Composite lithium-supplementing conductive material as well as preparation method and application thereof

By nano-depositing lithium oxalate on conductive materials, forming a composite lithium-supplemented conductive material, the problems of low efficiency and high voltage of lithium oxalate sacrificial lithium oxalate in lithium-ion batteries are solved, and the charging specific capacity and cycle stability of the battery are improved .

CN119050511APending Publication Date: 2024-11-29GANFENG LITHIUM CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411381513.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lithium oxalate sacrificial lithium supplement agents have low lithium replenishment efficiency and high voltage in lithium-ion batteries, which affects the battery's charging specific capacity and cycle stability.

Method used

By reacting oxalic acid dihydrate, lithium nitrate and conductive material in a solvent, a composite lithium supplement conductive material is formed, and lithium oxalate is nano-deposited on the outer surface of the conductive material, reducing the decomposition voltage of the lithium supplement agent and improving the lithium supplement efficiency.

Benefits of technology

It effectively improves the charging specific capacity of lithium-ion batteries, improves the lithium replenishment efficiency, and solves the low efficiency and high voltage problems of lithium oxalate sacrificial lithium replenishment agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050511A_ABST
    Figure CN119050511A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and provides a composite lithium-supplementing conductive material as well as a preparation method and application thereof. The preparation method of the composite lithium-supplementing conductive material comprises the following steps: mixing oxalic acid dihydrate, lithium nitrate, a conductive material and a solvent, and reacting to obtain the composite lithium-supplementing conductive material. The lithium oxalate precipitate is formed in the solvent, and the lithium oxalate is nanocrystallized and deposited on the outer surface of the conductive material and compounded with the conductive material, so that the decomposition voltage of the lithium supplement agent is effectively reduced, the lithium supplement efficiency is improved, and the charging specific capacity of the lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite lithium-supplementing conductive material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in various electronic products, electric vehicles and energy storage power stations. However, with the development of the industry, people's demand for electronic equipment is increasing, and the performance requirements for lithium-ion batteries are also increasing. Especially in the fields of electric vehicles, wearable devices, etc., higher requirements are placed on the energy density, cycle life and safety of batteries.

[0003] During the first charge of a lithium-ion battery, a solid electrolyte interface film (SEI) will form on the surface of the negative electrode, causing irreversible loss of active lithium. The main function of a sacrificial positive electrode lithium supplement is to supplement the lithium consumed by the formation of SEI during the first charge of the battery and the lithium lost during the cycle, thereby improving the capacity and cycle stability of the battery. The theoretical specific capacity of lithium oxalate sacrificial lithium supplement is 525mAh / g, which has a significant lithium supplement effect. It can be decomposed into active lithium ions and carbon dioxide gas during the battery formation process. The gas is discharged from the battery, and the active lithium ions compensate for the lithium loss, achieving the goal of maintaining the integrity of the battery without leaving any traces. In addition, because lithium oxalate sacrificial lithium supplements are low in cost, easy to prepare, and have good potential compatibility with battery manufacturing processes, they are regarded as high-potential lithium supplement additives for positive electrode materials. However, lithium oxalate sacrificial lithium supplements still have problems such as low lithium supplement efficiency and high voltage.

[0004] Therefore, a composite lithium-supplementing conductive material is provided to solve the problems existing in the existing lithium oxalate sacrificial lithium-supplementing agent, which has broad application prospects. Summary of the invention

[0005] The purpose of the present invention is to provide a composite lithium-supplementing conductive material and a preparation method and application thereof in view of the deficiencies in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a method for preparing a composite lithium-supplementing conductive material. Oxalic acid dihydrate, lithium nitrate, a conductive material and a solvent are mixed and reacted to obtain the composite lithium-supplementing conductive material.

[0008] Preferably, the conductive material comprises one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, graphyne, reduced graphene oxide, aluminum nanowires and two-dimensional layered metal carbides.

