Active composition, lithium-embedded adhesive tape and preparation method of lithium-embedded adhesive tape
By using active compositions with 60-99% conductive agent and 0.5-30% adhesive in lithium batteries to form the active layer, the accumulation problem caused by inequality in lithium ion transmission of lithium batteries is solved, and the safety of lithium batteries is significantly improved performance.
Patent Information
- Application Number
- CN202411047847.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
AI Technical Summary
During the charging and discharging process of lithium batteries, lithium ions transmission is inequality, resulting in accumulation, and then the dendrite puncture diaphragm is precipitated, reducing the safety of lithium batteries.
The active composition is mainly made of conductive agents and adhesives to form an active layer, with conductive agents accounting for 60-99% and adhesives accounting for 0.5-30% in order to store excess lithium ions, inhibit lithium ions accumulation, and Improve lithium ion transmission efficiency.
Effectively alleviate lithium ion accumulation, avoid dendrites, and improve the safety performance of lithium batteries.
Smart Images

Figure BDA0004974270060000171 
Figure BDA0004974270060000172 
Figure BDA0004974270060000181
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to an active composition, a lithium-embedded adhesive tape and a preparation method thereof. Background Art
[0002] Lithium batteries have the advantages of high energy density, long cycle life and low self-discharge rate. They mainly rely on the movement of lithium ions between the positive and negative electrodes to store and release electrical energy.
[0003] Lithium batteries are often made by stacking and winding the positive electrode, separator and negative electrode, and then going through processes such as hot pressing, liquid injection and chemical formation. During the winding process of the electrode, the winding bending radius will continue to increase with the increase in the number of winding turns, and the bending area of the curved part of the electrode along the radial far end is much larger than the proximal end. During the charging and discharging process of the lithium battery, lithium ion transmission inequality is prone to occur, causing lithium ion accumulation, and even further precipitation to form dendrites and puncture the separator, resulting in lower safety of the lithium battery.
[0004] In view of this, this application is hereby filed. Summary of the invention
[0005] The present application provides an active composition, a lithium-embedded tape and a preparation method thereof, aiming to solve or at least improve the problem of lithium ion accumulation caused by unequal lithium ion transmission during the charging and discharging process of lithium batteries in the prior art.
[0006] The present application provides an active composition for forming an active layer in a lithium-embedded tape. The active composition is mainly made of a conductive agent and an adhesive as raw materials; wherein, by weight, the conductive agent is 60-99 parts, and the adhesive is 0.5-30 parts.
[0007] The present application designs the components and proportions of the active composition so that the active composition can form an active layer in the lithium-embedded tape. The active composition is mainly made of a conductive agent and an adhesive as raw materials. The introduction of 60-99 parts of the conductive agent by weight enables the active layer formed by the active composition to store excess lithium ions during the battery charging and discharging process to inhibit the accumulation of lithium ions at the interface of the electrode piece; 0.5-30 parts of the adhesive serve as a carrier of the conductive agent, allowing the conductive agent to be evenly distributed in the active layer formed by the active composition to improve the lithium storage capacity of the active layer. At the same time, 0.5-30 parts of the adhesive can also improve the adhesion of the active layer, so that the active layer can be closely attached to the surface of the electrode piece, so as to promote the transmission efficiency of lithium ions at the interface and further alleviate the accumulation of lithium ions at the interface of the electrode piece.
[0008] Therefore, the present application prepares an active composition by using 60-99 parts by weight of a conductive agent and 0.5-30 parts by weight of an adhesive as main raw materials. The active composition can form an active layer in a lithium-embedded tape, and the lithium-embedded tape can be directly adhered to the electrode. During the charging and discharging process of the lithium battery, excess lithium ions at the electrode interface can migrate to the active layer storage transition formed by the active composition in the lithium-embedded tape, thereby alleviating the accumulation of lithium ions caused by unequal transmission, avoiding the precipitation of lithium ions to form dendrites and puncture the diaphragm, and thereby significantly improving the safety performance of the lithium battery.
[0009] In some embodiments, the raw materials of the active composition further include: functional additives: 0.01-10 parts.
[0010] In some embodiments, the conductive agent comprises a granular conductive powder with a particle size of less than 1 μm; optionally, the conductive agent comprises at least one of graphite, hard carbon, conductive carbon black, carbon nanotubes or graphene; optionally, the graphite has a specific surface area in the range of 1-20 m 2 / g; Optionally, the hard carbon is selected from at least one of resin carbon, organic polymer pyrolytic carbon or carbon black, and the reversible specific capacity of the hard carbon is 500-700mAH; Optionally, the resistivity of the conductive carbon black is 0.8-1.8Ω·m, and the thermal volatile component is ≤0.8%; Optionally, the carbon nanotubes are single-walled or multi-walled carbon nanotubes.
[0011] In some embodiments, the adhesive is a pressure-sensitive hot-melt material, and the bonding temperature is 50-100°C; optionally, the adhesive includes at least one of a water-based adhesive or an oily adhesive; optionally, the water-based adhesive includes at least one of a polyolefin resin, an ethylene-vinyl acetate copolymer, an ethylene-acrylic acid copolymer, an ethylene-ethyl acrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-methacrylic acid copolymer or polyvinylidene fluoride; optionally, the oily adhesive includes at least one of a maleic anhydride-modified polypropylene resin, a polyester resin, a polyurethane thermoplastic elastomer, a polyacrylate resin or an ethylene-vinyl acetate copolymer.
[0012] In some embodiments, the functional additive includes at least one of a thickener, a dispersant or a defoamer; optionally, the thickener includes at least one of silica, cellulose, polyacrylic acid or polyether; optionally, the dispersant includes at least one of oily dispersants BYK-P 105, BYK-W96076, BYK-W969 or BYK-W980; optionally, the dispersant includes at least one of aqueous dispersants BYK-154, BYK-AT-250 or BYK-DISPERSANT-2152; optionally, the defoamer includes at least one of oily defoamers BYK-014, BYK-066N or BYK-1752; optionally, the defoamer includes at least one of aqueous defoamers BYK-012, BYK-024, BYK-039 or BYK-1640.
[0013] A second aspect of the present application provides a lithium-intercalated tape, comprising a substrate layer and an active layer formed by the above-mentioned active composition, wherein the active layer is supported on the substrate layer.
[0014] In some embodiments, the active layer has a porous structure; optionally, the active layer has a thickness of 5-100 μm; optionally, the substrate layer has a thickness of 5-50 μm; optionally, the substrate layer has a porosity of 30-85% and a pore size of ≤10 μm.
[0015] In some embodiments, the substrate layer is at least one of a polypropylene membrane, a polyethylene membrane, a polyimide membrane or a polyvinylidene fluoride membrane; optionally, the substrate layer is at least one of a polypropylene non-woven fabric, a polyethylene non-woven fabric, a polyester non-woven fabric or a polytetrafluoroethylene non-woven fabric.
