Preparation method of perovskite thin film and perovskite solar cell

By introducing organic materials such as PMMA in the preparation process of perovskite film, porous lead iodide film is formed and reacted with organic amine salts, the problem of lead iodide residue is solved, and the quality of perovskite film and the efficiency of solar cells is improved.

CN119072201AActive Publication Date: 2024-12-03HUANENG RENEWABLES CORPORATION LIMITED +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310632459.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

During the existing two-step perovskite film preparation process, the dense lead iodide film cannot fully react with the organic amine salt, resulting in too much lead iodide residue in the perovskite film, affecting device performance.

Method used

By introducing organic sacrificial materials such as PMMA into the lead iodide layer, a porous lead iodide film is deposited and reacted with the organic amine salt solution, thereby promoting the complete conversion of lead iodide into a perovskite film.

Benefits of technology

It effectively reduces the residue of lead iodide, improves the quality of perovskite films and the photoelectric conversion efficiency of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004258890610000011
    Figure HDA0004258890610000011
  • Figure HDA0004258890610000012
    Figure HDA0004258890610000012
  • Figure HDA0004258890610000021
    Figure HDA0004258890610000021
Patent Text Reader

Abstract

The invention provides a preparation method of a perovskite thin film, which comprises the following steps of: depositing a lead iodide solution on a substrate, and performing primary annealing to obtain a lead iodide thin film; soaking the lead iodide thin film in an anti-solvent and then carrying out secondary annealing to obtain a porous lead iodide thin film; reacting the porous lead iodide thin film with an organic amine salt solution to obtain a perovskite thin film; the lead iodide solution contains PMMA (polymethyl methacrylate). The porous lead iodide is prepared by introducing the organic sacrificial material into the lead iodide layer, so that a channel is provided for diffusion and reaction of organic amine salt, and the lead iodide is promoted to be completely converted into perovskite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a method for preparing a perovskite film and a perovskite solar cell. Background Art

[0002] In recent years, solar cell technology has made great progress. The current photoelectric conversion efficiency of perovskite solar cells has exceeded 25%, which is comparable to that of crystalline silicon solar cells. Perovskite solar cells use organic-metal halides with a perovskite lattice structure as the light absorption layer. This material has excellent photoelectric properties such as narrow band gap, strong light absorption, and high carrier mobility. The preparation methods of organic-metal halides usually include solution method, evaporation method, and liquid / gas phase mixed deposition method. In the solution method, the two-step sequential deposition method can easily achieve the preparation of dense perovskite films, laying the foundation for high-performance perovskite solar cells. In the traditional two-step solution method, lead iodide is first deposited on the substrate, and then the organic amine salt solution is deposited on the lead iodide layer, contacting and reacting with the lead iodide to form a perovskite light absorption layer. However, the first deposited lead iodide will form a dense film that cannot fully react with the organic amine salt, which causes a large amount of lead iodide residue in the film, thereby affecting the device performance. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a method for preparing a perovskite film and a perovskite solar cell, so as to solve the problem that in the existing two-step perovskite film preparation process, a dense lead iodide film cannot completely react with an organic amine salt, resulting in excessive lead iodide residue in the final perovskite film.

[0004] The present invention provides a method for preparing a perovskite film, comprising:

[0005] After the lead iodide solution is deposited on the substrate, annealing is performed once to obtain a lead iodide film;

[0006] The lead iodide film is immersed in an anti-solvent and then subjected to secondary annealing to obtain a porous lead iodide film;

[0007] reacting the porous lead iodide film with an organic amine salt solution to obtain a perovskite film;

[0008] The lead iodide solution contains PMMA (polymethyl methacrylate).

[0009] In an embodiment of the present invention, the lead iodide solution may include: lead iodide, PMMA and a solvent; the concentration of lead iodide in the lead iodide solution may be selected from 0.5 to 1.5 mol / L, such as 0.8 mol / L, 1 mol / L, and 1.2 mol / L; the molar ratio of PMMA to lead iodide may be selected from (0.5% to 10%): 1, such as 1%: 1, 2%: 1, 3%: 1, 5%: 1, and 8%: 1; the solvent may be selected from at least one of DMF (N,N-dimethylformamide), DMSO (dimethyl sulfoxide), NMP (N-methylpyrrolidone), and GBL (γ-butyrolactone).

[0010] In an embodiment of the present invention, the lead iodide solution deposition method can be selected from one or more of spin coating, scraping, and coating, such as spin coating, and the spin coating speed can be selected from 4500 to 5500 rpm, such as 4800 rpm, 5000 rpm, and 5200 rpm; the spin coating time can be selected from 20 to 40s, such as 25s, 30s, and 35s; the deposition thickness can be selected from 200 to 500nm, such as 300nm and 400nm.

