Desulfurization method for full waste steel electric furnace process

Through the electric furnace plus VD vacuum degassing process, combined with foam slag and slag elution and sulfur treatment, the problem of nitrogen removal in electric furnace steelmaking is solved, and efficient control of liquid steel composition and production of advanced steel is achieved.

CN119061235AActive Publication Date: 2024-12-03SHOUGANG GROUP CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411229346.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The lack of desulfurization facilities during the electric furnace steelmaking process leads to a lot of raw material impurities and the refining process is difficult to achieve efficient nitrogen removal and dehydrogenation. The traditional LF refining process is prone to nitrogen increase and difficult to denitrogenation.

Method used

The electric furnace plus VD vacuum degassing process is adopted, and the foaming slag slag elution and VD vacuum degassing treatment of the smelting steel liquid can be achieved, desulfurization, nitrogen removal and dehydrogenation of the steel liquid can be achieved, and the target components are achieved.

Benefits of technology

Rapidly realize the desulfurization, nitrogen removal and dehydrogenation of high-grade steel, which improves the problem of nitrogen increase in electric furnace steelmaking during the desulfurization process, and achieves efficient control of liquid steel composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061235A_ABST
    Figure CN119061235A_ABST
Patent Text Reader

Abstract

The invention relates to a desulfurization method for a full scrap steel electric furnace process, and belongs to the technical field of metal smelting. The method comprises the steps that an electric furnace is adopted for smelting full scrap steel, foaming slag making treatment is carried out, and smelted molten steel is obtained; tapping the smelted molten steel, and carrying out slag washing desulfurization to obtain intermediate molten steel; the intermediate molten steel is subjected to VD vacuum degassing treatment, desulfurized molten steel is obtained, and desulfurization is completed; according to the method, the electric furnace and VD vacuum degassing technology is adopted, the requirements for desulfurization, denitrification and dehydrogenation of high-grade steel are rapidly met, target components are achieved, and the effect of solving the problem that nitrogen is likely to be increased in the desulfurization process of electric furnace steelmaking is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal smelting, and in particular to a desulfurization method for a full scrap steel electric furnace process. Background Art

[0002] At present, the steel industry is still heavily dependent on coal-based fossil energy, with large carbon emissions. Therefore, effectively reducing carbon emissions in the steel production process has become a major issue that the steel industry and even the country need to solve urgently. The low steel ratio of electric furnaces is one of the important reasons for the large carbon emissions, high energy consumption and heavy pollution in the steel industry. The advantages of developing short-process electric furnaces in energy conservation and emission reduction are very obvious.

[0003] As users' requirements for steel quality continue to increase, the requirements for the cleanliness of molten steel are also getting higher and higher, especially the requirements for sulfur elements are very strict. Most domestic steel mills use a long converter process for production, which can be desulfurized by pretreatment of molten iron. The electric furnace process does not have desulfurization facilities, so it has strict requirements on raw materials and refining processes. However, since the raw materials used in the electric furnace process are mainly scrap steel, the source range is wide and there are many impurity elements, which brings challenges to the desulfurization of electric furnace production. The traditional process is to use an electric furnace plus LF desulfurization process, but the LF refining process is easy to increase nitrogen, and the whole process is difficult to denitrify and dehydrogenate. Summary of the invention

[0004] The present application provides a desulfurization method for a full scrap steel electric furnace process, so as to improve the problem of easy nitrogen increase during the desulfurization process of current electric furnace steelmaking.

[0005] The present application provides a desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0006] The whole scrap steel is smelted by an electric furnace and foamed slag is processed to obtain molten steel;

[0007] tapping the smelted steel liquid, and performing slag washing and desulfurization to obtain intermediate steel liquid;

[0008] The intermediate molten steel is subjected to VD vacuum degassing treatment to obtain desulfurized molten steel, thereby completing desulfurization.

[0009] As an optional implementation manner, the vacuum degree of the VD vacuum degassing treatment is 60Pa to 80Pa; and / or

[0010] The VD vacuum degassing treatment time is 10 min to 30 min.