[0016] In some embodiments, the lithium-embedded tape further comprises a conductive adhesive layer, which is loaded on a side of the active layer away from the substrate layer; optionally, the conductive adhesive layer has a thickness of less than 10 μm; optionally, the conductive adhesive layer is prepared from a raw material selected from a mixture of at least one of an aqueous emulsion, a polyacrylate resin, a rubber system, a polyurethane thermoplastic elastomer and an ethylene vinyl acetate copolymer and a conductive agent.
[0017] In some implementations, the mass fraction of the conductive agent in the conductive adhesive layer is 5-30%.
[0018] In some embodiments, the lithium-embedded tape further includes a release layer, which is disposed on a side of the substrate layer away from the active layer, or on a surface of the conductive adhesive layer; optionally, the release layer has a thickness of less than 1 μm.
[0019] The third aspect of the present application also provides a method for preparing the above-mentioned lithium-intercalated tape, comprising: uniformly mixing a conductive agent, an adhesive and a functional additive in a predetermined ratio and coating the mixture on a substrate layer to form an active layer to obtain a lithium-intercalated tape; or
[0020] In some embodiments, the preparation method of the lithium-embedded tape further includes: after forming the active layer, applying a mixture of a non-sticky adhesive and a conductive agent at room temperature to the side of the active layer facing away from the substrate layer to form a conductive adhesive layer to obtain the lithium-embedded tape; or after forming the active layer, applying a mixture of a sticky adhesive and a conductive agent at room temperature to the side of the active layer facing away from the substrate layer to form a conductive adhesive layer, and providing a release layer on the surface of the conductive adhesive layer, or applying a release agent to the side of the substrate layer facing away from the active layer to form a release layer to obtain the lithium-embedded tape. DETAILED DESCRIPTION
[0021] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0022] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0023] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0024] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0025] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may also include or contain other components not listed, or may only include or contain the listed components.
[0026] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0027] Based on the above, considering that the bending areas of the inner and outer sides of the bending part of the electrode after winding in the prior art are asymmetric, the lithium ions transmitted from the outside to the inside will form accumulation in the relatively smaller part on the inner side. The general inventive concept of the present application is to provide an active composition, which is made of raw materials such as a conductive agent and an adhesive, so that the active composition can form an active layer. After the active layer is loaded on the surface of the electrode, during the charging and discharging process of the lithium battery, the active layer can be used as a storage warehouse for lithium ions, and the excess lithium ions generated by the unequal transmission at the interface of the electrode are stored, thereby alleviating the accumulation of lithium ions at the interface of the electrode, avoiding the precipitation of lithium ions to form dendrites that pierce the diaphragm, and effectively improving the safety of the lithium battery.
[0028] Based on the above-mentioned general inventive concept, an embodiment of the present application provides an active composition for forming an active layer in a lithium-embedded tape, wherein the active composition is mainly made of a conductive agent and an adhesive as raw materials; wherein, in parts by weight, the conductive agent is 60-99 parts, and the adhesive is 0.5-30 parts.
[0029] It should be noted that the lithium-embedded tape in the embodiment of the present application is a special lithium battery tape, which can be used for electrode winding and pole piece protection in the middle production process of lithium battery cells (winding / stacking, shell welding and sealing processes, etc.).
[0030] It should be noted that in order to make the active layer formed by the active composition fully contact and fit with the pole piece, the active composition in this embodiment uses the substrate layer of the lithium-embedded tape as a carrier, and forms an active layer on the substrate layer of the lithium-embedded tape. By attaching the lithium-embedded tape to the pole piece and winding it together with the pole piece to form a lithium battery, the convenience of using the active composition is greatly improved. It should be understood that in some embodiments, the active composition can also directly form an active layer on the surface of the pole piece to store excess lithium ions on the pole piece interface during the charging and discharging process of the lithium battery.
[0031] In this embodiment, by designing the conductive agent to be 60-99 parts by weight and the adhesive to be 0.5-30 parts by weight, the active layer formed by the active composition can be sufficiently enriched with the conductive agent. The conductive agent can be evenly dispersed and filled in the adhesive to form an active layer with a porous structure, which is beneficial to improving the lithium storage capacity of the active layer and effectively storing excess lithium ions at the electrode interface during the lithium ion transmission process.
[0032] It should be understood that when the conductive agent in the raw materials of the active composition is less than 60 parts by weight, the active layer formed by the active composition has a poor lithium storage capacity and cannot effectively store excess lithium ions at the electrode interface; and when the adhesive is greater than 30 parts by weight, the air permeability of the active layer is poor, resulting in a low lithium ion transmission efficiency of the active layer, which is not conducive to the storage and transmission of lithium ions in the active layer.
[0033] For example, in the raw materials of the active composition of this embodiment, the conductive agent may be 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts, 98 parts, 99 parts or any part value or any part value range in the range of 60 to 99 parts; the adhesive can be 0.5 parts, 2 parts, 4.5 parts, 8 parts, 10.5 parts, 12 parts, 14.5 parts, 16 parts, 18.5 parts, 20 parts, 22.5 parts, 24 parts, 26.5 parts, 28 parts, 30 parts or any part value or any part value range in the range of 0.5 to 30 parts. In some embodiments, in order to improve the stability of the active composition when forming an active layer, the active composition further includes: functional additives: 0.01-10 parts. Functional additives are mainly used to regulate the fluidity of the active composition and the dispersibility of the conductive agent, and to improve the stability of the active composition in the process of forming an active layer. By introducing 0.01-10 parts by weight of the functional additives into the raw materials of the active composition, the active composition can have suitable fluidity. The active composition can be coated on the substrate layer of the lithium-embedded tape to stably form a more uniform active layer, and the conductive agent can be more evenly dispersed in the active layer to further improve the lithium storage capacity of the active layer.
[0034] For example, in the raw materials of the active composition in this embodiment, the functional additive can be 0.01, 0.05, 0.1, 0.6, 1.1, 1.6, 2.1, 2.6, 3.1, 4.1, 4.6, 5.1, 5.6, 6.1, 6.6, 7.1, 7.6, 8.1, 8.6, 9.1, 9.6, 10, or any value or range of values within the range of 0.01 to 10, by weight.
[0035] In addition, it should be noted that in the active composition of this embodiment, 60-99 parts by weight of conductive agent, 0.5-30 parts by weight of adhesive and 0.01-10 parts by weight of functional additives are reasonably proportioned, which is also beneficial to improving the adhesion of the active layer formed by the active layer composition to the carrier, so that the active layer is stably formed on the substrate layer of the lithium-embedded tape, avoiding cracking, falling off and other damage to the active layer after the lithium-embedded tape is wound with the pole piece, so as to ensure that the lithium storage capacity of the active layer is fully utilized.
