A surface coating for regulating magnesium alloy degradation in stages and its preparation method and application
By preparing microarc oxidation coatings and electrodeposition iron-rich layers on the surface of magnesium alloys and covering polylactic acid coatings, the shortcomings of existing magnesium alloy fracturing balls in the initial corrosion resistance and later degradation performance are solved, and magnesium is achieved The alloy surface has good corrosion resistance in the early stage and rapid degradation in the later stage, and is suitable for oil and gas mining and other fields.
Patent Information
- Application Number
- CN202310035673.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-01-10
AI Technical Summary
The existing magnesium alloys for soluble fracturing balls cannot meet the service characteristics of good corrosion resistance in the early stage and rapid degradation in the later stage. It is urgent to develop new technologies for grading and regulating the degradation of magnesium alloys to promote its application.
The surface coating that regulates the degradation of magnesium alloys is adopted, including microarc oxidation coating, iron-rich layer and degradable polymer layer, is prepared by microarc oxidation treatment and electrodeposition methods to form a dense layer and porous layer structure, combined with polymerization Lactic acid coating to achieve initial corrosion resistance and later rapid degradation.
It has achieved good initial corrosion resistance and rapid degradation of the magnesium alloy surface coating, met the service requirements of soluble fracturing balls, has good wear resistance and environmental protection, and is suitable for oil and gas mining and other fields.
Smart Images

Figure CN116043306B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a surface coating for step-by-step regulation of magnesium alloy degradation, a preparation method and application thereof, and belongs to the technical field of magnesium alloy corrosion regulation. Background Art
[0002] Horizontal well staged fracturing technology is an important technology for exploiting dense low-permeability oil fields. In downhole stratified staged fracturing, it is necessary to drop balls or lower bridge plugs between layers to isolate the layers, and the temporary plugging tools need to be removed after the construction is completed. Downhole temporary plugging tools such as soluble fracturing balls can dissolve by themselves after the fracturing operation is completed, avoiding the drilling and milling removal steps after fracturing, and have the advantages of high efficiency, safety, and low cost. As an ideal material for downhole temporary plugging tools, degradable magnesium alloys have certain requirements in terms of mechanical properties as well as solubility properties. Generally, soluble magnesium alloy fracturing balls are required to degrade quickly after the fracturing operation is completed. Therefore, efficient protection in the early stage and rapid degradation in the later stage are important characteristics for service reliability.
[0003] Existing research technologies mainly focus on the composition, processing technology, and organizational structure of magnesium alloys for soluble fracturing balls. Magnesium alloys suitable for downhole temporary plugging tools have been developed one after another. The magnesium alloys for soluble fracturing balls currently under development cannot meet the service characteristics of good corrosion resistance in the early stage and rapid degradation in the later stage. It is urgent to develop new technologies for graded regulation of magnesium alloy degradation to promote the application and promotion of soluble magnesium alloy fracturing balls. Summary of the invention
[0004] The present invention aims to provide a method for preparing a surface coating for regulating the degradation of magnesium alloy in stages. The soluble magnesium alloy fracturing ball prepared by the method has good wear resistance and controllable degradation rate.
[0005] At the same time, the present invention provides a surface coating for regulating the degradation of magnesium alloy in stages.
[0006] At the same time, the present invention provides an application of a surface coating for step-by-step regulation of magnesium alloy degradation in a soluble magnesium alloy fracturing ball.
[0007] At the same time, the present invention provides a soluble magnesium alloy fracturing ball.
[0008] At the same time, a soluble magnesium alloy fracturing ball is used in oil and gas production.
[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0010] A surface coating for step-by-step regulation of magnesium alloy degradation comprises a micro-arc oxidation coating, wherein the micro-arc oxidation coating comprises a fluorine-rich dense layer bonded to a magnesium alloy substrate and a porous layer located above the dense layer; the iron-rich layer penetrates into the microporous structure of the porous layer, and above the porous layer is a degradable polymer layer with swelling properties.
