High stress impact wear resistant plasma surfacing flux-cored wire and preparation method thereof
By adding Mn, Nb, Mo, V, B, Ti and other elements to the flux-core welding wire, a fine hard phase is formed, and combined with the outer skin of low-carbon cold-rolled steel strip, the prone to cracks in high-stress impact wear environments is solved. The problem of peeling has achieved high hardness and wear resistance, met the requirements of strong impact conditions, and reduced costs.
Patent Information
- Application Number
- CN202411464783.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional flux-core welding wires are prone to cracks and peeling in high-stress impact wear environments, making it difficult to meet the wear resistance requirements of strong impact conditions, especially in the plasma surfacing process, which lacks targeted improvement.
By adding elements such as Mn, Nb, Mo, V, B, Ti, etc. to the medicament core, a variety of fine hard phases such as Nb, TiC, VC, Fe2B and other submicrons are formed, and combined with the outer skin of low-carbon cold-rolled steel strips, the preparation is carried out. The plasma surfacing flux core welding wire with a diameter of 1.2 to 2.8mm is produced, and the high-stress impact wear resistance is achieved by using nitrogen protection.
It significantly improves the hardness and wear resistance of the surfacing alloy, avoids cracks and peeling, enhances the resistance to high-stress impact, meets the requirements of high-stress wear conditions, and avoids the need to use slag-making agents and gas-making agents. , improves economical practicality.
Smart Images

Figure CN119057304A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of welding materials, and in particular relates to a plasma surfacing flux-cored welding wire resistant to high stress, impact and wear and a preparation method thereof. Background Art
[0002] The hammer head of the hammer crusher, the impact plate of the impact crusher, etc., they crush the ore during high-speed rotation (or crush the ore rushing up at high speed). High-stress impact abrasive wear behavior is widely present in mechanical equipment in the mining, energy, metallurgy, power and other industries, and the economic losses caused by it are very huge.
[0003] Wear-resistant materials such as high-carbon alloy steel, high-chromium steel, and high-chromium cast iron have sufficient hardness but low impact toughness, and are prone to early fracture. Traditional austenitic wear-resistant manganese steel has sufficient impact toughness but low original hardness, and surface work hardening occurs during strong impact. At the same time, high manganese steel has a low yield strength (about 350MPa), and workpieces are prone to plastic deformation during use, especially in the early stages of use. Although the hardness and impact toughness of low-alloy wear-resistant steel can meet the requirements, due to its low alloy content, poor hardenability, and low content of hard phases in the matrix structure, the overall wear resistance is poor.
[0004] Traditional flux-cored welding wires are mostly self-protected wear-resistant cladding flux-cored welding wires. A small amount of slag-forming agent and gas-forming agent needs to be added to the flux core to protect the weld, improve weldability, and improve the comprehensive mechanical properties of the cladding alloy. In plasma cladding, argon gas protects the weld, which can play the role of slag-forming agent and gas-forming agent. At present, there are few flux-cored welding wires for plasma cladding, so it is particularly important to develop new flux-cored welding wires for plasma cladding to meet the actual needs of the project. Summary of the invention
[0005] The purpose of the present invention is to provide a plasma cladding flux-cored welding wire resistant to high stress impact wear and a preparation method thereof, which solves the problem that the alloy layer is prone to cracking and peeling during high stress impact wear by adding Mn, Nb, Mo, V, B and Ti. It can adapt to working conditions with strong impact and has the performance of resisting high stress impact, crack propagation and abrasive wear.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A high stress, impact and wear resistant plasma surfacing flux-cored welding wire comprises an outer skin and a flux core, wherein the flux core is composed of the following raw materials in percentage by weight: 1wt% to 3wt% of graphite powder, 1wt% to 3wt% of high carbon ferrochrome powder, 15wt% to 27% of micro-carbon ferrochrome, 13wt% to 22wt% of chromium carbide powder, 1wt% to 5wt% of ferromolybdenum powder, 1wt% to 4wt% of ferrovanadium powder, 1wt% to 5% of ferroniobium, 1wt% to 2wt% of silicon carbide powder, 5wt% to 15% of ferroboron, 1wt% to 5% of titanium carbide powder, 1wt% to 3wt% of electrolytic manganese powder, and the remainder is reduced iron powder; the outer skin is a low carbon cold-rolled steel strip.
