray plating. After multiple spray platings, a layer of fluorinated silica nanostructure is generated on the aluminum film, which is used as a strong hydrophobic layer, that is, a fluorinated silica nanofilm strong hydrophobic layer.

[0032] As an example, when the nanosilver colloid is added to the strong hydrophobic layer of the fluorinated silicon dioxide nanofilm, due to the unique strong hydrophobic layer structure, no coffee ring will appear after the nanosilver colloid dries.

[0033] As an example, a laser marking method is used to mark uniform points on the strongly hydrophobic layer of the fluorinated silicon dioxide nanofilm as nanosilver aggregation points; nanosilver colloid is added dropwise, and after the nanosilver colloid is dried, the laser marked points are surface enhanced Raman spectroscopy test points.

[0034] As an example, the certain period of time is preferably 20 minutes.

[0035] Beneficial effects of the present invention:

[0036] This chip uses a composite metal film and a strong hydrophobic layer structure to avoid the coffee ring effect after the nanosilver colloid is dried, and the nanosilver colloid is concentrated at the laser marking point. This chip not only has a low Raman background signal, improves the Raman spectrum signal intensity, speeds up sample testing, saves characterization time, but also provides new ideas for spectral testing chips. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1This is a chip specification and dimension diagram of Example 1 of a low Raman background coffee ring-free aggregated nanosilver test chip of the present invention.

[0038] Figure 2 This is a side view of the chip structure of Example 1 of a low Raman background, coffee-ring-free aggregated nanosilver test chip of the present invention.

[0039] Figure 3 This is a schematic diagram of parameter testing of Example 1 of a low Raman background, coffee ring-free nanosilver aggregation test chip of the present invention.

[0040] Figure 4 Schematic diagram showing the difference between a conventional chip (B1) in the prior art and a chip (B2) of the present invention after multiple groups of nanosilver colloids are added to a low Raman background and coffee ring-free nanosilver test chip of the present invention.

[0041] Figure 5 This is a schematic diagram showing the difference between a conventional chip A in the prior art and a chip B of the present invention after a nanosilver colloid is added to a low Raman background and coffee ring-free nanosilver test chip of the present invention.

[0042] Figure 6 This is a Raman background signal data diagram of the chip of the present invention after adding nanosilver colloid to a low Raman background and coffee ring-free nanosilver test chip of the present invention.

[0043] Figure 7 This is a schematic diagram of the difference in Raman spectrum between a conventional chip in the prior art and the chip of the present invention using Rhodamine 6G to verify the low Raman background and coffee ring-free nanosilver test chip of the present invention. (The left figure A is a schematic diagram of the Raman spectrum of a common chip, and the right figure B is a schematic diagram of the Raman spectrum of the chip of Example 1 of the present invention). DETAILED DESCRIPTION

[0044] Below, reference Figures 1 to 7 As shown, a low Raman background coffee ring-free nanosilver aggregation test chip and a manufacturing method, wherein:

[0045] A low Raman background and coffee ring-free nanosilver aggregation test chip, comprising:

[0046] A glass slide, a metal bottom film layer and a fluorinated silicon dioxide nanofilm strong hydrophobic layer, wherein the metal bottom film layer is located below the fluorinated silicon dioxide nanofilm strong hydrophobic layer; the glass slide is located below the metal bottom film layer; when nanosilver colloid is dripped into the fluorinated silicon dioxide nanofilm strong hydrophobic layer, the hydrophobic angle generated by the layer should be no less than 137 degrees.

[0047] As an example, after the nanosilver is dropped onto the chip, due to the presence of the strong hydrophobic layer of the fluorinated silica nanofilm, the nanosilver will not form a coffee ring after drying, but will gather at one point, which can further enhance its spectral characterization intensity.

[0048] As an example, the metal base film layer is: aluminum film.

[0049] As an example, the hydrophobic angle refers to the obtuse angle formed between the tangent line of the circle at the contact edge point on one side and the horizontal line of the point after the droplet contacts the strong hydrophobic layer of the fluorinated silica nanofilm when the nanosilver colloid is added.

[0050] A method for manufacturing a low Raman background coffee ring-free nanosilver aggregation test chip, comprising:

[0051] Step 1: Place the glass slide in anhydrous ethanol and perform ultrasonic treatment for five minutes, then take out the glass slide and place it in deionized water and perform ultrasonic treatment for five minutes; after taking it out again, use stable gas to blow dry for later use;

[0052] As an example, anhydrous ethanol and deionized water can be used to effectively remove organic matter and impurities on the surface of a glass slide through ultrasonic treatment.