[0011] As an optional embodiment, the composition of the whole scrap steel includes, by mass fraction: C: 0.03% to 20%, Si: 0.15% to 0.5%, Mn: 0.10% to 0.5%, P: 0.005% to 0.045%, S: 0.002% to 0.035%, and the rest is Fe and unavoidable impurities.

[0012] As an optional embodiment, the oxygen supply during the smelting process is 25m 3 / t steel~42m 3 / t steel; and / or

[0013] The number of oxygen lances for supplying oxygen in the smelting process is no less than 3.

[0014] As an optional embodiment, the foaming slag treatment includes adding first lime, dolomite and carbon powder during the smelting process.

[0015] As an optional embodiment, the amount of the first lime added is 35kg / t steel to 40kg / t steel; and / or

[0016] The amount of dolomite added is 6kg / t steel to 10kg / t steel; and / or

[0017] The amount of carbon powder added is 20kg / t steel to 30kg / t steel.

[0018] As an optional embodiment, the slag washing and desulfurization includes adding aluminum, a second lime and fluorite during the steel tapping process.

[0019] As an optional embodiment, the amount of aluminum added is 2kg / t steel to 2.3kg / t steel; and / or

[0020] The amount of the second lime added is 12kg / t steel to 18kg / t steel; and / or

[0021] The added amount of fluorite is 4kg / t steel to 8kg / t steel.

[0022] As an optional implementation manner, the start timing of the steel tapping satisfies at least one of the following:

[0023] a) the mass content of carbon in the smelting molten steel is 0.03% to 0.2%;

[0024] b) the mass content of phosphorus in the smelting molten steel is not higher than 0.02%;

[0025] c) the mass content of sulfur in the smelting molten steel is not higher than 0.12%;

[0026] d) The temperature of the smelting molten steel is 1600°C to 1680°C.

[0027] As an optional embodiment, the composition of the desulfurized steel liquid includes, by mass fraction: C: 0.03%~0.60%, Si: 0.05%~0.50%, Mn: 0.05%~0.95%, P: <0.015%, S: <0.010%, Als: 0.010%~0.050%, and the rest is Fe and unavoidable impurities.

[0028] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0029] The method provided in the embodiment of the present application adopts an electric furnace plus VD vacuum degassing process to quickly achieve the requirements of desulfurization, denitrification and dehydrogenation of high-grade steel, achieve the target composition, and improve the problem of nitrogen increase that is easy to occur during the desulfurization process of electric furnace steelmaking. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0032] Figure 1 A flowchart of the method provided in the embodiment of the present application. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0035] The electric furnace process does not have desulfurization facilities, so it has strict requirements on raw materials and refining processes. Since the raw materials used in the electric furnace process are mainly scrap steel, which has a wide range of sources and many impurity elements, it brings challenges to the desulfurization of electric furnace production. The traditional process is to use an electric furnace plus LF desulfurization process, but the LF refining process is prone to nitrogen addition, and the whole process is difficult to denitrify and dehydrogenate.

[0036] To this end, the present application intends to provide a method for desulfurization of an all-scrap steel electric furnace process. Since the raw materials of the electric arc furnace contain many harmful elements, the process settings have been optimized, and an electric arc furnace plus VD vacuum degassing process has been adopted to quickly achieve the requirements of desulfurization, denitrification and dehydrogenation of high-grade steel and achieve the target composition.

[0037] Figure 1 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 1 As shown, the embodiment of the present application provides a desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0038] S1. Using an electric furnace (or arc furnace) to smelt all scrap steel and perform foam slag treatment to obtain molten steel;

[0039] In some embodiments, the composition of the whole scrap steel includes, by mass fraction, C: 0.03% to 20%, Si: 0.15% to 0.5%, Mn: 0.10% to 0.5%, P: 0.005% to 0.045%, S: 0.002% to 0.035%, and the rest is Fe and unavoidable impurities.