[0011] A method for preparing a surface coating for step-by-step regulation of magnesium alloy degradation comprises the following steps:
[0012] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: placing magnesium alloy for soluble fracturing ball in micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain micro-arc oxidation coating;
[0013] S2. Deposition of iron-rich compounds on porous structures of micro-arc oxidation coatings: Electrodeposition of iron-rich compounds on soluble magnesium alloy for fracturing balls after micro-arc oxidation treatment;
[0014] S3. Degradable polymer coating: The polymer coating is prepared by the immersion pulling method.
[0015] In S1, the micro-arc oxidation electrolyte is a silicate system aqueous solution, and its electrolyte composition is 20~30g / L Na2SiO3·9H2O, 1~2g / L NaOH and 4~8g / L KF·2H2O.
[0016] In S1, the process of micro-arc oxidation treatment is: Constant current mode: forward current is 10~20A / dm 2 , negative current is 0~5A / dm 2 , frequency 500~1000Hz, duty cycle: 15~30%, termination voltage 450~500V.
[0017] In S2, during the electrodeposition, the magnesium alloy after micro-arc oxidation is the cathode, the stainless steel is the anode, the electrodeposition solution is a 0.005~0.015 mol / L FeCl2 solution, the solvent of the FeCl2 solution is water, the voltage is 2.0~3.0 V, and the processing time is 10~20 min.
[0018] In S3, the degradable polymer coating is polylactic acid with a molecular weight of 40,000 to 150,000, which is dissolved in a dichloromethane solution at a ratio of 50 to 100 g / L; the immersion pulling rate is 0.5 to 1 mm / s, and the pulling is performed 3 to 5 times.
[0019] Application of a surface coating for step-by-step regulation of magnesium alloy degradation in soluble magnesium alloy fracturing balls.
[0020] A soluble magnesium alloy fracturing ball comprises a surface coating for step-by-step regulation of magnesium alloy degradation according to claim 1.
[0021] The invention discloses an application of a soluble magnesium alloy fracturing ball in oil and gas production.
[0022] The present invention provides a surface coating for step-by-step regulation of magnesium alloy degradation, and a preparation method and application thereof, including preparing a micro-arc oxidation coating on the surface of the magnesium alloy, depositing iron-rich compounds on the porous structure of the micro-arc oxidation coating, and coating a degradable polymer coating, thereby obtaining a surface coating with good initial corrosion resistance and accelerated degradation in the later stage.
[0023] The beneficial effects of the present invention are:
[0024] 1) The present invention relates to a surface coating for step-by-step regulation of magnesium alloy degradation, and a preparation method and application thereof. The silicate system micro-arc oxidation coating is composed of a dense layer and a porous layer, and has good initial corrosion protection function; the micro-arc oxidation coating phase is mainly Mg2SiO4, which has good chemical stability, low ion dissolution rate, and good wear resistance; the porous structure can be used as a loading material for iron-rich compounds; the iron-rich compounds and polylactic acid are used together to seal the porous structure; the dense layer of the micro-arc oxidation coating is rich in F elements, which can effectively inhibit the direct contact between the iron-rich compounds and the magnesium matrix, thereby avoiding affecting the initial corrosion resistance.
[0025] 2) The micro-arc oxidation coated magnesium alloy was treated with a divalent ferrous ion solution. The electrodeposition method achieved the directional deposition of iron-rich compounds and reduced the chemical dissolution of the micro-arc oxidized magnesium alloy in the acidic ferrous ion solution. The iron-rich compounds were mainly deposited in the microporous structure in the form of FeOOH and a small amount of divalent ferrous compounds, and the iron-rich compounds were richly loaded.
[0026] 3) The polylactic acid coating is biodegradable, and its degradation products will not pollute the environment; it has good thermal stability and can stably serve within 100°C, meeting the service conditions; in the early stage of service, it can effectively prevent corrosive media from penetrating into the coating and prevent the chemical dissolution of iron-rich compounds.