[0053] As an example, the stabilizing gas is nitrogen.

[0054] As an example, the stabilizing gas may also be: an inert gas.

[0055] Step 2: Using vacuum evaporation method, a layer of aluminum film is spread on the surface of the glass slide;

[0056] As an example, the use of the aluminum film can ensure that when the Raman signal of the sample is detected, the Raman enhancement structure formed by the reflective structure of the aluminum film not only enables the excitation light to pass through the sample twice and generate two excitations, but also the Raman signal in the direction of the transmitted sample can also be reflected back to the Raman collection system through the aluminum film. These three Raman signals greatly improve the Raman signal-to-noise ratio of the system.

[0057] As an example, the thickness of the aluminum film is 25 nm.

[0058] As an example, the three Raman signals are:

[0059] ① The excitation light directly irradiates the sample, and the Raman signal is generated on the sample surface;

[0060] ② The excitation light penetrates the sample, and the excitation light that penetrates the sample is reflected by the aluminum film, irradiating the Raman signal generated on the sample surface;

[0061] ③The excitation light passes through the sample, and the Raman signal generated inside the sample is collected after reflection from the aluminum film.

[0062] Step 3: using a high-yield reaction method to prepare a fluorinated silicon dioxide nanofilm;

[0063] ① First, place 20nm silica particles in an appropriate amount of anhydrous ethanol solvent and place it in a sealed reactor;

[0064] ② Then, the sealed reactor is placed on a heated stirring table, and at the same time, hydrogen fluoride gas is slowly delivered to the sealed reactor through a gas delivery system, and the reaction temperature and pressure are gradually increased to promote the reaction rate and yield;

[0065] As an example, the reaction time is set to 2 hours.

[0066] As an example, the flow rate of the hydrogen fluoride gas is controlled to ensure the uniformity and safety of the reaction.

[0067] As an example, during the reaction, the reaction mixture is continuously stirred using a stirrer to ensure that the silicon dioxide is fully contacted with the hydrogen fluoride gas;

[0068] The reaction equations of the two are as follows:

[0069] SiO2+2HF→SiO2F2+H2O.

[0070] ③ After the reaction is completed, stop introducing hydrogen fluoride gas and cool the reactor to room temperature; filter the reaction mixture to separate the generated fluorinated silicon dioxide; and place the fluorinated silicon dioxide in anhydrous ethanol solvent to form a fluorinated silicon dioxide ethanol solvent, which is sealed and stored;

[0071] Step 4: Treat the aluminum film with a plasma sputtering method for a certain period of time to hydroxylate the surface of the aluminum film to form a hydrophilic state, and then put the fluorinated silica ethanol solvent into a nano-spray plating machine. Under a nitrogen atmosphere, set the nano-spray plating machine to have a consistent jet airflow direction to ensure uniform spray plating. After multiple spray platings, a layer of fluorinated silica nanostructure is generated on the aluminum film, which is used as a strong hydrophobic layer, that is, a fluorinated silica nanofilm strong hydrophobic layer.

[0072] As an example, when the nanosilver colloid is added to the strong hydrophobic layer of the fluorinated silicon dioxide nanofilm, due to the unique strong hydrophobic layer structure, no coffee ring will appear after the nanosilver colloid dries.

[0073] As an example, a laser marking method is used to mark uniform points on the strongly hydrophobic layer of the fluorinated silicon dioxide nanofilm as nanosilver aggregation points; nanosilver colloid is added dropwise, and after the nanosilver colloid is dried, the laser marked points are surface enhanced Raman spectroscopy test points.

[0074] As an example, the certain period of time is preferably 20 minutes.

[0075] In order to better illustrate the design principle of the present invention, an example is given below using specific parameters:

[0076] Embodiment 1:

[0077] First, a glass slide A with a size of 12.5*7.5 cm was placed in anhydrous ethanol and deionized water, and ultrasonically treated for five minutes to remove organic matter and impurities on the glass surface, and then dried with nitrogen; see Figure 1 shown.

[0078] Secondly, a layer of aluminum film with a thickness of about 25 nm is spread on the surface of the glass slide by vacuum evaporation. When detecting Raman signals from samples, the Raman enhancement device with the aluminum film reflection structure not only enables the excitation light to pass through the sample twice to produce secondary excitation, but also the Raman signal in the transmission direction can be reflected back to the Raman collection system through the reflection coating, thereby improving the Raman signal-to-noise ratio of the system.