[0008] The powder particle size of the high carbon ferrochrome powder, low carbon ferrochrome powder, chromium carbide powder, electrolytic manganese powder and reduced iron powder is ≤250um; the powder particle size of the ferromolybdenum powder, ferrovanadium powder, ferroniobium powder, ferroboron powder, silicon carbide powder and titanium carbide powder is ≤180um; and the graphite particle size is ≤75um.
[0009] The diameter of the flux-cored welding wire is 1.2-2.8 mm.
[0010] A method for preparing a high stress impact wear resistant plasma surfacing flux-cored welding wire comprises the following steps:
[0011] 1) mixing the raw materials of the drug core, heating and drying them in a vacuum heating furnace, and after the drug core powder is cooled to room temperature, mixing them in a powder mixer to obtain a mixed drug core powder;
[0012] 2) A low-carbon cold-rolled steel strip is made into a U-shaped groove, and a mixed flux core powder accounting for 30% to 50% of the total weight of the flux-cored welding wire is added into the U-shaped groove; the U-shaped groove is closed, the flux core is wrapped therein, and the flux core welding wire with a diameter of 1.2 to 2.8 mm is finally obtained by drawing and reducing the diameter step by step.
[0013] The drying temperature in step 1) is 200-250° C., and the drying time is 90-180 min.
[0014] Step 1) The mixing time in the powder mixer is 30 to 60 minutes.
[0015] The main strengthening phase of Fe-Cr-C alloy is M7C3 carbide, which has good wear resistance and low price. It is the most widely used iron-based wear-resistant material. M7C3 carbide has a good application effect in low-stress abrasive wear environment, but M7C3 carbide is not able to resist high-stress wear and is prone to cracking and peeling when impacted. When the volume fraction of M7C3 carbide exceeds 35%, the hardness of the surfacing alloy no longer increases, and the tendency to crack increases.
[0016] In order to improve the ability to resist high stress impact wear, it is necessary to reduce the content of C and Cr elements, and improve the impact wear resistance of the surfacing alloy by adding Nb, Mo, V, B, and Ti. In the surfacing metal, Ti and C can form TiC, whose microhardness can reach HV3200, which plays a dispersion strengthening role on the surfacing alloy. And Ti can serve as the nucleation point of the metal in the molten pool, hinder the diffusion of carbon atoms, and promote the grain refinement of the surfacing alloy. Nb can generate NbC, with a melting point of 3500℃ and a microhardness of HV2400. Nb can improve the impact toughness of the weld and effectively refine the grain strengthening structure. Nb can also absorb excess C atoms, reduce the carbon content of the matrix, and improve the toughness and wear resistance of the surfacing alloy. The V element can generate fine carbides VC and V2C, and can also inhibit the growth of grains. In addition to forming separate TiC, VC, NbC, etc., the addition of multiple alloying elements will also form (Nb, Ti, V) C composite carbides, which have higher hardness and thermal stability than (Cr, Fe) 7C3 carbides, and can further improve the stability and wear resistance of the surfacing alloy structure. In addition, the use of multi-component composite addition method may control the total amount of strong carbide-forming elements added at a lower level under the condition of ensuring the formation of MC-type primary composite carbides, thereby achieving the purpose of cost saving and small amount of multi-component strengthening.