[0011] In an embodiment of the present invention, the substrate may include:

[0012] Base material;

[0013] A SnO2 layer is provided on the surface of the substrate.

[0014] In an embodiment of the present invention, the substrate can be selected from transparent conductive glass, such as FTO or ITO; the substrate can be treated before preparing the SnO2 layer; the treatment can include washing, drying and UV-ozone treatment; washing can be carried out using acetone, isopropanol and water in sequence, and the water can be selected from deionized water; drying can be selected from blow drying; the time of UV-ozone treatment can be selected from 10 to 30 minutes, such as 15 minutes, 20 minutes, and 25 minutes.

[0015] In an embodiment of the present invention, the thickness of the SnO2 layer may be selected from 15 to 25 nm, such as 18 nm, 20 nm, and 22 nm; and the method for preparing the SnO2 layer may include:

[0016] The SnO2 solution is spin coated and then annealed to obtain a SnO2 layer.

[0017] In an embodiment of the present invention, the SnO2 solution includes a SnO2 product and water, the SnO2 product can be selected from commercially available products, such as SnO2 dispersion; water can be selected from deionized water; the volume ratio of the SnO2 product and water can be selected from 1: (3-5), such as 1: 4; the spin coating speed can be selected from 3500-4500 rpm, such as 3800 rpm, 4000 rpm, 4200 rpm; the spin coating time can be selected from 15-25s, such as 18s, 20s, 22s; the annealing temperature can be selected from 160-200°C, such as 170°C, 180°C, 190°C; the annealing time can be selected from 20-40min, such as 25min, 30min, 35min.

[0018] In an embodiment of the present invention, the temperature of the primary annealing can be selected from 50 to 100° C., such as 60° C., 70° C., 80° C., and 90° C.; the time of the primary annealing can be selected from 30 to 300 seconds, such as 60 seconds, 120 seconds, 180 seconds, and 240 seconds.

[0019] In an embodiment of the present invention, the thickness of the lead iodide film may be selected from 300 to 400 nm, such as 320 nm, 340 nm, 360 nm, and 380 nm.

[0020] In an embodiment of the present invention, the anti-solvent may be selected from at least one of chloroform, chlorobenzene, toluene and dichloroethane.

[0021] In an embodiment of the present invention, the soaking time may be selected from 30 to 300 seconds, such as 60 seconds, 120 seconds, 180 seconds, and 240 seconds.

[0022] In an embodiment of the present invention, the temperature of the secondary annealing can be selected from 50 to 100° C., such as 60° C., 70° C., and 80° C.; the time of the secondary annealing can be selected from 1 to 5 minutes, such as 2 minutes, 3 minutes, and 4 minutes.

[0023] In an embodiment of the present invention, the organic amine salt solution may include: a solute and a solvent; the solute may be selected from at least one of formamidine hydroiodide, formamidine hydrobromide, methylamine hydroiodide, and methylamine hydrobromide; the solvent may be selected from isopropanol; the concentration of the solute in the organic amine salt solution may be selected from 60 to 100 mg / mL, such as 70 mg / mL, 80 mg / mL, and 90 mg / mL. In an embodiment of the present invention, the organic amine salt solution may also include: an additive; the additive may be selected from methyl ammonium chloride; the concentration of the additive in the organic amine salt solution may be selected from 5 to 15 mg / mL, such as 8 mg / mL, 9 mg / mL, and 12 mg / mL.

[0024] In an embodiment of the present invention, the reaction method may include:

[0025] The organic amine salt solution was deposited on the porous lead iodide film and then annealed three times to obtain the perovskite film.

[0026] In an embodiment of the present invention, the method of depositing the organic amine salt solution can be selected from one or more of spin coating, scraping, and coating; for example, it can be selected from spin coating, and the spin coating speed can be selected from 2000 to 3000 rpm, such as 2500 rpm; the spin coating time can be selected from 20 to 40s, such as 25s, 30s, and 35s.

[0027] In an embodiment of the present invention, the volume ratio of the lead iodide solution to the organic amine salt solution can be selected from (0.5-1.5):1, such as (0.8-1.2):1, 1:1.

[0028] In an embodiment of the present invention, the temperature of the three annealing processes can be selected from 100 to 150° C., such as 110° C., 120° C., 130° C., and 140° C.; the time of the three annealing processes can be selected from 5 to 15 minutes, such as 8 minutes, 10 minutes, and 12 minutes.