[0036] In some embodiments, the conductive agent includes granular conductive powder with a particle size less than 1 μm. By using conductive powder with a particle size range less than 1 μm as the conductive agent, it is beneficial to promote the dispersion of the conductive agent in the adhesive and avoid the accumulation or agglomeration of the conductive agent during the formation of the active layer, thereby obtaining an active layer with a more uniform dispersion of the conductive agent.
[0037] In some embodiments, the conductive agent includes at least one of graphite, hard carbon, conductive carbon black, carbon nanotubes or graphene; the above substances as conductive agents have low resistivity, can effectively store lithium ions, and can transmit charges, thereby satisfying the lithium storage function of the active layer formed by the active composition.
[0038] It should be clarified that the graphite, hard carbon, conductive carbon black, carbon nanotubes, and graphene in this embodiment can be used as a conductive agent alone, or multiple types can be compounded into a mixed powder as a conductive agent. Compounding multiple types into a mixed powder as a conductive agent is beneficial to further improve the lithium ion storage capacity of the active layer formed by the active composition; for example, the conductive agent can be a mixed powder obtained by compounding hard carbon with at least one of graphite and conductive carbon black, wherein the mass ratio of hard carbon, graphite and conductive carbon black is (20-95):(0-70):(0-20).
[0039] In some preferred embodiments, the conductive agent is a mixed powder obtained by compounding at least two of graphite, conductive carbon black, carbon nanotubes and graphene with hard carbon, and the mass proportion of hard carbon in the conductive agent is 35% to 90%.
[0040] In some embodiments, the graphite has a specific surface area ranging from 1 to 20 m 2 / g, graphite has a larger specific surface area and smaller particle size. Using it as a conductive agent is beneficial to improving the conductive performance of the active layer, and at the same time enables the conductive agent to be fully dispersed in the active layer to form a more uniform active layer.
[0041] In some embodiments, the hard carbon is selected from at least one of resin carbon, organic polymer pyrolytic carbon or carbon black, and the reversible specific capacity of the hard carbon is 500-700mAH; the above substances have high reversible specific capacity as conductive agents, which can make the active layer have excellent conductivity and cycle stability, promote the transmission of electrons and ions in the active layer, and improve the lithium storage performance of the active layer.
[0042] It should be noted that the resin carbon in this embodiment is a carbon material prepared by carbonizing a resin or a polymer, and has the property of being difficult to be graphitized.
[0043] In some embodiments, the resistivity of the conductive carbon black is 0.8-1.8Ω·m, and the thermally volatile component is ≤0.8%; the conductive carbon black in the conductive agent has a lower resistivity, which is beneficial to the efficient transmission of lithium ions in the active layer, thereby improving the lithium storage capacity of the active layer. At the same time, the conductive carbon black has a lower thermally volatile component, which is beneficial to improving the thermal stability of the active layer during the battery charging and discharging process.
[0044] In some embodiments, the carbon nanotubes are single-walled or multi-walled carbon nanotubes, both of which have good electrical conductivity and mechanical stability, which are beneficial to exerting the lithium storage performance of the active layer while improving the stability of the active layer.
[0045] In some embodiments, the adhesive is a pressure-sensitive hot-melt material, and the bonding temperature is 50-100°C, which means that the active layer formed by the active composition is non-sticky at room temperature, and in the temperature range of 50-100°C, the active layer will soften and show its bonding properties, so that the active layer formed by the active composition can be directly hot-pressed onto the electrode at 50-100°C.
[0046] It should be noted that, in this embodiment, the adhesive is measured in dry weight at 0.5-30 parts by weight; before being combined with the conductive agent, the adhesive can be mixed with deionized water, organic solvents and other solvents to prepare a liquid adhesive with a solid content of 10-40%, so as to facilitate the uniform dispersion of the conductive agent; wherein the organic solvent includes at least one of toluene, xylene, methylcyclohexane, ethyl acetate, butyl acetate, butanone, methyl isobutyl ketone, ethanol, and isopropanol.
[0047] In some embodiments, the adhesive includes at least one of an aqueous adhesive or an oily adhesive; the adhesive in this embodiment can be an aqueous adhesive or an oily adhesive. When the adhesive is an aqueous adhesive, it can be mixed with deionized water to prepare a liquid adhesive with a solid content of 10-40%. When the adhesive is an oily adhesive, it can be mixed with an organic solvent to prepare a liquid adhesive with a solid content of 10-40%. Both can be used for dispersing the conductive agent to form a uniform active layer, and at the same time, the active layer has a certain adhesion to facilitate the bonding of the electrode or the substrate layer carrier of the lithium-embedded tape, so as to exert the lithium storage performance during the charging and discharging process of the lithium battery.
[0048] In some embodiments, the aqueous adhesive includes at least one of polyolefin resin, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer or polyvinylidene fluoride; the above substances as aqueous adhesives have good dispersibility for conductive agents and enable the active layer to be attached to the substrate layer carrier of the pole piece or lithium-embedded tape. Exemplarily, the polyolefin resin can be selected from at least one of polypropylene resin, amorphous α-olefin copolymer, ethylene-octene or ethylene-butene copolymer, maleic anhydride grafted polyolefin, acrylic acid grafted polyolefin, methacrylic acid grafted polyolefin, acrylic acid / methacrylic acid blended modified polyolefin.
[0049] In some embodiments, the aqueous adhesive further includes an optional tackifying resin, and the tackifying resin is selected from at least one of hydrogenated C5, hydrogenated C9 resin, hydrogenated C5 / C9 copolymer resin, hydrogenated DCPD, hydrogenated rosin, and hydrogenated polyterpene resin; the above substances as tackifying resins can adjust the viscosity of the aqueous adhesive to facilitate uniform dispersion of the conductive agent to form a uniform active layer.
[0050] In some embodiments, the oily adhesive includes at least one of maleic anhydride-modified polypropylene resin, polyester resin, polyurethane thermoplastic elastomer, polyacrylate resin or ethylene vinyl acetate copolymer; the above substances as oily adhesives have good dispersibility for conductive agents, and at the same time enable the active layer to adhere to the electrode or the substrate layer carrier of the lithium-embedded tape.
[0051] In some embodiments, the functional additive includes at least one of a thickener, a dispersant or a defoamer; it is understood that the thickener can improve the rheological properties of the active composition so that it can stably adhere to the substrate layer of the lithium-embedded tape during the formation of the active layer; the dispersant is beneficial to promote the dispersion of the conductive agent in the active layer, prevent the aggregation and deposition of the conductive agent particles, and promote the uniform mixing of the particles and the adhesive medium; the defoamer can reduce the surface tension of the active composition, destroy the formation of bubbles during the formation of the active layer, and avoid the bubbles from affecting the lithium storage performance of the active layer.
[0052] In some embodiments, the thickener includes at least one of silica, cellulose, polyacrylic acid or polyether; the above substances as thickeners can effectively regulate the rheological properties of the active composition.