[0027] 4) In the early stage of service, the composite coating has excellent corrosion protection ability because the coating is relatively dense. During the service process, the mechanical-chemical coupling causes damage to the coating, and the corrosive medium will penetrate into the interior of the coating until it penetrates into the interface between the coating and the substrate. A large amount of corrosive medium will penetrate and exist at the interface between the polymer coating and the micro-arc oxidation coating. The iron-rich compound has a large solubility in the aqueous solution medium and is easy to dissolve trivalent iron ions. When the trivalent iron ions come into contact with the substrate, the magnesium alloy substrate will be severely corroded. The reduced divalent iron ions are easily oxidized to form trivalent iron ions, which then show catalytic corrosion behavior. Even if the oxygen content in the service environment is insufficient, the divalent iron ions will be reduced to elemental iron, and iron and magnesium will form a galvanic pair, which will show galvanic corrosion behavior.
[0028] 5) During the service process, the polylactic acid will swell and break locally, and a large amount of corrosive media will penetrate and exist at the interface between the upper polylactic acid layer and the micro-arc oxidation coating. Due to the existence of the upper polylactic acid layer, the iron-rich compounds in the micropores of the micro-arc oxidation coating are not easy to dissolve into the open environmental solution, and the iron ions are confined to the damaged part of the coating, causing the corrosion rate to accelerate.
[0029] 6) The present invention relates to a surface coating for step-by-step regulation of magnesium alloy degradation, as well as a preparation method and application thereof. The surface coating is not limited to the composition of the magnesium alloy matrix material and can retain the physical and chemical properties of the magnesium alloy matrix material. The surface coating can also achieve the service characteristics of good initial corrosion resistance and rapid degradation in the later stage of the magnesium alloy, thus meeting the reliable and safe service requirements of the soluble fracturing ball.
[0030] The invention relates to a surface coating for step-by-step regulation of magnesium alloy degradation, a preparation method and an application thereof. The surface coating is made of degradable and environmentally friendly materials and will not pollute the medium environment.
[0031] The present invention discloses a surface coating for regulating the degradation of magnesium alloy in stages, and a preparation method and application thereof, and relates to the surface treatment of magnesium alloy for soluble fracturing balls. The preparation method comprises the following steps: S1, preparation of micro-arc oxidation coating on the surface of magnesium alloy; S2, deposition of iron-rich compounds on the porous structure of micro-arc oxidation coating; S3, coating of polymer coating. The composite coating has the characteristics of good initial corrosion protection and later promotion of degradation, and can be applied to oil and gas production and other fields requiring staged degradation. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The cross-sectional morphology and element analysis diagram of the composite coating on the surface of the magnesium alloy prepared in Example 1 of the present invention;
[0033] Figure 2 is the wear rate of the surface coating magnesium alloy in Examples 1-3 of the present invention and Comparative Examples 1-3;
[0034] Figure 3 It is the dissolution rate of the surface coating magnesium alloy in Examples 1-3 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0036] Example 1
[0037] A method for preparing a surface coating for step-by-step regulation of magnesium alloy degradation comprises the following steps:
[0038] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 20g / L Na2SiO3·9H2O, 1g / L NaOH and 4g / L KF·2H2O, and the solvent is water; constant current mode: forward current is 10A / dm 2 , negative current is 0A / dm 2 , frequency 500Hz, duty cycle: 15%, termination voltage 450V.
[0039] S2. Deposition of iron-rich compounds on porous structure of micro-arc oxidation coating: micro-arc oxidation magnesium alloy was used as cathode and stainless steel as anode. The electrodeposition solution was 0.005 mol / L FeCl2 solution, the solvent was water, the voltage was set to 2.0 V, and the treatment time was 10 min.
[0040] S3. Degradable polymer coating: The polylactic acid coating was prepared by the immersion pulling method; the molecular weight of polylactic acid was 40,000, and polylactic acid was dissolved in a dichloromethane solution at a ratio of 50 g / L; the immersion pulling rate was 0.5 mm / s, and the pulling was performed 3 times.