[0040] In some embodiments, the oxygen supply during the smelting process is 25m 3 / t steel~42m 3 / t steel; the number of oxygen lances for supplying oxygen in the smelting process is not less than 3.

[0041] For example, the oxygen supply during the smelting process may be 25 m 3 / t steel, 26m 3 / t steel, 27m 3 / t steel, 28m 3 / t steel, 29m 3 / t steel, 30m 3 / t steel, 31m 3 / t steel, 32m 3 / t steel, 33m 3 / t steel, 34m 3 / t steel, 35m 3 / t steel, 36m 3 / t steel, 37m 3 / t steel, 38m 3 / t steel, 39m 3 / t steel, 40m 3 / t steel, 41m 3 / t steel or 42m 3 / t steel, etc., which can also be 25m 3 / t steel~42m 3 / t steel range. It should be noted that m 3 / t steel refers to the oxygen supply volume per ton of scrap steel. For example, the oxygen supply volume is 2 5m 3 / t steel means the oxygen supply for every ton of scrap steel is 25m 3 .

[0042] In some embodiments, the foaming slag treatment includes adding first lime, dolomite and carbon powder during the smelting process, wherein the first lime is added in an amount of 35kg / t steel to 40kg / t steel, the dolomite is added in an amount of 6kg / t steel to 10kg / t steel, and the carbon powder is added in an amount of 20kg / t steel to 30kg / t steel.

[0043] Lime is an air-hardening inorganic cementitious material with calcium oxide as its main component. Lime is made from limestone, dolomite, chalk, shells and other products with high calcium carbonate content, calcined at 900-1100℃.

[0044] The chemical composition of dolomite includes CaMg(CO3)2, and the crystal belongs to the trigonal carbonate mineral. There are iron dolomite and manganese dolomite. The crystal structure of dolomite is similar to that of calcite. The crystal shape is rhombohedral, and the crystal face is often bent into a saddle shape. Polysynthetic twins are common, and they are mostly blocky and granular aggregates.

[0045] Exemplarily, the amount of carbon powder added can be 20kg / t steel, 21kg / t steel, 22kg / t steel, 23kg / t steel, 24kg / t steel, 25kg / t steel, 26kg / t steel, 27kg / t steel, 28kg / t steel, 29kg / t steel or 30kg / t steel, etc., and it can also be any value within the range of 20kg / t steel to 30kg / t steel. It should be noted that kg / t steel refers to the mass amount of the first lime, dolomite or carbon powder corresponding to each ton of scrap steel. For example, the amount of carbon powder added is 20kg / t steel, which means that the amount of carbon powder corresponding to each ton of scrap steel is 20kg.

[0046] S2. tapping the smelted steel and performing slag washing and desulfurization to obtain an intermediate steel liquid;

[0047] In some embodiments, the timing of starting steel tapping is to meet at least one of the following conditions: a) the mass content of carbon in the smelting steel liquid is 0.03% to 0.2%; b) the mass content of phosphorus in the smelting steel liquid is not higher than 0.02%; c) the mass content of sulfur in the smelting steel liquid is not higher than 0.12%; d) the temperature of the smelting steel liquid is 1600℃ to 1680℃.

[0048] In some embodiments, the slag washing and desulfurization includes adding aluminum, a second lime and fluorite during the steel tapping process.

[0049] The amount of aluminum added is 2kg / t steel to 2.3kg / t steel; the amount of the second lime added is 12kg / t steel to 18kg / t steel; the amount of fluorite added is 4kg / t steel to 8kg / t steel.

[0050] S3. Performing VD vacuum degassing treatment on the intermediate molten steel to obtain desulfurized molten steel, thereby completing desulfurization.

[0051] In some embodiments, the vacuum degree of the VD vacuum degassing treatment is 60Pa to 80Pa; the time of the VD vacuum degassing treatment is 10min to 30min. By controlling the vacuum degree and treatment time of the VD vacuum degassing treatment within an appropriate range, it is beneficial to remove sulfur and thus achieve the target composition.