[0009] Preferably, the solvent is anhydrous ethanol and / or N-methylpyrrolidone.

[0010] Preferably, the mass volume ratio of the oxalic acid dihydrate, lithium nitrate, conductive material and solvent is 0.1-2 g: 0.1-1 g: 0.1-1 g: 100-200 ml.

[0011] Preferably, the reaction temperature is 40-60° C., and the reaction time is 10-40 min.

[0012] Preferably, the particle size of the composite lithium-supplementing conductive material is 5 to 500 nm.

[0013] The invention also provides a composite lithium-supplementing conductive material prepared by the preparation method.

[0014] The present invention also provides application of the composite lithium-supplementing conductive material in the positive electrode of a lithium-ion battery.

[0015] Preferably, the positive electrode of the lithium-ion battery comprises a composite lithium-supplementing conductive material, a positive electrode material and a binder, and the mass ratio of the composite lithium-supplementing conductive material, the positive electrode material and the binder is 1:7 to 9:1.

[0016] Preferably, the positive electrode material comprises a lithium iron phosphate positive electrode material, a lithium iron manganese phosphate positive electrode material, a lithium-rich manganese-based positive electrode material or a nickel-cobalt-manganese ternary positive electrode material.

[0017] Beneficial effects of the present invention:

[0018] The present invention forms lithium oxalate precipitation in a solvent, and deposits the lithium oxalate on the outer surface of a conductive material in a nanometer form to compound with the conductive material, thereby effectively reducing the decomposition voltage of the lithium supplement agent, improving the lithium supplement efficiency, and thus improving the charging specific capacity of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The X-ray diffraction pattern of the composite lithium-supplementing conductive material prepared in Example 1;

[0020] Figure 2 This is a scanning electron microscope image of the composite lithium-supplementing conductive material prepared in Example 1;

[0021] Figure 3 A comparison chart of the decomposition capacity of the composite lithium-supplementing conductive material prepared in Example 1 and the pure lithium oxalate lithium-supplementing agent;

[0022] Figure 4 The charge and discharge curves of the composite lithium-supplementing conductive material prepared in Example 1 and the pure lithium oxalate lithium-supplementing agent in the NCM9 positive electrode. DETAILED DESCRIPTION

[0023] The invention provides a method for preparing a composite lithium-supplementing conductive material. Oxalic acid dihydrate, lithium nitrate, a conductive material and a solvent are mixed and reacted to obtain the composite lithium-supplementing conductive material.

[0024] In the present invention, the conductive material preferably comprises one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, graphyne, reduced graphene oxide, aluminum nanowires and two-dimensional layered metal carbides.

[0025] In the present invention, the solvent is preferably anhydrous ethanol and / or N-methylpyrrolidone.

[0026] In the present invention, the mass volume ratio of the oxalic acid dihydrate, lithium nitrate, conductive material and solvent is preferably 0.1-2g:0.1-1g:0.1-1g:100-200ml, more preferably 0.5-1.5g:0.2-0.81g:0.2-0.8g:120-180ml, and more preferably 1.0g:0.4g:0.4g:140ml.

[0027] In the present invention, preferably, oxalic acid dihydrate, a conductive material and a first portion of a solvent are mixed to obtain a mixed solution I, lithium nitrate and a second portion of a solvent are mixed to obtain a mixed solution II, and the mixed solution II is added dropwise to the mixed solution I.

[0028] In the present invention, the volume ratio of the first part of the solvent to the second part of the solvent is preferably 110-130:20, more preferably 120:20; the dripping rate is preferably 1-3 ml / min, more preferably 2 ml / min.

[0029] In the present invention, the reaction is preferably carried out under stirring conditions, and the stirring speed is preferably 500 to 1000 rpm, and more preferably 600 to 800 rpm.

[0030] In the present invention, the reaction temperature is preferably 40 to 60° C., more preferably 45 to 55° C., and more preferably 50° C.; the reaction time is preferably 10 to 40 min, and more preferably 20 to 30 min.

