Ultrathin semiconductor / diamond superconducting heterostructure based on exciton coupling and preparation method thereof
By introducing boron and nitrogen doping into diamond and forming an ultra-thin semiconductor layer, exciton coupling is used to increase the superconducting transition temperature of diamond, the problem of low transition temperature of traditional diamond superconducting materials is solved, and higher superconducting performance is achieved , provides material support for high-temperature superconducting and quantum detection.
Patent Information
- Application Number
- CN202411167407.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The transition temperature of traditional diamond superconducting materials is low, and there is a lack of practical experimental verification methods to effectively improve the performance of high-temperature superconducting.
Microwave plasma chemical vapor deposition (MPCVD) method introduces boron and nitrogen doping into diamond to form bound excitons and form an ultra-thin semiconductor layer on the surface of the diamond. The synergistic effect of in vivo and interlayer exciton coupling is used to improve the diamond's Superconducting transition temperature.
It effectively increases the superconducting transition temperature of diamond, provides a solid material foundation for high-temperature superconducting theory and application, and promotes the application of diamond in the field of quantum detection.
Smart Images

Figure CN119053235A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling and a preparation method thereof, belonging to the technical field of semiconductors and superconducting techniques. Background Art
[0002] Traditional superconductivity is obtained through the interaction between electrons and phonons. With the further development of superconductivity, new superconducting mechanisms are constantly updated, such as the continuous discovery of high-temperature superconducting materials, and these new superconducting mechanisms also bring new developments in superconducting materials. Among them, the use of excitons to pair electrons is expected to become a high-temperature superconductor. Since the interaction between excitons and electrons or holes is much stronger than the interaction between phonons and electrons, scientists are spending a lot of time looking for such materials or structures. These new materials or superconducting structures under the action of excitons will bring new high-temperature superconducting applications. Although theoretical articles continue to appear, there is still a lack of actual direct and effective experimental verification. Since excitons are electrons and holes, there is a large exciton binding energy in wide bandgap semiconductors or ultra-thin semiconductors. As a semiconductor material with an ultra-wide bandgap, diamond has an exciton binding energy of up to 80meV, so it is expected to form interlayer excitons with other semiconductor materials, such as tungsten diselenide, molybdenum disulfide and other ultra-thin semiconductor materials, drive electrons to form electron-Cooper pairs, and obtain new superconducting structures. Summary of the invention
[0003] The object of the present invention is to provide an ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling and a preparation method thereof, which can effectively increase the superconducting transition temperature of diamond.
[0004] The technical solution adopted by the present invention is:
[0005] A method for preparing diamond by microwave plasma chemical vapor deposition (MPCVD) based on an ultra-thin semiconductor / diamond superconducting heterostructure with exciton coupling. Two doping gases are introduced simultaneously during the preparation process: a boron-containing doping gas and a nitrogen-containing doping gas, so that the diamond is co-doped with boron and nitrogen during the growth process, so that the holes formed by the doped B atoms and the electrons formed by the doped N atoms are coupled to form bound excitons. An ultra-thin semiconductor layer is further formed on the surface of the diamond to obtain an ultra-thin semiconductor / diamond heterostructure, and electron holes interact with each other between the semiconductor layer and the diamond interface to form interlayer excitons. Benefiting from the synergistic effect of the coupling between the intrabody excitons and the interlayer excitons, the electron pairs are enhanced, thereby increasing the transition temperature of the diamond superconductor.
[0006] In the above technical solution, the boron-containing doping gas is one or more boron-containing gases such as borane and ethylboron.
[0007] The nitrogen-containing doping gas is one or more of nitrogen-containing gases such as nitrogen, nitrogen dioxide, and ammonia.
[0008] The ultra-thin semiconductor is one of molybdenum disulfide, tungsten diselenide, black phosphorus, silicon, NbN and the like, and the thickness is generally not more than 100 nm.
[0009] The preparation of diamond by MPCVD method specifically includes: using a clean single crystal diamond as a substrate, placing it in an MPCVD reaction chamber, evacuating the chamber, and then introducing a carbon source gas and a doping gas into the reaction chamber to grow diamond. The evacuation is performed until the background vacuum in the reaction chamber is not less than 1×10 -3 Torr.