[0017] B exists mainly as an interstitial atom in Fe-Cr-C alloys, which is equivalent to the role of carbon. It can interact with alloying elements to directly form borides, thereby improving the hardness and wear resistance of the surfacing alloy. In addition, boron can also replace part of carbon and dissolve into MC and M7C3 carbides to increase the hardness of these carbides. The amount of boron dissolved in the iron matrix is very small, and it generally gathers near the grain boundaries, which can play a role in grain boundary strengthening. An appropriate amount of boron can refine the matrix structure and carbide grains, and improve the hardenability, hardness and wear resistance of the iron-based surfacing alloy. Moreover, B will form borides such as TiB2 and Fe2B with elements such as Fe and Ti, which are finely dispersed, play a role in dispersion strengthening, and can also significantly refine the grains. The primary carbides are in the shape of thin rods perpendicular to the wear surface. The matrix structure is composed of martensite and a small amount of austenite, and the strengthening phase and matrix strength and toughness are well matched, which has great advantages in improving the resistance of surfacing alloys to high stress wear.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The flux core of the present invention solves the problem that the alloy layer is prone to cracking and peeling during high stress impact wear by adding Mn, Nb, Mo, V, B, and Ti, and has the properties of abrasive wear resistance and high stress impact resistance of the deposited metal, meeting the service conditions requirements of high stress impact wear.
[0020] 2. The present invention forms a large number of submicron-level Nb, TiC, VC, Fe2B and other fine hard phases in the surfacing alloy structure, which are evenly distributed at the grain boundaries and in the grains, play the role of dispersion strengthening and fine grain strengthening, and increase the hardness of the matrix to 60-65HRC.
[0021] 3. The flux-cored welding wire of the present invention can greatly improve the hardness and wear resistance of the surfacing alloy without reducing the toughness of the surfacing alloy; there are no cracks, pores, slag inclusions, undercuts and other defects in the surfacing layer; there are no cracks or chipping in the impact wear test of the surfacing layer.
[0022] 4. The present invention does not require slag-forming agents and gas-forming agents. The high-stress wear resistance of the cladding layer is achieved only through the reasonable proportion of the core powder and nitrogen protection, which is economical and practical. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The microstructure of the metal coating after plasma surfacing of the flux-cored welding wire prepared in Example 1 of the present invention.
[0024] Figure 2 The microstructure of the metal coating after plasma surfacing of the flux-cored welding wire prepared in Example 2 of the present invention.
[0025] Figure 3 The microstructure of the metal coating after plasma surfacing of the flux-cored welding wire prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0026] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0027] Example 1
[0028] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0029] The composition and proportion of the core: graphite powder 2.1wt%, high carbon ferrochrome powder 2.5wt%, low carbon ferrochrome 24.3%, chromium carbide powder 16.2wt%, ferromolybdenum powder 2.3wt%, ferrovanadium powder 3.5wt%, ferroniobium 4.1%, silicon carbide powder 1.4wt%, ferroboron 7.3%, titanium carbide powder 1.1%, electrolytic manganese powder 1.3wt%, and the balance is reduced iron powder.
[0030] The outer skin is made of low carbon cold rolled steel strip.
[0031] The flux core formula and cold-rolled steel strip outer skin of Example 1 were used, and the filling rate of the flux core was controlled at 36%. A flux cored welding wire with a diameter of 1.2 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 62.7 HRC. The microstructure morphology of the surfacing layer was shown in FIG. Figure 1 .
[0032] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.5342g. Under the same conditions, the ZGMn13 high manganese steel, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 63.8%, and the wear resistance was more than doubled.
[0033] Example 2
[0034] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0035] The composition and proportion of the core: graphite powder 2.4wt%, high carbon ferrochrome powder 2.3wt%, low carbon ferrochrome 22.3%, chromium carbide powder 14.2wt%, ferromolybdenum powder 2.4wt%, ferrovanadium powder 1.9wt%, ferroniobium 2.6%, silicon carbide powder 1.4wt%, ferroboron 6.1%, titanium carbide powder 1.1wt%, electrolytic manganese powder 1.1wt%, and the balance is reduced iron powder.
[0036] The outer skin is made of low carbon cold rolled steel strip.