[0041] A surface coating for step-by-step regulation of magnesium alloy degradation comprises a micro-arc oxidation coating, wherein the micro-arc oxidation coating comprises a fluorine-rich dense layer bonded to a magnesium alloy substrate and a porous layer located above the dense layer; the iron-rich layer penetrates into the microporous structure of the porous layer, and above the porous layer is a degradable polymer layer with swelling properties.
[0042] Application of a surface coating for step-by-step regulation of magnesium alloy degradation in soluble magnesium alloy fracturing balls.
[0043] A soluble magnesium alloy fracturing ball comprises a surface coating of the present embodiment for regulating the degradation of the magnesium alloy in stages.
[0044] The invention discloses an application of a soluble magnesium alloy fracturing ball in oil and gas production.
[0045] Example 2
[0046] A method for preparing a surface coating for step-by-step regulation of magnesium alloy degradation comprises the following steps:
[0047] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 30g / L Na2SiO3·9H2O, 2g / L NaOH and 8g / L KF·2H2O; constant current mode: forward current is 20A / dm 2 , negative current is 5A / dm 2 , frequency 1000Hz, duty cycle: 30%, termination voltage 500V.
[0048] S2. Deposition of iron-rich compounds on porous structure of micro-arc oxidation coating: using micro-arc oxidation magnesium alloy as cathode and stainless steel as anode, the electrodeposition solution is 0.015 mol / L FeCl2 solution, the voltage is set to 3.0 V, and the treatment time is 20 min.
[0049] S3. Degradable polymer coating: The polylactic acid coating was prepared by the immersion pulling method; the polylactic acid had a molecular weight of 150,000 and was dissolved in a dichloromethane solution at a ratio of 100 g / L; the immersion pulling rate was 1 mm / s, and the pulling was performed 5 times.
[0050] A surface coating for step-by-step regulation of magnesium alloy degradation comprises a micro-arc oxidation coating, wherein the micro-arc oxidation coating comprises a fluorine-rich dense layer bonded to a magnesium alloy substrate and a porous layer located above the dense layer; the iron-rich layer penetrates into the microporous structure of the porous layer, and above the porous layer is a degradable polymer layer with swelling properties.
[0051] Application of a surface coating for step-by-step regulation of magnesium alloy degradation in soluble magnesium alloy fracturing balls.
[0052] A soluble magnesium alloy fracturing ball comprises a surface coating of the present embodiment for regulating the degradation of the magnesium alloy in stages.
[0053] The invention discloses an application of a soluble magnesium alloy fracturing ball in oil and gas production.
[0054] Example 3
[0055] A method for preparing a surface coating for step-by-step regulation of magnesium alloy degradation comprises the following steps:
[0056] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 25g / L Na2SiO3·9H2O, 1.2g / L NaOH, 6g / L KF·2H2O; constant current mode: forward current is 12A / dm 2 , negative current is 2A / dm 2 , frequency 600Hz, duty cycle: 20%, and termination voltage 470V.
[0057] S2. Deposition of iron-rich compounds on porous structure of micro-arc oxidation coating: using micro-arc oxidation magnesium alloy as cathode and stainless steel as anode, the electrodeposition solution is 0.010 mol / L FeCl2 solution, the voltage is set to 2.5 V, and the treatment time is 15 min.
[0058] S3. Degradable polymer coating: The polylactic acid coating was prepared by the immersion pulling method; the polylactic acid had a molecular weight of 100,000 and was dissolved in a dichloromethane solution at a ratio of 75 g / L; the immersion pulling rate was 0.6 mm / s, and the pulling was performed 4 times.
[0059] A surface coating for step-by-step regulation of magnesium alloy degradation comprises a micro-arc oxidation coating, wherein the micro-arc oxidation coating comprises a fluorine-rich dense layer bonded to a magnesium alloy substrate and a porous layer located above the dense layer; the iron-rich layer penetrates into the microporous structure of the porous layer, and above the porous layer is a degradable polymer layer with swelling properties.
[0060] Application of a surface coating for step-by-step regulation of magnesium alloy degradation in soluble magnesium alloy fracturing balls.
[0061] A soluble magnesium alloy fracturing ball comprises a surface coating of the present embodiment for regulating the degradation of the magnesium alloy in stages.