[0010] The carbon source gas is methane, and the input power range of the microwave source is controlled to be 1-10kW during the growth process, and the cavity pressure range is 10-150Torr. Preferably, the flow ratio of the carbon source gas to the doping gas should be no higher than 3:1; the boron-nitrogen atomic ratio of the boron-containing doping gas to the nitrogen-containing doping gas in the doping gas is 1:5-5:1. The acceptor and donor coupling brought by the two doping atoms form bound excitons. Further, an ultra-thin semiconductor layer is transferred or grown on the surface of the obtained diamond to form an ultra-thin semiconductor / diamond superconducting heterostructure, and the electron holes between the semiconductor layer and the diamond interface interact to form interlayer excitons. When the temperature is reduced, the excitons in the diamond body and the ultra-thin semiconductor / diamond interlayer excitons interact to form Cooper electron pairs, thereby realizing the transition to the superconducting state. Moreover, benefiting from the synergistic enhancement of the coupling between the excitons in the body and the interlayer excitons, the superconducting transition temperature of diamond can be further increased, promoting the theoretical research and practical application of high-temperature superconductivity.
[0010] According to a specific embodiment of the present invention, a method for preparing an ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling includes the following steps: 1) Using single crystal diamond with (100) crystal orientation as substrate; 2) ultrasonically cleaning the substrate using acetone, isopropanol, ethanol and deionized water before growth on the substrate surface; 3) Using MPCVD equipment to evacuate; 4) During the growth stage, the microwave source input power was maintained at 5 kW, the cavity pressure was maintained at 10 Torr, and methane gas was used as the main carbon source; 5) During the doping growth stage, a mixed gas of 20 sccm of borane and 5 sccm of nitrogen is introduced as a doping source to achieve co-doping of boron atoms and nitrogen atoms during the diamond growth process; 6) A monolayer of molybdenum disulfide is transferred onto the surface of the diamond after the doping growth is completed to obtain a molybdenum disulfide / diamond superconducting heterostructure.
[0012] Compared with the prior art, the present invention has the following beneficial effects: Traditional diamond superconductors are mostly based on polycrystalline diamonds, and the superconductivity theory is based on the BCS theory, which originates from the interaction between phonons and electrons. However, the present invention is an exciton-coupled ultra-thin semiconductor / diamond superconducting heterostructure, which mainly introduces boron acceptors and nitrogen donors in the process of growing single-crystalline diamond using MPCVD equipment, thereby introducing a large number of bound excitons. Furthermore, an ultra-thin semiconductor layer is formed on the surface of the diamond to obtain an ultra-thin semiconductor / diamond heterostructure, and electron holes interact with each other between the semiconductor layer and the diamond interface to form interlayer excitons. When the temperature is lowered, the excitons in the diamond body and the ultra-thin semiconductor / diamond interlayer excitons interact to form Cooper electron pairs, effectively increasing the superconducting transition temperature of diamond, and providing a solid material foundation for the application of diamond materials in high-temperature superconductivity, quantum detection and other fields. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 Schematic diagram of low temperature resistance test of an ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling prepared by the method of Example 1; Figure 2 This is a graph showing the relationship between the low temperature resistance and temperature of the exciton-coupled molybdenum disulfide / diamond superconducting heterostructure obtained by the method of Example 1. The test range is 2K to 300K. When the temperature is gradually reduced to 5K, the resistance of the molybdenum disulfide / diamond structure drops to zero. Figure 3 The relationship between the low temperature resistance of diamond and the temperature of the surface untransferred ultra-thin semiconductor obtained by the method of Example 2 is shown in the test range of 2K to 20K. When the temperature is gradually reduced to 2K, the diamond resistance is still 0.002Ω; Figure 4 This is a graph showing the relationship between the low temperature resistance and temperature of the exciton-coupled molybdenum disulfide / diamond superconducting structure obtained by the method of Example 2. The test range is 2K to 20K. When the temperature is gradually reduced to 5K, the resistance of the molybdenum disulfide / diamond structure drops to zero. Figure 5 This is a distribution diagram of B, C and N elements inside the diamond substrate material in the exciton-coupled tungsten diselenide / diamond superconducting structure obtained using Example 4. DETAILED DESCRIPTION
[0014] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0015] Reference Figure 1The present invention is based on an exciton-coupled ultra-thin semiconductor / diamond superconducting heterostructure. In the process of preparing diamond by MPCVD growth, a mixed gas of borane and nitrogen is used for doping to obtain a single-crystal diamond material co-doped with boron and nitrogen. Boron and nitrogen are doped into diamond to introduce holes and electrons as carriers to couple and form excitons in the body. An ultra-thin semiconductor / diamond heterostructure is formed by transferring or growing an ultra-thin semiconductor on the surface of diamond, and interlayer excitons are formed at the interface. When the temperature is lowered, the excitons in the diamond body and the interlayer excitons at the interface of the ultra-thin semiconductor / diamond structure interact with each other to form Cooper electron pairs, thereby achieving a transition to a superconducting state with a higher transition temperature. Figure 1 In the structure, a gold electrode is prepared on the surface of the ultra-thin semiconductor / diamond superconducting heterostructure for testing. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling of the present invention can effectively provide an experimental basis for the theory of high-temperature superconductivity, promote the development of superconducting theory and the application of diamond quantum detection.