[0031] In the present invention, after the reaction is completed, it is preferred to filter out the solid product by suction, and then dry the solid product to obtain the composite lithium-supplementing conductive material.

[0032] In the present invention, the filtration pressure is preferably 0.05 to 0.1 MPa, more preferably 0.07 to 0.098 MPa; the filtration time is preferably 3 to 5 min, more preferably 4 min.

[0033] In the present invention, the drying temperature is preferably 50 to 70° C., more preferably 60° C.; the drying time is preferably 20 to 28 h, more preferably 24 h.

[0034] In the present invention, the particle size of the composite lithium-supplementing conductive material is preferably 5 to 500 nm, more preferably 20 to 400 nm, and even more preferably 100 to 200 nm.

[0035] The invention also provides a composite lithium-supplementing conductive material prepared by the preparation method.

[0036] The present invention also provides application of the composite lithium-supplementing conductive material in the positive electrode of a lithium-ion battery.

[0037] In the present invention, the positive electrode of the lithium ion battery preferably comprises a composite lithium-supplementing conductive material, a positive electrode material and a binder. The mass ratio of the composite lithium-supplementing conductive material, the positive electrode material and the binder is preferably 1:7 to 9:1, more preferably 1:7.5 to 8.5:1, and more preferably 1:8:1.

[0038] In the present invention, the positive electrode material preferably comprises a lithium iron phosphate positive electrode material, a lithium iron manganese phosphate positive electrode material, a lithium-rich manganese-based positive electrode material or a nickel-cobalt-manganese ternary positive electrode material.

[0039] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0040] Example 1

[0041] 1.5 g of oxalic acid dihydrate and 0.4 g of multi-walled carbon nanotubes were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0042] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0043] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0044] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 20 nm.

[0045] Example 2

[0046] 1.0 g of oxalic acid dihydrate and 0.4 g of multi-walled carbon nanotubes were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0047] 0.4 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0048] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0049] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 5 nm.

[0050] Example 3

[0051] 0.5 g of oxalic acid dihydrate and 0.4 g of multi-walled carbon nanotubes were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0052] 0.2 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0053] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0054] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 100 nm.

[0055] Example 4

[0056] 1.5 g of oxalic acid dihydrate and 0.8 g of multi-walled carbon nanotubes were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0057] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0058] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0059] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 200 nm.

[0060] Example 5

[0061] 1.5 g of oxalic acid dihydrate and 0.2 g of multi-walled carbon nanotubes were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0062] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0063] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0064] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 500 nm.

[0065] Example 6

[0066] 1.5 g of oxalic acid dihydrate and 0.4 g of reduced graphene oxide (RGO) were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0067] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0068] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0069] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 20 nm.

[0070] Example 7

[0071] 1.0 g of oxalic acid dihydrate and 0.4 g of reduced graphene oxide (RGO) were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0072] 0.4 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0073] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0074] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 5 nm.

[0075] Example 8

[0076] 0.5 g of oxalic acid dihydrate and 0.4 g of reduced graphene oxide (RGO) were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0077] 0.2 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0078] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0079] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 100 nm.

[0080] Example 9

[0081] 1.5 g of oxalic acid dihydrate and 0.8 g of reduced graphene oxide (RGO) were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0082] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0083] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0084] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 200 nm.

[0085] Example 10

[0086] 1.5 g of oxalic acid dihydrate and 0.4 g of aluminum nanowires were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0087] 0.81 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0088] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0089] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 20 nm.

[0090] Embodiment 11

[0091] 1.0 g of oxalic acid dihydrate and 0.4 g of aluminum nanowires were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0092] 0.4 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0093] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0094] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 5 nm.

[0095] Example 12

[0096] 0.5 g of oxalic acid dihydrate and 0.4 g of aluminum nanowires were dispersed in 120 ml of anhydrous ethanol to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 45° C. and the mixture was stirred at a speed of 800 rpm.