[0053] In some embodiments, when the adhesive is an oily adhesive, the dispersant includes at least one of the oily dispersants BYK-P105, BYK-W96076, BYK-W969 or BYK-W980; the above substances as oily dispersants are beneficial to promote the dispersion of the conductive agent in the active layer, prevent the aggregation and deposition of the conductive agent particles, and promote the uniform mixing of the particles and the adhesive medium.
[0054] In some embodiments, when the adhesive is a water-based adhesive, the dispersant includes at least one of the water-based dispersants BYK-154, BYK-AT-250 or BYK-DISPERSANT-2152; the above substances as water-based dispersants are beneficial to promote the dispersion of the conductive agent in the active layer, prevent the aggregation and deposition of the conductive agent particles, and promote uniform mixing of the particles and the adhesive medium.
[0055] In some embodiments, when the adhesive is an oily adhesive, the defoaming agent includes at least one of the oily defoaming agents BYK-014, BYK-066N or BYK-1752; the above substances as oily defoaming agents can reduce the surface tension of the active composition, destroy the formation of bubbles in the process of forming the active layer, and avoid the bubbles from affecting the lithium storage performance of the active layer.
[0056] In some embodiments, when the adhesive is an aqueous adhesive, the defoaming agent includes at least one of aqueous defoaming agents BYK-012, BYK-024, BYK-039 or BYK-1640 as an aqueous defoaming agent, which can reduce the surface tension of the active composition, destroy bubble formation during the formation of the active layer, and avoid the bubbles from affecting the lithium storage performance of the active layer.
[0057] Another embodiment of the present application provides a lithium-intercalated tape, which includes a substrate layer and an active layer formed by the above-mentioned active composition, wherein the active layer is loaded on the substrate layer.
[0058] In this embodiment, the lithium-embedded tape includes a substrate layer and an active layer formed by an active composition. The substrate layer serves as a carrier of the active layer and can be loaded on its surface. During the use of the lithium-embedded tape, the active layer of the lithium-embedded tape can be directed to the surface of the negative electrode sheet. The lithium-embedded tape and the negative electrode sheet can be tightly fitted by hot pressing. After the negative electrode sheet with the lithium-embedded tape attached to the surface is wound into a lithium battery, the lithium-embedded tape can be used as a "lithium storage warehouse" to store excess lithium ions at the interface of the electrode sheet during the charging and discharging process of the lithium battery to avoid lithium ion accumulation, thereby improving the safety performance of the lithium battery.
[0059] In some embodiments, the active layer has a porous structure and has excellent air permeability, so as to promote the transmission efficiency of lithium ions in the active layer and improve the lithium storage performance of the active layer; the thickness of the active layer in this embodiment is 5-100 μm. Within this thickness range, the active layer can provide sufficient lithium storage capacity and electrochemical reaction surface area while maintaining high air permeability and ion transmission rate.
[0060] In some embodiments, the thickness of the substrate layer is 5 to 50 μm. By designing the thickness of the substrate layer to be within the above range, the substrate layer can provide effective support for the active layer to ensure the stability and uniformity of the active layer attached to the substrate layer. In some embodiments, the porosity of the substrate layer is 30-85%, and the pore size is ≤10 μm; by designing the porosity and pore size of the substrate layer to be within the above range, the substrate layer can have excellent air permeability, which is beneficial to promote the diffusion and transmission of lithium ions. In some embodiments, the substrate layer is at least one of a polypropylene (PP) diaphragm, a polyethylene (PE) diaphragm, a polyimide (PI) diaphragm, and a polyvinylidene fluoride (PVDF) diaphragm; the above substances as the substrate layer of the lithium-embedded tape can effectively load the active layer, so that the active layer is stably formed on the substrate layer.
[0061] In some embodiments, the substrate layer is at least one of polypropylene (PP) non-woven fabric, polyethylene (PE) non-woven fabric, polyester (PET) non-woven fabric and polytetrafluoroethylene (PTFE) non-woven fabric; the above materials as the substrate layer of the lithium-embedded tape can effectively load the active layer, so that the active layer is stably formed on the substrate layer.
[0062] In some embodiments, the lithium-embedded tape further includes a conductive adhesive layer, which is loaded on a side of the active layer away from the substrate layer; by further designing a conductive adhesive layer on the active layer, the bonding performance of the lithium-embedded tape can be further improved, so that the lithium-embedded tape can be closely attached to the surface of the electrode, thereby enabling the lithium storage performance of the lithium-embedded tape to be effectively exerted.
[0063] It can be understood that when the mass ratio of the adhesive to the conductive agent in the active layer is relatively high, for example, when the mass ratio is above 1:10, the active layer has good lithium storage performance and good hot pressing bonding performance, and can be stably bonded to the surface of the electrode; when the mass ratio of the adhesive to the conductive agent in the active layer is relatively low, for example, below 1:10, the adhesive is mainly used for bonding between the conductive agents, and the hot pressing bonding performance of the active layer is weak. At this time, a conductive adhesive layer needs to be provided on the surface of the active layer to achieve stable bonding to the surface of the electrode.
[0064] In some embodiments, the conductive adhesive layer is sticky or non-sticky at room temperature. The conductive adhesive layer is sticky at room temperature, so that the lithium-embedded tape can be directly and tightly attached to the surface of the pole piece through the conductive adhesive layer at room temperature; the conductive adhesive layer is non-sticky at room temperature, which is conducive to the storage and transportation of the lithium-embedded tape. When in use, the lithium-embedded tape can be tightly attached to the surface of the pole piece through a hot pressing process.
[0065] In some embodiments, the thickness of the conductive adhesive layer is less than 10 μm. By designing the thickness of the conductive adhesive layer, it is helpful to reduce the interface impedance between the lithium-embedded tape and the electrode, so that excess lithium ions at the electrode interface can quickly migrate to the active layer through the conductive adhesive layer for storage.
[0066] In some embodiments, the conductive adhesive layer is patterned and covered on the surface of the active layer to form a discontinuous conductive adhesive layer, wherein the conductive adhesive layer covers an area of 10-50% of the total area of the active layer. The pattern includes at least one of a dot-shaped spacing pattern, a linear spacing pattern, and a grid pattern. By patterning the conductive adhesive layer, the effect of the conductive adhesive layer on the air permeability of the lithium-embedded tape can be reduced, thereby improving the transmission efficiency of lithium ions.
[0067] In some embodiments, the raw materials for preparing the conductive adhesive layer are selected from a mixture of at least one of aqueous emulsion, polyacrylate resin, rubber system, polyurethane thermoplastic elastomer (TPU) and ethylene vinyl acetate copolymer (EVA) and a conductive agent; all of the above substances can effectively form a conductive adhesive layer on the surface of the active layer to improve the bonding performance of the lithium-embedded tape.