[0062] The invention discloses an application of a soluble magnesium alloy fracturing ball in oil and gas production.
[0063] Comparative Example 1
[0064] A method for preparing a surface coating for regulating the degradation of a magnesium alloy comprises the following steps:
[0065] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 20g / L Na2SiO3·9H2O, 1g / L NaOH, 4g / L KF·2H2O; constant current mode: forward current is 10A / dm 2 , negative current is 0A / dm 2 , frequency 500Hz, duty cycle: 15%, termination voltage 450V.
[0066] S2. Deposition of iron-rich compounds on porous structure of micro-arc oxidation coating: using micro-arc oxidation magnesium alloy as cathode and stainless steel as anode, the electrodeposition solution is 0.005 mol / L FeCl2 solution, the voltage is set to 2.0 V, and the treatment time is 10 min.
[0067] Comparative Example 2
[0068] A method for preparing a surface coating for regulating the degradation of a magnesium alloy comprises the following steps:
[0069] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 20g / L Na2SiO3·9H2O, 1g / L NaOH, 4g / L KF·2H2O; constant current mode: forward current is 10A / dm2 , negative current is 0A / dm 2 , frequency 500Hz, duty cycle: 15%, termination voltage 450V.
[0070] S2. Degradable polymer coating: The polylactic acid coating was prepared by the immersion pulling method; the polylactic acid had a molecular weight of 40,000 and was dissolved in a dichloromethane solution at a ratio of 50 g / L; the immersion pulling rate was 0.5 mm / s, and the pulling was performed 3 times.
[0071] Comparative Example 3
[0072] A method for preparing a surface coating for regulating the degradation of a magnesium alloy comprises the following steps:
[0073] S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: The soluble magnesium alloy for fracturing ball is placed in a silicate system micro-arc oxidation electrolyte for micro-arc oxidation treatment; the electrolyte composition is 30g / L Na2SiO3·9H2O, 2g / L NaOH, 8g / L KF·2H2O; constant current mode: forward current is 20A / dm 2 , negative current is 5A / dm 2 , frequency 1000Hz, duty cycle: 30%, termination voltage 500V.
[0074] S2. Deposition of iron-rich compounds on porous structure of micro-arc oxidation coating: The micro-arc oxidized magnesium alloy was immersed in a 50°C, 0.015 mol / L FeCl2 solution for 20 min.
[0075] S3. Degradable polymer coating: The polylactic acid coating on the surface of the magnesium alloy was prepared by the immersion pulling method; the polylactic acid had a molecular weight of 150,000 and was dissolved in a dichloromethane solution at a ratio of 100 g / L; the immersion pulling rate was 1 mm / s, and the pulling was performed 5 times.
[0076] That is, S2 of this comparative example adopts the impregnation method to deposit the iron-rich compound.
[0077] Characterization results
[0078] Figure 1 The cross-sectional morphology and elemental analysis diagram of the composite coating on the surface of the magnesium alloy prepared in Example 1. The coating comprises a micro-arc oxidation layer, an iron-rich layer, and a polymer layer, wherein the iron-rich layer penetrates into the microporous structure of the micro-arc oxidation layer, and the fluorine-rich layer in the micro-arc oxidation layer can effectively inhibit the iron-rich compound from continuing to penetrate into the coating and the substrate.
[0079] The wear resistance and corrosion resistance of the surface coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated. Figure 2is the wear rate of the surface coating (25N, 20mm / s, the friction pair is Al2O3 ball). The surface coating can effectively improve the wear resistance of the magnesium alloy, but the micro-arc oxidation coating in Comparative Example 3 will be corroded and dissolved by the acidic ferrous chloride solution, and the wear resistance is slightly reduced. Figure 3 The dissolution rate of the coated magnesium alloy in a 3wt.% KCl solution, the surface coatings prepared in Examples 1 to 3 have good initial corrosion resistance in KCl solution and a step-by-step degradation characteristic of promoting the dissolution of the magnesium alloy in the later stage. The surface coating prepared in Comparative Example 1 has poor initial corrosion resistance because it is not enclosed by an outer polymer coating; the ability to promote the dissolution of the magnesium alloy in the later stage is reduced due to the dissolution of iron ions into the open solution medium environment. The surface coating prepared in Comparative Example 2 does not contain an iron-rich layer, so the coating does not have the ability to promote the dissolution of the magnesium alloy in the later stage. The iron-rich layer of the surface coating prepared in Comparative Example 3 is not effectively deposited into the micropores of the micro-arc oxidation coating, the amount of iron-rich compound deposition is small, and the micro-arc oxidation coating undergoes corrosion and dissolution when immersed in an acidic ferrous chloride solution, so the initial corrosion resistance and the ability to promote degradation in the later stage are both poor.