[0097] 0.2 g of lithium nitrate was dispersed in 20 ml of anhydrous ethanol to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 2 ml / min to the mixed solution I stirred at a speed of 800 rpm to react for 30 minutes.

[0098] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.098 MPa for 5 minutes to obtain a solid product. The solid product is dried at 60° C. for 24 hours to obtain a composite lithium-supplementing conductive material.

[0099] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 100 nm.

[0100] Example 13

[0101] 1.5 g of oxalic acid dihydrate and 0.4 g of two-dimensional layered metal carbide were dispersed in 110 ml of N-methylpyrrolidone to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 50° C. and the solution was stirred at a speed of 500 rpm.

[0102] 0.4 g of lithium nitrate was dispersed in 20 ml of N-methylpyrrolidone to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 1 ml / min to the mixed solution I stirred at a speed of 500 rpm to react for 40 minutes.

[0103] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.05 MPa for 4 minutes to obtain a solid product. The solid product is dried at 50° C. for 28 hours to obtain a composite lithium-supplementing conductive material.

[0104] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 100 nm.

[0105] Embodiment 14

[0106] 1.5 g of oxalic acid dihydrate and 0.4 g of graphyne were dispersed in 130 ml of N-methylpyrrolidone to obtain a mixed solution I. The temperature of the mixed solution I was controlled to be 60° C. and the solution was stirred at a speed of 1000 rpm.

[0107] 0.4 g of lithium nitrate was dispersed in 20 ml of N-methylpyrrolidone to obtain a mixed solution II; the mixed solution II was added dropwise at a rate of 3 ml / min to the mixed solution I stirred at a speed of 1000 rpm to react for 20 minutes.

[0108] After the reaction is completed, stirring is stopped, the mixture is cooled to room temperature, and suction filtration is performed at a pressure of 0.1 MPa for 3 minutes to obtain a solid product. The solid product is dried at 70° C. for 20 hours to obtain a composite lithium-supplementing conductive material.

[0109] The particle size of the composite lithium-supplementing conductive material prepared in this embodiment is 200 nm.

[0110] The composite lithium supplement conductive material of Examples 1 to 5, the ternary positive electrode material NCM9, and the binder PVDF were respectively made into positive electrodes in a mass ratio of 1:8:1, and assembled into batteries with graphite negative electrodes. The first charge was carried out at 30°C at 0.1C to determine the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. Comparative Example 1 only used lithium oxalate as a lithium supplement agent, and Comparative Example 2 only used multi-walled carbon nanotubes as a lithium supplement agent. The lithium supplement agents of Comparative Examples 1 and 2 were respectively made into positive electrodes with the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1, and assembled into batteries with graphite negative electrodes. The first charge was carried out at 30°C at 0.1C to determine the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. The results of the charge specific capacity determination are shown in Table 1.

[0111] Table 1 Measurement results of composite lithium-supplementing conductive materials of Examples 1 to 5

[0112]

[0113] The composite lithium supplement conductive material of Examples 6 to 9 was respectively used with lithium iron phosphate positive electrode material and binder PVDF in a mass ratio of 1:8:1 to prepare positive electrode, and assembled with graphite negative electrode into battery, and the first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. Comparative Example 3 only used lithium oxalate as a lithium supplement agent, and Comparative Example 4 only used reduced graphene oxide (RGO) as a lithium supplement agent. The lithium supplement agents of Comparative Examples 3 and 4 were respectively used with lithium iron phosphate positive electrode material and binder PVDF in a mass ratio of 1:8:1 to prepare positive electrode, and assembled with graphite negative electrode into battery, and the first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. The results of the charge specific capacity measurement are shown in Table 2.