[0068] In some embodiments, the mass fraction of the conductive agent in the conductive adhesive layer is 5-30%. By adding a proper amount of conductive agent to the conductive adhesive layer, the conductivity of the conductive adhesive layer can be increased while maintaining the bonding performance, thereby improving the transmission efficiency of lithium ions.
[0069] In some embodiments, the type of aqueous emulsion in the conductive adhesive layer is the same as the type of aqueous adhesive in the active layer, and the type of conductive agent in the conductive adhesive layer is the same as the type of conductive agent in the active layer, that is, graphite, hard carbon, conductive carbon black, carbon nanotubes, and graphene can be used alone as conductive agents, or multiple types can be compounded into a mixed powder as a conductive agent.
[0070] In some embodiments, the lithium-embedded tape further includes a release layer, which is disposed on the side of the substrate layer away from the active layer, or on the surface of the conductive adhesive layer. Since the lithium-embedded tape is often stored and transported by being rolled into a tape roll, when the adhesive layer is sticky at room temperature, it is easy to adhere to the substrate layer during the rolling process, causing damage to the structure of the lithium-embedded tape; in the case where the conductive adhesive layer described in this embodiment is sticky at room temperature, a release layer is also disposed on the side of the substrate layer away from the active layer, or a release layer is disposed on the surface of the conductive adhesive layer, and the thickness of the release layer is less than 1 μm; by designing the release layer, during the rolling process of the lithium-embedded tape, the two sides of the conductive adhesive layer along the thickness direction can contact the active layer and the release layer respectively, so as to avoid the conductive adhesive layer directly adhering to the substrate layer and causing damage to the structure of the lithium-embedded tape.
[0071] Another embodiment of the present application further provides a method for preparing the lithium-intercalated tape, comprising: uniformly mixing a conductive agent, an adhesive and a functional additive in a predetermined ratio and coating the mixture on a substrate layer to form an active layer to obtain the lithium-intercalated tape.
[0072] In some embodiments, after the active layer is formed, a mixture of a non-sticky adhesive and a conductive agent at room temperature is applied to the side of the active layer facing away from the substrate layer to form a conductive adhesive layer to obtain a lithium-embedded tape; or after the active layer is formed, a mixture of an adhesive and a conductive agent that is sticky at room temperature is applied to the side of the active layer facing away from the substrate layer to form a conductive adhesive layer, and a release layer is provided on the surface of the conductive adhesive layer, or a release agent is applied to the side of the substrate layer facing away from the active layer to form a release layer to obtain a lithium-embedded tape.
[0073] It should be understood that the lithium-embedded tape provided in this embodiment can be directly attached to one or both sides of the negative electrode sheet in the thickness direction, and can be wound together with the positive electrode, separator and other components to form a lithium battery. The lithium-embedded tape designed with a release layer in this embodiment can be directly attached to the surface of the electrode sheet without a hot pressing process because the conductive adhesive layer is sticky at room temperature, while the lithium-embedded tape without a release layer needs to be attached to the surface of the electrode sheet under hot pressing conditions, which makes the application scenarios of the lithium-embedded tape more flexible and diversified.
[0074] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0075] Example 1
[0076] 30 parts of hard carbon, 60 parts of graphite, 9 parts of conductive carbon black, 100 parts of homemade emulsion (containing 30 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.3 parts of functional additives (containing 2 parts of thickener, 0.1 parts of aqueous dispersant and 0.2 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 30 μm to obtain a lithium-embedded tape.
[0077] Example 2
[0078] 88 parts of hard carbon, 10 parts of graphite, 1 part of conductive carbon black, 3 parts of homemade emulsion (containing 0.9 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.009 parts of functional additives (containing 2 parts of thickener, 0.003 parts of aqueous dispersant and 0.006 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 40 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade emulsion, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0079] Example 3
[0080] 88 parts of hard carbon, 10 parts of graphite, 1 part of conductive carbon black, 12.5 parts of homemade polyacrylate resin (including 5 parts of hydroxyl / carboxyl terminated acrylic resin), 100 parts of organic solvent, and 0.05 parts of functional additives (including 0.04 parts of oily dispersant and 0.01 parts of oily defoaming agent) are mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 9 μm to form an active layer with a thickness of 35 μm. Conductive carbon black with a mass fraction of 15% is added to the homemade emulsion, mixed evenly, and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounts for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0081] Example 4
[0082] 88 parts of hard carbon, 10 parts of graphite, 1 part of conductive carbon black, 3 parts of homemade emulsion (containing 0.9 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.009 parts of functional additives (containing 2 parts of thickener, 0.003 parts of aqueous dispersant and 0.006 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 9 μm to form an active layer with a thickness of 35 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade emulsion, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0083] Example 5
[0084] 72 parts of hard carbon, 26 parts of graphite, 1 part of multi-walled carbon nanotubes, 4.5 parts of homemade emulsion (including 1.35 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.0135 parts of functional additives (including 2 parts of thickener, 0.0045 parts of aqueous dispersant and 0.009 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 35 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade emulsion, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0085] Example 6
[0086] 94 parts of hard carbon, 4 parts of graphite, 1 part of graphene, 3 parts of homemade emulsion (containing 0.9 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.009 parts of functional additives (containing 2 parts of thickener, 0.003 parts of aqueous dispersant and 0.006 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 um to form an active layer with a thickness of 35 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade polyacrylate resin, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer. A release agent was coated on the side of the polypropylene diaphragm away from the active layer to form a release layer with a thickness of less than 0.5 μm to obtain a lithium-embedded tape.
[0087] Example 7
[0088] 76 parts of hard carbon, 8 parts of graphite, 1 part of conductive carbon black, 45 parts of homemade emulsion (containing 13.5 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.135 parts of functional additives (containing 2 parts of thickener, 0.045 parts of aqueous dispersant and 0.09 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 um to form an active layer with a thickness of 35 μm to obtain a lithium-embedded tape.
[0089] Example 8
[0090] 88 parts of hard carbon, 10 parts of conductive carbon black, 45 parts of homemade emulsion (containing 13.5 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.135 parts of functional additives (containing 2 parts of thickener, 0.045 parts of aqueous dispersant and 0.09 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 35 μm to obtain a lithium-embedded tape.
[0091] Comparative Example 1
[0092] 30 parts of hard carbon, 60 parts of graphite, 9 parts of conductive carbon black, 130 parts of homemade emulsion (including 39 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.12 parts of functional additives (including 2 parts of thickener, 0.04 parts of aqueous dispersant and 0.08 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 30 μm to obtain a lithium-embedded tape.