[0080] It should be understood that in order to streamline the present disclosure and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting the intention that the claimed invention requires more features than those expressly recited in each claim. Rather, as reflected in the claims, inventive aspects lie in less than all of the features of the previously disclosed embodiments. Therefore, the claims that follow the detailed description are hereby expressly incorporated into the detailed description, with each claim itself serving as a separate embodiment of the present invention.
[0081] Although the present invention has been described according to a limited number of embodiments, it will be apparent to those skilled in the art, with the benefit of the above description, that other embodiments may be envisioned within the scope of the invention thus described. In addition, it should be noted that the language used in this specification is selected primarily for readability and teaching purposes, rather than for explaining or defining the subject matter of the present invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the present invention is illustrative, not restrictive, with respect to the scope of the present invention, which is defined by the appended claims.
[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A surface coating for step-by-step regulation of magnesium alloy degradation. It is characterized in that The micro-arc oxidation coating includes a fluorine-rich dense layer bonded to a magnesium alloy substrate and a porous layer located above the dense layer; the iron-rich layer penetrates into the microporous structure of the porous layer, and a degradable polymer layer with swelling properties is located above the porous layer; The preparation method comprises the following steps: S1. Preparation of micro-arc oxidation coating on magnesium alloy surface: placing magnesium alloy for soluble fracturing ball in micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain micro-arc oxidation coating; S2. Deposition of iron-rich compounds on porous structures of micro-arc oxidation coatings: Electrodeposition of iron-rich compounds on soluble magnesium alloy for fracturing balls after micro-arc oxidation treatment; S3, coating of degradable polymer coating: the polymer coating is prepared by immersion and pulling method; in S3, the degradable polymer coating is polylactic acid, with a molecular weight of 40,000 to 150,000, dissolved in a dichloromethane solution at a ratio of 50 to 100 g / L; the immersion and pulling rate is 0.5 to 1 mm / s, and the pulling is performed 3 to 5 times; Among them: In S1, the micro-arc oxidation electrolyte is a silicate system aqueous solution, and its electrolyte composition is 20~30g / L Na 2 SiO 3 9H 2 O, 1~2g / L NaOH and 4~8g / L KF·2H 2 O.
2. A surface coating for stepwise regulation of magnesium alloy degradation according to claim 1, It is characterized in that In S1, the process of micro-arc oxidation treatment is: Constant current mode: forward current is 10~20A / dm 2 , negative current is 0~5A / dm 2 , frequency 500~1000Hz, duty cycle: 15~30%, termination voltage 450~500V.
3. The surface coating for step-by-step regulation of magnesium alloy degradation according to claim 1, It is characterized in that In S2, during the electrodeposition, the magnesium alloy after micro-arc oxidation is the cathode, the stainless steel is the anode, and the electrodeposition solution is 0.005~0.015mol / L FeCl 2 solution, voltage is 2.0~3.0V, and processing time is 10~20min.
4. Application of a surface coating for step-by-step regulation of magnesium alloy degradation according to claim 1 in a soluble magnesium alloy fracturing ball.
5. A soluble magnesium alloy fracturing ball, It is characterized in that It comprises a surface coating for step-by-step regulation of magnesium alloy degradation as described in claim 1.
6. Use of the soluble magnesium alloy fracturing ball according to claim 5 in oil and gas production.