[0037] The flux core formula and cold-rolled steel strip outer skin of Example 2 were used, and the filling rate of the flux core was controlled at 46%. A flux cored welding wire with a diameter of 2.4 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 61.3 HRC. The microstructure morphology of the surfacing layer was shown in FIG. Figure 2 .
[0038] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.5597g. Under the same conditions, the ZGMn13, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 62.1%, and the wear resistance was more than doubled.
[0039] Example 3
[0040] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0041] The composition and proportion of the core: graphite powder 2.7wt%, high carbon ferrochrome powder 2.8wt%, low carbon ferrochrome 25.9%, chromium carbide powder 16.9wt%, ferromolybdenum powder 2.43wt%, ferrovanadium powder 1.3wt%, ferroniobium 3.1%, silicon carbide powder 1.1wt%, ferroboron 8.4%, titanium carbide powder 1.0%, electrolytic manganese powder 1.7wt%, and the remainder is reduced iron powder.
[0042] The outer skin is made of low carbon cold rolled steel strip.
[0043] The flux core formula and cold-rolled steel strip outer skin of Example 3 were used, and the filling rate of the flux core was controlled at 48%. A flux cored welding wire with a diameter of 2.8 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 63.7 HRC. The microstructure morphology of the surfacing layer was shown in FIG. Figure 3 .
[0044] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.4849g. Under the same conditions, the ZGMn13, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 67.1%, and the wear resistance was more than doubled.
[0045] Example 4
[0046] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0047] The composition and proportion of the core: graphite powder 1.9wt%, high carbon ferrochrome powder 2.0wt%, micro carbon ferrochrome 22.0%, chromium carbide powder 13.0wt%, ferromolybdenum powder 1.6wt%, ferrovanadium powder 2.4wt%, ferroniobium 4.0%, silicon carbide powder 1.0wt%, ferroboron 10.0%, titanium carbide powder 1.1%, electrolytic manganese powder 1.1wt%, and the balance is reduced iron powder.
[0048] The outer skin is made of low carbon cold rolled steel strip.
[0049] The flux core formula and cold-rolled steel strip outer skin of Example 4 were used, and the filling rate of the flux core was controlled at 46%. A flux cored welding wire with a diameter of 2.8 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 59.8 HRC.
[0050] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.6723g. Under the same conditions, the ZGMn13, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 54.52%, and the wear resistance was more than doubled.
[0051] Example 5
[0052] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0053] The composition and proportion of the flux core: graphite powder 2.1wt%, high carbon ferrochrome powder 2.5wt%, low carbon ferrochrome 23.9%, chromium carbide powder 18.0wt%, ferromolybdenum powder 2.0wt%, ferrovanadium powder 1.1wt%, ferroniobium 2.7%, silicon carbide powder 1.0wt%, ferroboron 11.5%, titanium carbide powder 1.1%, electrolytic manganese powder 1.0wt%, and the balance is reduced iron powder.
[0054] The outer skin is made of low carbon cold rolled steel strip.
[0055] The flux core formula and cold-rolled steel strip outer skin of Example 5 were used, and the filling rate of the flux core was controlled at 48%. A flux cored welding wire with a diameter of 2.8 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 61.9 HRC. Figure 3 .
[0056] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.6435g. Under the same conditions, the ZGMn13, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 55.79%, and the wear resistance was more than doubled.
[0057] Example 6
[0058] High stress impact wear resistant plasma cladding flux-cored welding wire, comprising a sheath and a flux core, wherein:
[0059] The composition and proportion of the core: graphite powder 1.6wt%, high carbon ferrochrome powder 1.9wt%, low carbon ferrochrome 26.0%, chromium carbide powder 17.0wt%, ferromolybdenum powder 1.2wt%, ferrovanadium powder 2.5wt%, ferroniobium 1.9%, silicon carbide powder 1.0wt%, ferroboron 7.7%, titanium carbide powder 1.0wt%, electrolytic manganese powder 1.0wt%, and the balance is reduced iron powder.