[0093] Comparative Example 2
[0094] 88 parts of hard carbon, 10 parts of graphite, 1 part of conductive carbon black, 160 parts of homemade emulsion (including 48 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.15 parts of functional additives (including 2 parts of thickener, 0.05 parts of aqueous dispersant and 0.1 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 40 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade emulsion, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0095] Comparative Example 3
[0096] 30 parts of hard carbon, 20 parts of graphite, 100 parts of homemade emulsion (containing 30 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.3 parts of functional additives (containing 2 parts of thickener, 0.1 parts of aqueous dispersant and 0.2 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 20 μm to form an active layer with a thickness of 35 μm to obtain a lithium-embedded tape.
[0097] Comparative Example 4
[0098] 88 parts of hard carbon, 20 parts of conductive carbon black, 3 parts of homemade emulsion (containing 0.9 parts of maleic anhydride grafted polypropylene), 100 parts of deionized water, and 2.009 parts of functional additives (containing 2 parts of thickener, 0.003 parts of aqueous dispersant and 0.006 parts of aqueous defoaming agent) were mixed evenly and coated on the surface of a polypropylene diaphragm with a thickness of 9 μm to form an active layer with a thickness of 40 μm. Conductive carbon black with a mass fraction of 15% was added to the homemade emulsion, mixed evenly and sprayed on the surface of the active layer to form a conductive adhesive layer with a thickness of less than 1 μm. The coverage area of the conductive adhesive layer accounted for 30% of the total area of the active layer, thereby obtaining a lithium-embedded tape.
[0099] It should be noted that the homemade emulsions in the above-mentioned embodiments and comparative examples are prepared by using existing emulsion preparation technology, and the preparation process is as follows: maleic anhydride grafted polypropylene (water-based adhesive), deionized water and emulsifier are used as main raw materials, the components are mixed and stirred, high-speed shearing is performed, and a water-based homemade emulsion is obtained after distillation treatment; wherein, the solid content of the homemade emulsion is 30%, and the particle size D50 of the latex particles is 0.5-5μm.
[0100] The preparation process of the self-made polyacrylate resin in the above embodiments and comparative examples is as follows: by mass fraction, 98-99% of hydroxyl / carboxyl terminated acrylate resin (molecular weight of 100,000-1,000,000) and 1-2% of curing agent (selected from multifunctional epoxy resin) are used as main raw materials, and the self-made polyacrylate resin is prepared by thermal initiation method; wherein, the hydroxyl / carboxyl terminated acrylate resin is an oily adhesive polyacrylate resin, and the solid content of the self-made polyacrylate resin is 40%. In the above embodiments and comparative examples, the functional additives include thickeners, dispersants and defoamers, wherein the functional additives corresponding to the aqueous adhesive system are carboxymethyl cellulose thickeners, BYK-154 dispersants (aqueous dispersants) and BYK-024 defoamers (aqueous defoamers); the functional additives corresponding to the oily adhesive system are oily dispersants BYK-W969 and oily defoamers BYK-066N. In addition, the organic solvent in the above embodiments and comparative examples is toluene.
[0101] The structures and components of the lithium-embedded tapes obtained in Examples 1 to 8 and Comparative Examples 1 to 4 are shown in Tables 1 and 2 below:
[0102] Table 1: Statistical table of structure and component data of lithium-embedded tapes in various embodiments
[0103]
[0104] Table 2. Comparative Examples of Lithium-embedded Tapes Lithium-embedded Tape Structure and Component Data Statistics
[0105]
[0106]
[0107] In order to verify the performance of the lithium-intercalated tapes prepared in the above embodiments, the lithium-intercalated tapes prepared in embodiments 1 to 8 and comparative examples 1 to 4 were tested for performance respectively, and the test method is as follows:
[0108] Peeling force test (before soaking): cut the lithium-embedded tape into strips with a width of 20 mm and a length of 100 mm; stick a double-sided tape with a width of 30 mm on the surface of the stainless steel plate, and then stick the active layer or the conductive adhesive layer of the lithium-embedded tape strip toward the double-sided tape, and use a 2kg pressure wheel to reciprocate and roll the substrate layer of the lithium-embedded tape strip three times at a speed of 300 mm / min. After rolling, cure for 20 minutes; fix one end of the stainless steel plate on the first clamp of the tensile testing machine and perpendicular to the horizontal plane. The second clamp of the tensile testing machine clamps the substrate layer of the tape strip, and performs a peeling test at a speed of 304.8 mm / min. Select a section with stable data (not shorter than 80 mm) for peeling force calculation.
[0109] Peeling force test (after soaking): Place the lithium-embedded tape specimens cut in the above peeling force test (before soaking) into a container filled with electrolyte solvent and cover the liquid surface. After sealing and baking at 85°C for 24 hours, take out the lithium-embedded tape specimens, wipe off the surface solvent and then test. The subsequent test steps are the same as the peeling force test (before soaking).
[0110] Air permeability test (before soaking): Use an air permeability tester to perform an air permeability test. Cut the lithium-embedded tape into circular films with a diameter of >10cm; turn on the air permeability tester switch, and hold the slide barrel against the top of the slide barrel; rotate the slide barrel, and the infrared probe is perpendicular to the central axis of the 100ml test area; place the film to be tested on the test seat and tighten it; the screen displays "TIMERSEEKING STARTING MARK", press the "RESET" key and release the slide barrel to start the test; after the test is completed, read the value on the screen, the unit is s / 100cc.
[0111] Air permeability test (after soaking): put the lithium-embedded tape film obtained by the above air permeability test (before soaking) into a container filled with electrolyte solvent and cover the liquid surface, seal it and bake it at 85℃ for 24h, then take it out and wipe off the surface solvent. The subsequent test steps are the same as the air permeability test (before soaking).
[0112] Volume resistivity test: measure the overall thickness of the lithium-embedded tape several times, take the average of three times and subtract the substrate thickness, record the thickness as t (μm), cut the lithium-embedded tape into long strips with a width of 1-2 mm, record the width as W (mm), place the strips on the four-corner probe test fixture of the multi-function measuring instrument, ensure that each antenna is in good contact with the sample, wait for the instrument to display the reading, record it as R (Ω), and record the length between the inner probe pairs as L (mm); calculate the volume resistivity (Ω·cm) by the following formula:
[0113] (Ω·cm)=R*(W*t)*10-4 / L.
[0114] The test data of the lithium-embedded tapes obtained in Examples 1 to 8 and Comparative Examples 1 to 4 were statistically analyzed, and the statistical results are shown in Table 3 and Table 4 below:
[0115] Table 3. Statistical table of test data of lithium-embedded tapes in various embodiments
[0116]
[0117] Table 4. Statistical table of test data of lithium-embedded tapes in various comparative examples
[0118]
[0119]
[0120] It should be noted that "s / 100cc" in Tables 3 and 4 refers to the time (in seconds) required for a unit area of material to pass 100cc of gas under certain conditions. It is used to characterize the degree of gas permeability of an object or material. The lower the value, the better the air permeability, which is more conducive to the lithium ion transmission capacity and conductivity.