[0079] Then, fluorinated silicon dioxide is prepared by a reaction method with high yield;

[0080] Put silicon dioxide with a particle size of about 20 nm into an appropriate amount of anhydrous ethanol solvent, place it in a sealed reactor, and then place it on a heated stirring table. Slowly introduce hydrogen fluoride gas into the reactor through a gas delivery system, increase the reaction temperature and pressure to promote the reaction rate and yield, and the reaction time is 2 hours; control the flow rate of hydrogen fluoride gas to ensure the uniformity and safety of the reaction; during the reaction process, use a stirrer to continuously stir the reaction mixture to ensure that the silicon dioxide powder is fully in contact with the hydrogen fluoride gas;

[0081] The reaction equation is as follows:

[0082] SiO2+2HF→SiO2F2+H2O

[0083] After the reaction is completed, the introduction of hydrogen fluoride gas is stopped, and the reactor is cooled to room temperature. The reaction mixture is filtered to separate the generated fluorinated silicon dioxide. After separation, the fluorinated silicon dioxide is placed in anhydrous ethanol solvent and sealed for storage.

[0084] Finally, after the aluminum is fixed, it is treated with plasma sputtering for 20 minutes to hydroxylate the surface of the aluminum film and form a hydrophilic state. Then, the fluorinated silica ethanol solvent is placed in a nano-spray plating machine. In a nitrogen atmosphere, the jet airflow direction is set to be consistent to ensure uniform spray plating. The nozzle is set 10 cm above the chip and a suitable spray speed is set. After multiple spray plating, another layer of fluorinated silica nanostructure grows on the aluminum film. This structure forms a strong hydrophobic layer, and no coffee ring will appear when nanosilver colloid is added later. After the strong hydrophobic layer of the fluorinated silica nanofilm is fixed, laser marking is used to mark uniform points on the chip as nanosilver aggregation points. Nanosilver colloid is added, and after waiting for the nanosilver to dry, the laser-marked points are surface enhanced Raman spectroscopy test points.

[0085] After the above operation, a low Raman background and coffee ring-free nanosilver aggregation test chip can be obtained. The chip is 12.5 cm long, 7.5 cm wide, and 1 mm thick. Figure 2 shown.

[0086] The parameters of the low Raman background and coffee ring-free nanosilver test chip obtained in Example 1 were tested:

[0087] Can be obtained from Figure 3 It can be seen from the figure that after the chip obtained in Example 1 is dripped with nanosilver colloid, the hydrophobic angle it produces is 137.41°, which is close to 140°, and has good hydrophobic ability.

[0088] from Figure 4 It can be seen that after adding multiple groups of nanosilver colloids, the conventional chip (B1) of the prior art produces multiple groups of coffee ring effects, which is significantly different from the chip (B2) of the present invention that forms larger bottom bulges.

[0089] from Figure 5 It can be seen more clearly in the figure that after a group of nanosilver colloids are added, the conventional chip immediately becomes hydrophilic, forming a larger contact area, and produces a coffee ring effect after drying. However, the chip of the present invention, due to its strong hydrophobic structure, forms a smaller contact area and does not form a coffee ring effect. Instead, the nanosilver colloids are gathered at one point, further enhancing the Raman signal.

[0090] from Figure 6 It can be seen from the Raman background signal generated by the chip of the present invention that the background signal (interference) is relatively weak, and has the advantages of low background and strong stability.

[0091] A specific sample test was performed on a low Raman background, coffee ring-free nanosilver test chip obtained in Example 1;

[0092] The Hooke P300 confocal Raman detection platform was used to compare the enhancement effect of the chip of the present invention with that of the conventional chip.

[0093] Rhodamine 6G (Allura Red) is a commonly used food additive, and its conventional Raman spectrum has a strong fluorescence spectrum. This dye is used to compare and verify the chip obtained in Example 1 with a conventional chip;

[0094] from Figure 7 It can be seen that the left picture (conventional chip A) has a strong fluorescence background (interference), and its Raman peak cannot be seen; the right picture (chip B of Example 1) shows that the chip can obviously quench the fluorescence background, and the Raman peak is obvious;

[0095] The conventional chip in the left figure A has a weak enhanced signal strength due to the existence of the coffee ring effect. After using the chip of Example 1, due to the absence of the coffee ring effect, the enhanced signal strength is significantly enhanced, reaching nearly 5 times the value of the conventional chip. Therefore, the chip of Example 1 of the present invention can further enhance the signal strength on the basis of the existing technology and is suitable for promotion.