[0052] In some embodiments, the composition of the desulfurized steel liquid includes, by mass fraction: C: 0.03% to 0.60%, Si: 0.05% to 0.50%, Mn: 0.05% to 0.95%, P: <0.015%, S: <0.010%, Als: 0.010% to 0.050%, and the rest is Fe and unavoidable impurities.

[0053] Specifically, in this embodiment, the desulfurization process of the entire all-scrap steel electric furnace process can be as follows: all scrap steel is added into the electric furnace, and then the electric furnace is powered on (powered by a 45MVA transformer), and oxygen is blown for smelting; lime, dolomite, and carbon powder are added during the smelting process to make foamed slag until the steel tapping end requirements are met: carbon 0.03% to 0.20%, phosphorus not higher than 0.020%, sulfur not higher than 0.12%, and temperature 1600°C to 1680°C; then aluminum, lime, and fluorite are added to the steel for slag washing and desulfurization; the molten steel enters the VD vacuum degassing device for vacuum stirring; the vacuum degree is 67Pa, and the vacuum time is 20 minutes.

[0054] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0055] Example 1

[0056] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0057] S1. Using a 70-ton electric furnace to smelt 72 tons of all scrap steel, the smelting process was added first lime, dolomite, carbon powder to make foam slag to obtain smelting molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 500kg, the amount of carbon powder is 50kg;

[0058] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0059] S3. The intermediate molten steel is subjected to VD vacuum degassing treatment to obtain desulfurized molten steel and complete desulfurization; wherein the vacuum degree of the VD vacuum degassing treatment is 67 Pa and the vacuum time is 20 minutes.

[0060] The composition of molten steel in each smelting process is shown in the following table:

[0061]

[0062] Example 2

[0063] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0064] S1. Using a 70-ton electric furnace to smelt 72 tons of all scrap steel, the smelting process was added first lime, dolomite, carbon powder to make foam slag to obtain smelting molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 500kg, the amount of carbon powder is 50kg;

[0065] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0066] S3. The intermediate molten steel is subjected to VD vacuum degassing treatment to obtain desulfurized molten steel and complete desulfurization; wherein the vacuum degree of the VD vacuum degassing treatment is 67 Pa and the vacuum time is 20 minutes.

[0067] The composition of molten steel in each smelting process is shown in the following table:

[0068]

[0069] Example 3

[0070] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0071] S1. Using a 70-ton electric furnace to smelt 72 tons of all scrap steel, the smelting process was added first lime, dolomite, carbon powder to make foam slag to obtain smelting molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 500kg, the amount of carbon powder is 50kg;

[0072] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0073] S3. The intermediate molten steel is subjected to VD vacuum degassing treatment to obtain desulfurized molten steel and complete desulfurization; wherein the vacuum degree of the VD vacuum degassing treatment is 67 Pa and the vacuum time is 20 minutes.

[0074] The composition of molten steel in each smelting process is shown in the following table:

[0075]

[0076]

[0077] Comparative Example 1

[0078] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0079] S1. A 70-ton electric furnace is used to smelt 72 tons of all scrap steel. During the smelting process, lime, dolomite and carbon powder are added to make foam slag to obtain molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 100kg, and the amount of carbon powder is 50kg;

[0080] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0081] S3. Perform LF smelting treatment on the intermediate molten steel to obtain desulfurized molten steel, thereby completing desulfurization.

[0082] The composition of molten steel in each smelting process is shown in the following table:

[0083]

[0084] Comparative Example 2

[0085] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0086] S1. A 70-ton electric furnace is used to smelt 72 tons of all scrap steel. During the smelting process, lime, dolomite and carbon powder are added to make foam slag to obtain molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 100kg, and the amount of carbon powder is 50kg;

[0087] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0088] S3. Perform LF smelting treatment on the intermediate molten steel to obtain desulfurized molten steel, thereby completing desulfurization.