[0121] It can be seen from Tables 1 to 4 above that, compared with Comparative Examples 1 to 4, the lithium-embedded tapes prepared in Examples 1 to 8 all have good air permeability and low volume resistivity, and the comprehensive air permeability of the lithium-embedded tape before and after soaking changes little, reflecting that the lithium-embedded tape has good lithium ion transmission ability and conductivity, so that during the lithium battery cycle, lithium ions can be effectively transmitted to the active layer of the lithium-embedded tape for storage, so as to avoid accumulation on the surface of the electrode, thereby improving the safety performance of the lithium battery; at the same time, in the lithium-embedded tapes prepared in Examples 1 to 8, the active layer and the substrate layer have a large peeling force, and the active layer and the substrate layer are tightly bonded to ensure that the lithium-embedded tape has excellent stability in the lithium battery, so that the lithium storage performance of the active layer can be fully utilized. In Examples 1, 7 and 8, the adhesive content in the active layer is relatively high, so that the active layer has good heat-activated adhesive properties, can be directly attached to the surface of the pole piece relatively stably, and the structure of the prepared lithium-embedded tape is relatively simple; in Examples 2-6, the adhesive content in the active layer is relatively low, and a conductive adhesive layer needs to be provided on the surface of the active layer to make the lithium-embedded tape more stably attached to the surface of the pole piece. Although the structure of the prepared lithium-embedded tape is relatively complex, it has excellent lithium storage performance. The structure of the lithium-embedded tape of the present invention is relatively flexible and can be selected according to actual work needs.
[0122] Specifically, compared with Example 1, in the active layer components of Comparative Example 1, the weight portion of the adhesive (maleic anhydride grafted polypropylene) is 39 parts, and the proportion of the adhesive is too large, far exceeding 30 parts by weight. Under the same air permeability of the substrate layer, the air permeability of the active layer formed in Comparative Example 1 is significantly increased, the air permeability of the active layer is poor, and the comprehensive air permeability of the lithium-embedded tape before and after the soaking is too large. At the same time, the volume resistivity of the lithium-embedded tape is too high, which is 6.78Ω·cm, which is much higher than the volume resistivity of the lithium-embedded tape prepared in Example 1, indicating that the lithium-ion transmission capacity and conductivity of the lithium-embedded tape in Comparative Example 1 are poor; while the active layer component of Example 1 Among them, the conductive agent is 99 parts, the adhesive (maleic anhydride grafted polypropylene) is 30 parts, the active layer of the prepared lithium-embedded tape has low air permeability and good air permeability, the comprehensive permeability of the lithium-embedded tape before and after soaking is small, and the volume resistivity of the lithium-embedded tape is 1.28Ω·cm, which is much lower than that of comparative example 1, reflecting that the lithium-embedded tape has better lithium ion transmission ability and conductive performance; in addition, the peeling force between the active layer and the substrate layer of comparative example 1 is significantly reduced after soaking compared with that of embodiment 1, the bonding tightness between the active layer and the substrate layer is poor, the stability of the lithium-embedded tape in the lithium battery is low, which is not conducive to the effective use of the lithium storage performance of the active layer.
[0123] Furthermore, compared with Example 1, in the active layer components of Comparative Example 3, the weight fraction of the conductive agent is 50 parts, and the weight fraction of the conductive agent is much lower than 60 parts. Under the condition that the air permeability of the substrate layer is the same, the air permeability of the active layer formed in Comparative Example 3 is significantly increased, the air permeability of the active layer is poor, and the comprehensive air permeability change of the lithium-embedded tape before and after soaking is 173.7s / 100cc, and the comprehensive air permeability change is too large. At the same time, the volume resistivity of the lithium-embedded tape is too high, which is 37.45Ω·cm, which is much higher than the volume resistivity of the lithium-embedded tape prepared in Example 1. The peeling force between the active layer and the substrate layer is severely attenuated after soaking, indicating that the lithium-ion transmission capacity and conductivity of the lithium-embedded tape in Comparative Example 3 are poor, and the bonding tightness between the active layer and the substrate layer is poor. Therefore, by designing the conductive agent to be 60-99 parts by weight and the adhesive to be 0.5-30 parts by weight, the active layer formed by the active composition can be sufficiently enriched with the conductive agent, and the conductive agent can be evenly dispersed and filled in the adhesive to form an active layer with a porous structure, which is beneficial to improving the lithium storage capacity of the active layer and improving the adhesion of the active layer formed by the active layer composition to the carrier, so as to effectively store the excess lithium ions at the electrode interface during the lithium ion transmission process while maintaining high stability.
[0124] Furthermore, compared with Example 2, in the active layer components of Comparative Example 4, the weight fraction of the conductive agent is 108 parts, and the weight fraction of the conductive agent is much higher than 100 parts. The proportion of the conductive agent is too high, and the peeling force between the active layer and the substrate layer in the obtained lithium-embedded tape is extremely poor. After the lithium-embedded tape is wound with the pole piece, the active layer is damaged by cracking, falling off, etc., which is not conducive to the full play of the lithium storage capacity of the active layer; and, in the components of the active layer of Comparative Example 4, due to the excessive proportion of the conductive agent, the bonding conditions with the pole piece are more stringent, requiring 110°C 1MPa 2min, and it is more difficult to bond with the pole piece. In contrast, the bonding conditions of the lithium-embedded tape obtained in Example 2 with the pole piece are 90°C 0.5MPa 2s, it is explained that the conductive agent is designed to be 60-99 parts by weight and the adhesive is designed to be 0.5-30 parts by weight, so that the active layer formed by the active composition can be sufficiently enriched with the conductive agent, and the conductive agent can be evenly dispersed and filled in the adhesive to form an active layer with a porous structure, which is beneficial to improve the lithium storage capacity of the active layer and improve the adhesion of the active layer formed by the active layer composition to the carrier, so as to effectively store the excess lithium ions at the electrode interface during the lithium ion transmission process while maintaining high stability.
[0125] Furthermore, in Example 2, compared with Example 2, in the active layer components of Example 2, the weight portion of the adhesive (maleic anhydride grafted polypropylene) is 48 parts, and the proportion of the adhesive is too large, far exceeding 30 parts by weight. Under the same air permeability of the substrate layer, the air permeability of the active layer formed in Example 2 is significantly increased, the air permeability of the active layer is poor, and the comprehensive air permeability of the lithium-embedded tape before and after the soaking is too large. At the same time, the volume resistivity of the lithium-embedded tape is too high, which is 13.53Ω·cm, which is much higher than the volume resistivity of the lithium-embedded tape prepared in Example 2, indicating that the lithium-ion transmission capacity and conductivity of the lithium-embedded tape in Example 2 are poor; while the active layer of Example 2 Among the components, the conductive agent is 99 parts, and the adhesive (maleic anhydride grafted polypropylene) is 0.9 parts. The active layer of the prepared lithium-embedded tape has low air permeability and good air permeability. The comprehensive air permeability of the lithium-embedded tape before and after soaking is small, and the volume resistivity of the lithium-embedded tape is 0.31Ω·cm, which is much lower than that of Comparative Example 2, reflecting that the lithium-embedded tape has better lithium ion transmission ability and conductive performance; at the same time, the peeling force between the active layer and the substrate layer of Comparative Example 2 is significantly reduced after soaking compared with Example 2, and the bonding tightness between the active layer and the substrate layer is poor. The lithium-embedded tape has low stability in the lithium battery, which is not conducive to the effective use of the lithium storage performance of the active layer.