[0016] Embodiment 1: 1) Take a single crystal diamond with a (100) crystal orientation and a size of 9 mm × 9 mm as a substrate, and polish the growth surface to ensure that the growth surface is smooth and flat; 2) The substrate was ultrasonically cleaned in acetone, isopropanol, ethanol and deionized water in turn, and each solvent was used for 10 minutes to remove organic impurities attached to the surface, and then dried with N2; 3) Use MPCVD equipment to evacuate to 10 -3 Torr; 4) During the growth stage, the microwave source input power was maintained at 5 kW, the cavity pressure was maintained at 140 Torr, the growth temperature was maintained at 920°C, and methane gas was used as the main carbon source; 5) During the growth stage, a mixed gas of borane and nitrogen is introduced as a direct doping source, wherein the gas flow rates of borane and nitrogen are 20 sccm and 5 sccm, respectively, to achieve co-doping of diamond with boron atoms and nitrogen atoms. 6) A monolayer of molybdenum disulfide is transferred onto the surface of the doped diamond to prepare a molybdenum disulfide / diamond superconducting heterostructure. The relationship between the resistance and temperature of an ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling prepared in this example is as follows: Figure 2As shown, when the ambient temperature drops to 4.9K, the resistance begins to decrease. According to the relationship diagram of the diamond resistance value changing with temperature, it can be seen that the ultra-thin semiconductor / diamond superconducting structure based on exciton coupling of the present invention utilizes boron and nitrogen doped in diamond to introduce holes and electrons as carriers, couples to form excitons in the body, and transfers a single layer of molybdenum disulfide on the surface of diamond to form interlayer excitons at the interface, so that the excitons in the diamond body and the interlayer excitons at the interface of the molybdenum disulfide / diamond structure interact with each other to form Cooper electron pairs, thereby realizing the transition to the superconducting state.
[0017] Embodiment 2: 1) Take a single crystal diamond with a (100) crystal orientation and a size of 5 mm × 5 mm as a substrate, and polish the growth surface to ensure that the growth surface is smooth and flat; 2) The substrate was ultrasonically cleaned in acetone, isopropanol, ethanol and deionized water in turn, and each solvent was used for 20 minutes to remove organic impurities attached to the surface, and then dried with N2; 3) Use MPCVD equipment to evacuate to 10 -3 Torr; 4) During the growth stage, the microwave source input power was maintained at 3 kW, the cavity pressure was maintained at 100 Torr, the growth temperature was maintained at 1000° C., and methane gas was used as the main carbon source. 5) During the growth stage, a mixed gas of borane and nitrogen is introduced as a direct doping source, wherein the gas flow rates of borane and nitrogen are 20 sccm and 5 sccm, respectively, to achieve co-doping of diamond with boron atoms and nitrogen atoms. 6) A monolayer of molybdenum disulfide is transferred onto the surface of the doped diamond to prepare a molybdenum disulfide / diamond heterojunction structure. The relationship between the resistance value and temperature of the diamond without molybdenum disulfide transfer on the surface obtained in 5) is as follows: Figure 3 As shown in the figure, when the ambient temperature drops to 4.2K, the resistance value begins to decrease; when the ambient temperature is 2K, the resistance still fails to drop to zero. Figure 4 In comparison, after the treatment in step 6), i.e., after the molybdenum disulfide is transferred to the diamond surface, the transition temperature of the molybdenum disulfide / diamond structure is increased to 4.9K, and the resistance value is reduced to zero at a temperature of 3.6K. Therefore, compared with diamond, by transferring molybdenum disulfide on the diamond surface to form a molybdenum disulfide / diamond structure, it is beneficial to form interlayer excitons at the interface, and the synergistic effect of the coupling of excitons in the diamond body and interlayer excitons at the interface helps to increase the transition temperature of diamond and achieve superconductivity.