[0114] Table 2 Measurement results of composite lithium-supplementing conductive materials of Examples 6 to 9

[0115]

[0116] The composite lithium supplement conductive material of Examples 10 to 12 was respectively used with the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and assembled with the graphite negative electrode into a battery, and the first charge was carried out at 30°C at 0.1C to measure the charge specific capacity, and the charge voltage was cut off when it reached 4.45V. Comparative Example 5 only used aluminum nanowires as a lithium supplement agent and the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and assembled with the graphite negative electrode into a battery, and the first charge was carried out at 30°C at 0.1C to measure the charge specific capacity, and the charge voltage was cut off when it reached 4.45V. The charge specific capacity measurement results are shown in Table 3.

[0117] Table 3 Measurement results of composite lithium-supplementing conductive materials of Examples 10 to 12

[0118]

[0119] The composite lithium supplement conductive material of Example 13 was used with the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and assembled with the graphite negative electrode into a battery, and the first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. Comparative Example 6 only used two-dimensional layered metal carbide as a lithium supplement agent and the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and assembled with the graphite negative electrode into a battery, and the first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. The results of the charge specific capacity measurement are shown in Table 4.

[0120] The composite lithium supplement conductive material of Example 14 was used with the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and the battery was assembled with the graphite negative electrode. The first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. Comparative Example 7 only used graphyne as a lithium supplement agent and the ternary positive electrode material NCM9 and the binder PVDF in a mass ratio of 1:8:1 to prepare the positive electrode, and the battery was assembled with the graphite negative electrode. The first charge was carried out at 30°C at 0.1C to measure the specific charge capacity, and the charging voltage was cut off when it reached 4.45V. The results of the charge specific capacity measurement are shown in Table 4.

[0121] Table 4 Measurement results of composite lithium-supplementing conductive materials of Examples 13 to 14

[0122]

[0123] As shown in Tables 1 to 4, the present invention deposits nano-lithium oxalate on the outer surface of the conductive material and compounds it with the conductive material, thereby effectively reducing the decomposition voltage of the lithium supplement agent, improving the lithium supplement efficiency, and increasing the initial charge specific capacity of the lithium ion battery by 7 to 28.8%.

[0124] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a composite lithium-supplementing conductive material, It is characterized in that The composite lithium-supplementing conductive material is obtained by mixing oxalic acid dihydrate, lithium nitrate, a conductive material and a solvent and reacting them.

2. The preparation method according to claim 1, It is characterized in that The conductive material comprises one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, graphyne, reduced graphene oxide, aluminum nanowires and two-dimensional layered metal carbides.

3. The preparation method according to claim 1 or 2, It is characterized in that The solvent is anhydrous ethanol and / or N-methylpyrrolidone.

4. The preparation method according to claim 3, It is characterized in that The mass volume ratio of the oxalic acid dihydrate, lithium nitrate, conductive material and solvent is 0.1-2g: 0.1-1g: 0.1-1g: 100-200ml.

5. The preparation method according to claim 4, It is characterized in that The reaction temperature is 40-60° C., and the reaction time is 10-40 min.

6. The preparation method according to claim 4 or 5, It is characterized in that The particle size of the composite lithium-supplementing conductive material is 5 to 500 nm.

7. The composite lithium-supplementing conductive material obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the composite lithium-supplementing conductive material according to claim 7 in the positive electrode of a lithium-ion battery.

9. The use according to claim 8, It is characterized in that The positive electrode of the lithium ion battery comprises a composite lithium-supplementing conductive material, a positive electrode material and a binder, and the mass ratio of the composite lithium-supplementing conductive material, the positive electrode material and the binder is 1:7 to 9:

1.

10. The use according to claim 9, It is characterized in that The positive electrode material comprises a lithium iron phosphate positive electrode material, a lithium iron manganese phosphate positive electrode material, a lithium-rich manganese-based positive electrode material or a nickel-cobalt-manganese ternary positive electrode material.

Citation Information

Cited By

  • Composite lithium supplement agent, preparation method thereof and lithium ion battery

    CN121812594A