[0126] In addition, the lithium-embedded tape in Example 6 has a release layer, so its comprehensive air permeability is high before soaking in liquid, but its air permeability is poor. After soaking in liquid, the release layer of the lithium-embedded tape is peeled off, and the comprehensive air permeability of the lithium-embedded tape is significantly reduced. Compared with Examples 1 to 7 and Example 8, it shows more excellent air permeability.
[0127] In summary, the embodiments of the present application design the components of the active composition, and use 60-99 parts by weight of a conductive agent and 0.5-30 parts by weight of an adhesive as the main raw materials of the active composition, so that the active composition can form an active layer in the lithium-embedded tape. The active layer formed by the active composition can store excess lithium ions during the charge and discharge process of the battery to inhibit the accumulation of lithium ions at the interface of the electrode, thereby effectively improving the safety performance of the lithium battery.
[0128] The various technical features described above can be combined arbitrarily. Although all possible combinations of these technical features are not described, any combination of these technical features should be considered to be covered by this specification as long as there is no contradiction in such combination.
[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. An active composition, characterized in that Used to form an active layer in a lithium-embedded tape, the active composition is mainly made of a conductive agent and an adhesive as raw materials; Calculated by weight, the conductive agent is 60-99 parts, and the adhesive is 0.5-30 parts.
2. The active composition according to claim 1, characterized in that The raw materials of the active composition also include: functional additives: 0.01-10 parts.
3. The active composition according to claim 1 or 2, characterized in that The conductive agent includes a granular conductive powder with a particle size less than 1 μm; Optionally, the conductive agent includes at least one of graphite, hard carbon, conductive carbon black, carbon nanotubes or graphene; Optionally, the graphite specific surface area ranges from 1 to 20 m 2 / g; Optionally, the hard carbon is selected from at least one of resin carbon, organic polymer pyrolytic carbon or carbon black, and the reversible specific capacity of the hard carbon is 500-700 mAH; Optionally, the conductive carbon black has a resistivity of 0.8-1.8Ω·m and a thermally volatile component of ≤0.8%; Optionally, the carbon nanotubes are single-walled or multi-walled carbon nanotubes.
4. The active composition according to claim 3, characterized in that The adhesive is a pressure-sensitive hot-melt material, and the bonding temperature is 50-100°C; Optionally, the adhesive includes at least one of a water-based adhesive or an oil-based adhesive; Optionally, the aqueous adhesive includes at least one of a polyolefin resin, an ethylene-vinyl acetate copolymer, an ethylene-acrylic acid copolymer, an ethylene-ethyl acrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-methacrylic acid copolymer or polyvinylidene fluoride; Optionally, the oily adhesive includes at least one of maleic anhydride-modified polypropylene resin, polyester resin, polyurethane thermoplastic elastomer, polyacrylate resin or ethylene vinyl acetate copolymer.
5. The active composition according to claim 4, wherein the functional additive comprises at least one of a thickener, a dispersant or a defoamer; Optionally, the thickener includes at least one of silica, cellulose, polyacrylic acid or polyether; Optionally, the dispersant includes at least one of the oily dispersants BYK-P 105, BYK-W96076, BYK-W969 or BYK-W980; Optionally, the dispersant includes at least one of aqueous dispersants BYK-154, BYK-AT-250 or BYK-DISPERSANT-2152; Optionally, the defoamer includes at least one of oily defoamers BYK-014, BYK-066N or BYK-1752; Optionally, the defoamer includes at least one of aqueous defoamers BYK-012, BYK-024, BYK-039 or BYK-1640.
6. A lithium-embedded tape, characterized in that: The lithium-intercalated tape comprises a substrate layer and an active layer formed by the active composition according to any one of claims 1 to 5, wherein the active layer is supported on the substrate layer.
7. The lithium-embedded tape according to claim 6, characterized in that: The active layer has a porous structure; Optionally, the active layer has a thickness of 5 to 100 μm; Optionally, the substrate layer has a thickness of 5 to 50 μm; Optionally, the porosity of the substrate layer is 30-85%, and the pore size is ≤10 μm; Optionally, the substrate layer is at least one of a polypropylene diaphragm, a polyethylene diaphragm, a polyimide diaphragm or a polyvinylidene fluoride diaphragm; Optionally, the substrate layer is at least one of polypropylene non-woven fabric, polyethylene non-woven fabric, polyester non-woven fabric or polytetrafluoroethylene non-woven fabric.
8. The lithium-embedded tape according to claim 6 or 7, characterized in that: The lithium-intercalated tape further comprises a conductive adhesive layer, and the conductive adhesive layer is supported on a side of the active layer away from the substrate layer; Optionally, the conductive adhesive layer has a thickness of less than 10 μm; Optionally, the conductive adhesive layer is prepared from a raw material selected from a mixture of at least one of an aqueous emulsion, a polyacrylate resin, a rubber system, a polyurethane thermoplastic elastomer or an ethylene vinyl acetate copolymer and a conductive agent; Optionally, the mass fraction of the conductive agent in the conductive adhesive layer is 5-30%.
9. The lithium-embedded tape according to claim 8, characterized in that: The lithium-embedded adhesive tape further comprises a release layer, wherein the release layer is arranged on a side of the substrate layer away from the active layer, or is arranged on a surface of the conductive adhesive layer; Optionally, the release layer has a thickness of less than 1 μm.
10. A method for preparing a lithium-intercalated tape as claimed in any one of claims 6 to 9, characterized in that: include: The conductive agent, adhesive and functional additive are mixed evenly in a predetermined ratio and then coated on the substrate layer to form an active layer to obtain the lithium-embedded adhesive tape; or, After forming the active layer, applying a mixture of a non-sticky adhesive and a conductive agent at room temperature to a side of the active layer away from the substrate layer to form a conductive adhesive layer to obtain a lithium-embedded tape; or, After the active layer is formed, a mixture of an adhesive and a conductive agent that is viscous at room temperature is applied to the side of the active layer that is away from the substrate layer to form a conductive adhesive layer, and a release layer is provided on the surface of the conductive adhesive layer, or a release agent is applied to the side of the substrate layer that is away from the active layer to form a release layer to obtain a lithium-embedded tape.