[0096] The above are only preferred embodiments of the present invention. It should be understood that the description of the above embodiments is only used to help understand the method and core ideas of the present invention, and is not used to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, etc. made within the ideas and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A low Raman background and coffee ring-free nanosilver test chip, characterized in that: include: A glass slide, a metal bottom film layer and a fluorinated silicon dioxide nanofilm strong hydrophobic layer, wherein the metal bottom film layer is located below the fluorinated silicon dioxide nanofilm strong hydrophobic layer; the glass slide is located below the metal bottom film layer; when nanosilver colloid is dripped into the fluorinated silicon dioxide nanofilm strong hydrophobic layer, the hydrophobic angle generated by the layer should be no less than 137 degrees.

2. The low Raman background coffee ring-free nanosilver test chip according to claim 1, characterized in that: The metal bottom film layer is: aluminum film.

3. The low Raman background and coffee ring-free nanosilver test chip according to claim 1, characterized in that: The hydrophobic angle refers to the obtuse angle formed between the tangent line of the circle at the contact edge point on one side and the horizontal line of the point after the droplet contacts the strong hydrophobic layer of the fluorinated silicon dioxide nanofilm when the nanosilver colloid is added dropwise.

4. A method for manufacturing a low Raman background coffee ring-free nanosilver test chip, characterized in that: include: Step 1: Place the glass slide in anhydrous ethanol and perform ultrasonic treatment for five minutes, then take out the glass slide and place it in deionized water and perform ultrasonic treatment for five minutes; after taking it out again, use stable gas to blow dry for later use; Step 2: Using vacuum evaporation method, a layer of aluminum film is spread on the surface of the glass slide; Step 3: using a high-yield reaction method to prepare a fluorinated silicon dioxide nanofilm; ① First, place 20nm silica particles in an appropriate amount of anhydrous ethanol solvent and place it in a sealed reactor; ② Then, the sealed reactor is placed on a heated stirring table, and at the same time, hydrogen fluoride gas is slowly delivered to the sealed reactor through a gas delivery system, and the reaction temperature and pressure are gradually increased to promote the reaction rate and yield; ③ After the reaction is completed, stop introducing hydrogen fluoride gas and cool the reactor to room temperature; filter the reaction mixture to separate the generated fluorinated silicon dioxide; and place the fluorinated silicon dioxide in anhydrous ethanol solvent to form a fluorinated silicon dioxide ethanol solvent, which is sealed and stored; Step 4: Treat the aluminum film with a plasma sputtering method for a certain period of time to hydroxylate the surface of the aluminum film to form a hydrophilic state, and then put the fluorinated silica ethanol solvent into a nano-spray plating machine. Under a nitrogen atmosphere, set the nano-spray plating machine to have a consistent jet airflow direction to ensure uniform spray plating. After multiple spray platings, a layer of fluorinated silica nanostructure is generated on the aluminum film, which is used as a strong hydrophobic layer, that is, a fluorinated silica nanofilm strong hydrophobic layer.

5. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 4, characterized in that: The stabilizing gas is one of nitrogen and inert gas.

6. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 4, characterized in that: The use of the aluminum film can ensure that when the Raman signal of the sample is detected, the Raman enhancement structure formed by the reflective structure of the aluminum film not only enables the excitation light to pass through the sample twice and generate two excitations, but also the Raman signal in the direction of the transmitted sample can be reflected back to the Raman collection system through the aluminum film. These three Raman signals greatly improve the Raman signal-to-noise ratio of the system.

7. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 6, characterized in that: The three Raman signals are: ① The excitation light directly irradiates the sample, and the Raman signal is generated on the sample surface; ② The excitation light penetrates the sample, and the excitation light that penetrates the sample is reflected by the aluminum film, irradiating the Raman signal generated on the sample surface; ③The excitation light passes through the sample, and the Raman signal generated inside the sample is collected after reflection from the aluminum film.

8. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 4, characterized in that: The thickness of the aluminum film is: 25 nm.

9. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 4, characterized in that: Use the laser marking method to mark uniform points on the strongly hydrophobic layer of the fluorinated silicon dioxide nanofilm as nanosilver aggregation points; add nanosilver colloid, wait for the nanosilver colloid to dry, and the laser marked points are surface enhanced Raman spectroscopy test points.

10. The method for manufacturing a low Raman background coffee ring-free nanosilver test chip according to claim 4, characterized in that: The certain period of time is: 20 minutes.