[0060] The outer skin is made of low carbon cold rolled steel strip.
[0061] The flux core formula and cold-rolled steel strip outer skin of Example 6 were used, and the filling rate of the flux core was controlled at 48%. A flux cored welding wire with a diameter of 2.4 mm was prepared by drawing. The flux cored welding wire was used for plasma surfacing, and the hardness of the surfacing layer obtained was 64.6 HRC. Figure 3 .
[0062] The impact wear test was conducted using an MLD-10 impact wear tester. The impact load was 5J, the lower sample was 45# steel, the hammer mass was 10kg, the upper sample impact times were 200 times / min, the lower sample speed was 200r / min; the abrasive particle size was 1.50-2.36mm refined quartz sand (HV1235), the abrasive flow rate was 40kg / h; the impact time was 8h. The impact wear weight loss of the cladding layer was 0.3977g. Under the same conditions, the ZGMn13, which is commonly used in impact wear environments, lost 1.4783g, the wear weight loss decreased by 73.1%, and the wear resistance was more than doubled.
Claims
1. A plasma cladding flux-cored welding wire resistant to high stress, impact and wear, characterized in that: The invention comprises an outer skin and a core, wherein the core is composed of the following raw materials in weight percentage: 1wt% to 3wt% of graphite powder, 1wt% to 3wt% of high-carbon ferrochrome powder, 15wt% to 27% of micro-carbon ferrochrome, 13wt% to 22wt% of chromium carbide powder, 1wt% to 5wt% of ferromolybdenum powder, 1wt% to 4wt% of ferrovanadium powder, 1wt% to 5% of ferroniobium, 1wt% to 2wt% of silicon carbide powder, 5wt% to 15% of ferroboron, 1wt% to 5% of titanium carbide powder, 1wt% to 3wt% of electrolytic manganese powder, and the remainder is reduced iron powder; the outer skin is a low-carbon cold-rolled steel strip.
2. The high stress impact wear resistant plasma surfacing flux-cored welding wire according to claim 1, characterized in that: The powder particle size of the high carbon ferrochrome powder, low carbon ferrochrome powder, chromium carbide powder, electrolytic manganese powder and reduced iron powder is ≤250um; the powder particle size of the ferromolybdenum powder, ferrovanadium powder, ferroniobium powder, ferroboron powder, silicon carbide powder and titanium carbide powder is ≤180um; and the graphite particle size is ≤75um.
3. The high stress impact wear resistant plasma cladding flux-cored welding wire according to claim 1, characterized in that: The diameter of the flux-cored welding wire is 1.2-2.8 mm.
4. A method for preparing a high stress impact wear resistant plasma cladding flux-cored welding wire according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) mixing the raw materials of the drug core, heating and drying them in a vacuum heating furnace, and after the drug core powder is cooled to room temperature, mixing them in a powder mixer to obtain a mixed drug core powder; 2) A low-carbon cold-rolled steel strip is made into a U-shaped groove, and a mixed flux core powder accounting for 30% to 50% of the total weight of the flux-cored welding wire is added into the U-shaped groove; the U-shaped groove is closed, the flux core is wrapped therein, and the flux core welding wire with a diameter of 1.2 to 2.8 mm is finally obtained by drawing and reducing the diameter step by step.
5. The method for preparing a high stress impact wear resistant plasma cladding flux-cored welding wire according to claim 4, characterized in that: The drying temperature in step 1) is 200-250° C., and the drying time is 90-180 min.
6. The method for preparing a high stress impact wear resistant plasma cladding flux-cored welding wire according to claim 4, characterized in that: Step 1) The mixing time in the powder mixer is 30 to 60 minutes.
Citation Information
Cited By
Impact-wear-resistant flux-cored wire for welding high-manganese steel lining plate and surfacing method
CN121373899A
An impact and wear resistant flux cored wire for welding high manganese steel liner plate and a surfacing method
CN121373899B