[0089] The composition of molten steel in each smelting process is shown in the following table:

[0090]

[0091] Comparative Example 3

[0092] A desulfurization method for a full scrap steel electric furnace process, the method comprising:

[0093] S1. Using a 70-ton electric furnace to smelt 72 tons of all scrap steel, the smelting process was added first lime, dolomite, carbon powder to make foam slag to obtain smelting molten steel; wherein the first amount of lime is 2500kg, the amount of dolomite is 500kg, the amount of carbon powder is 50kg;

[0094] S2. The smelted steel liquid is tapped, and aluminum, a second lime, and fluorite are added during the tapping process to perform slag washing and desulfurization to obtain an intermediate steel liquid; wherein the amount of aluminum is 132 kg, the amount of the second lime is 1000 kg, and the amount of fluorite is 200 kg.

[0095] S3. Perform LF smelting treatment on the intermediate molten steel to obtain desulfurized molten steel, thereby completing desulfurization.

[0096] The composition of molten steel in each smelting process is shown in the following table:

[0097]

[0098] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0099] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.

[0100] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A desulfurization method for a full scrap steel electric furnace process, characterized in that: The method comprises: The whole scrap steel is smelted by an electric furnace and foamed slag is processed to obtain molten steel; tapping the smelted steel liquid, and performing slag washing and desulfurization to obtain intermediate steel liquid; The intermediate molten steel is subjected to VD vacuum degassing treatment to obtain desulfurized molten steel, thereby completing desulfurization.

2. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The vacuum degree of the VD vacuum degassing treatment is 60Pa to 80Pa; and / or The VD vacuum degassing treatment time is 10 min to 30 min.

3. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The components of the whole scrap steel include, by mass fraction, C: 0.03% to 20%, Si: 0.15% to 0.5%, Mn: 0.10% to 0.5%, P: 0.005% to 0.045%, S: 0.002% to 0.035%, and the rest are Fe and unavoidable impurities.

4. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The oxygen supply during the smelting process is 25m 3 / t steel~42m 3 / t steel; and / or The number of oxygen lances for supplying oxygen in the smelting process is no less than 3.

5. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The foaming slag process includes adding first lime, dolomite and carbon powder during the smelting process.

6. The desulfurization method of the all-scrap steel electric furnace process according to claim 5, characterized in that: The amount of the first lime added is 35kg / t steel to 40kg / t steel; and / or The amount of dolomite added is 6kg / t steel to 10kg / t steel; and / or The amount of carbon powder added is 20kg / t steel to 30kg / t steel.

7. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The slag washing and desulfurization includes adding aluminum, second lime and fluorite during the steel tapping process.

8. The desulfurization method of the all-scrap steel electric furnace process according to claim 7, characterized in that: The amount of aluminum added is 2kg / t steel to 2.3kg / t steel; and / or The amount of the second lime added is 12kg / t steel to 18kg / t steel; and / or The added amount of fluorite is 2kg / t steel to 4kg / t steel.

9. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The start timing of steel tapping satisfies at least one of the following: a) the mass content of carbon in the smelting molten steel is 0.03% to 0.2%; b) the mass content of phosphorus in the smelting molten steel is not higher than 0.02%; c) the mass content of sulfur in the smelting molten steel is not higher than 0.12%; d) The temperature of the smelting molten steel is 1600°C to 1680°C.

10. The desulfurization method of the all-scrap steel electric furnace process according to claim 1, characterized in that: The components of the desulfurized steel liquid include, by mass fraction: C: 0.03%-0.60%, Si: 0.05%-0.50%, Mn: 0.05%-0.95%, P: <0.015%, S: <0.010%, Als: 0.010%-0.050%, and the rest are Fe and unavoidable impurities.

Citation Information

Patent Citations

  • Production method for ultralow-phosphorus hydroforming steel

    CN107868900A

  • Method for desulfurization though VD furnace

    CN111411196A

  • Electric furnace full scrap steel smelting process

    CN113215354A

  • Electric arc furnace smelting method based on hot charging of molten iron

    CN114107598A

  • Electric furnace smelting method for full scrap steel

    CN114107599A