[0018] Embodiment 3: 1) Take a single crystal diamond with a (100) crystal orientation and a size of 5 mm × 5 mm as a substrate, and polish the growth surface to ensure that the growth surface is smooth and flat; 2) The substrate was ultrasonically cleaned in acetone, isopropanol, ethanol and deionized water in turn, and each solvent was used for 20 minutes to remove organic impurities attached to the surface, and then dried with N2; 3) Use MPCVD equipment to evacuate to 10 -3 Torr; 4) During the growth stage, the microwave source input power was maintained at 3 kW, the cavity pressure was maintained at 100 Torr, the growth temperature was maintained at 1000° C., and methane gas was used as the main carbon source. 5) During the growth stage, a mixed gas of borane and nitrogen is introduced as a direct doping source, wherein the gas flow rates of borane and nitrogen are 35 sccm and 8 sccm, respectively, to achieve co-doping of diamond with boron atoms and nitrogen atoms. 6) Growing 100 nm thick NbN on the surface of the doped diamond to prepare a NbN / diamond heterostructure. Compared with diamond, the resistance of NbN / diamond heterostructure begins to decrease around 15K. The synergistic effect of the exciton coupling within the diamond body and the interlayer exciton coupling at the heterostructure interface helps to increase its superconducting transition temperature.
[0019] Embodiment 4: 1) Take a single crystal diamond with a (100) crystal orientation and a size of 9 mm × 9 mm as a substrate, and polish the growth surface to ensure that the growth surface is smooth and flat; 2) The substrate was ultrasonically cleaned in acetone, isopropanol, ethanol and deionized water in turn, and each solvent was used for 10 minutes to remove organic impurities attached to the surface, and then dried with N2; 3) Use MPCVD equipment to evacuate to 10 -3 After Torr; 4) During the growth stage, the microwave source input power was maintained at 5 kW, the cavity pressure was maintained at 150 Torr, the growth temperature was maintained at 920° C., and methane gas was used as the main carbon source. 5) During the growth stage, a mixed gas of borane and ammonia is introduced as a direct doping source, wherein the gas flow rates of borane and ammonia are 20 sccm and 5 sccm, respectively, to achieve co-doping of diamond with boron atoms and nitrogen atoms. 6) A monolayer of tungsten diselenide is transferred onto the surface of the doped diamond to prepare a tungsten diselenide / diamond superconducting heterostructure. The prepared tungsten diselenide / diamond superconducting heterostructure has the following distribution of elements in the diamond substrate: Figure 5It can be seen that by using the boron-nitrogen co-doping method, the doping atoms are evenly distributed in the diamond body, and the bulk material shows good uniformity as a whole. Obviously, the present invention is not limited to the above-mentioned specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different options and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. An ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling, characterized in that: Diamond is prepared by microwave plasma chemical vapor deposition (MPCVD) method. Two doping gases are introduced simultaneously during the preparation process: boron-containing doping gas and nitrogen-containing doping gas, so that boron and nitrogen elements are co-doped during the growth process of diamond, so that holes and electrons are coupled to form body excitons. An ultra-thin semiconductor layer is further formed on the surface of the diamond to obtain an ultra-thin semiconductor / diamond superconducting heterostructure. Electrons and holes interact with each other between the semiconductor layer and the diamond interface to form interlayer excitons. Carriers in the diamond are coupled with interlayer excitons through body excitons to form electron pairs, thereby increasing the superconducting transition temperature of the diamond.
2. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 1, characterized in that: The ultra-thin semiconductor is one of molybdenum disulfide, tungsten diselenide, black phosphorus, silicon and NbN.
3. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 1, characterized in that: The boron-containing doping gas is one or more of borane and diborane.
4. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 1, characterized in that: The nitrogen-containing doping gas is one or more of nitrogen, nitrogen dioxide and ammonia.
5. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 1, characterized in that: The preparation of diamond by MPCVD method specifically includes: using clean single crystal diamond as substrate, placing it in MPCVD reaction chamber, evacuating the chamber, and then introducing carbon source gas and doping gas into the reaction chamber to grow diamond.
6. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 5, characterized in that: The vacuum is evacuated to a level where the background vacuum in the reaction chamber is not less than 1×10 -3 Torr.
7. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 5, characterized in that: The carbon source gas is methane, and during the growth process, the input power range of the microwave source is controlled to be 1-10 kW, and the cavity pressure range is 10-150 Torr.
8. The ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling according to claim 2, characterized in that: An ultrathin semiconductor / diamond superconducting heterostructure is achieved by transferring or growing an ultrathin semiconductor layer on the co-doped diamond surface.
9. An ultra-thin semiconductor / diamond superconducting heterostructure based on exciton coupling, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.
Citation Information
Cited By
Superconducting coupling-based super-flow protons microwave generator and preparation method thereof
CN120046751A