[0029] In an embodiment of the present invention, the thickness of the perovskite film may be selected from 350 to 450 nm, such as 380 nm, 400 nm, and 420 nm.

[0030] The present invention provides a perovskite solar cell, comprising: a perovskite film;

[0031] The perovskite film is a perovskite film prepared by the method described in the above technical solution.

[0032] In an embodiment of the present invention, the perovskite solar cell further comprises:

[0033] A hole transport layer disposed on the surface of the perovskite film;

[0034] An electrode is disposed on the coating surface.

[0035] In an embodiment of the present invention, the thickness of the hole transport layer may be selected from 150 to 250 nm, such as 180 nm, 200 nm, and 220 nm; and the preparation method of the hole transport layer may include:

[0036] The hole transport layer solution is spin-coated on the surface of the perovskite film to prepare the hole transport layer.

[0037] In an embodiment of the present invention, the hole transport layer solution includes: a first solution and a second solution; the solute of the first solution includes: Spiro-OMeTAD and 4-tert-butylpyridine; the dosage ratio of Spiro-OMeTAD and 4-tert-butylpyridine can be selected from (65-75) mg: (35-45) μL, such as (68-73) mg: (38-42) μL, 72 mg: 39 μL; the solvent in the first solution may include chlorobenzene; the dosage ratio of Spiro-OMeTAD and chlorobenzene can be selected from (65-75) mg: 1 mL, such as 68 mg: 1 mL, 70 mg: 1 mL, 72 mg: 1 mL; the second solution is selected from bis(trifluoromethane) The concentration of the acetonitrile solution of lithium sulfonyl imide and the acetonitrile solution of lithium bis(trifluoromethanesulfonyl imide) can be selected from 500-550 mg / mL, such as 510 mg / mL, 520 mg / mL, 530 mg / mL, 540 mg / mL; the dosage ratio of Spiro-OMeTAD and the second solution can be selected from (65-75) mg: (20-25) μL, such as (68-73) mg: (22-24) μL, 73 mg: 23 μL; the spin coating speed can be selected from 2500-3500 rpm, such as 2800 rpm, 300 rpm, 3200 rpm; the spin coating time can be selected from 25-35 s, such as 28 s, 30 s, 32 s.

[0038] In an embodiment of the present invention, the electrode can be selected from a silver electrode, and the thickness of the electrode can be selected from 60 to 80 nm, such as 65 nm, 70 nm, and 75 nm; the electrode can be prepared on the surface of the hole transport layer by vacuum evaporation; the vacuum degree of vacuum evaporation can be less than 10 -4 Pa, the deposition rate can be selected from like

[0039] In order to solve the problem of incomplete reaction between the bottom lead iodide and the organic amine salt, the present invention introduces an organic sacrificial material into the lead iodide layer to prepare porous lead iodide, which provides a channel for the diffusion and reaction of the organic amine salt and promotes the complete conversion of the lead iodide into perovskite. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a SEM image of the perovskite film prepared in Example 1 of the present invention;

[0041] Figure 2 The current-voltage curve of the solar cell prepared in Example 1 of the present invention;

[0042] Figure 3 This is a SEM image of the perovskite film prepared in Example 2 of the present invention;

[0043] Figure 4The current-voltage curve of the solar cell prepared in Example 2 of the present invention;

[0044] Figure 5 This is a SEM image of the perovskite film prepared in Example 3 of the present invention;

[0045] Figure 6 This is the current-voltage curve of the solar cell prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0046] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] The FTO glass substrate was cleaned with acetone, isopropanol and deionized water in turn, dried and treated with UV-ozone for 20 minutes; the SnO2 dispersion was mixed with deionized water in a volume ratio of 1:4, spin-coated on the FTO substrate at 4000 rpm for 20 seconds, and annealed at 180°C for 30 minutes to obtain a SnO2 / FTO substrate.

[0049] 1.5 mmol PbI2 and 0.15 mmol PMMA were dissolved in 1 mL DMF to obtain solution A; 90 mg FAI (formamidine hydroiodide) and 9 mg MACl (methylammonium chloride) were dissolved in 1 mL IPA (isopropanol) to obtain solution B.

[0050] Take 50 μl of solution A and spin-coat it on the SnO2 / FTO substrate at 5000 rpm for 30 seconds, and heat it at 70°C for 1 minute to obtain a lead iodide film with a thickness of 360 nm (it is recommended to state the specific thickness); soak the above lead iodide film in chlorobenzene for 60 seconds, take it out, and anneal it at 70°C for 1 minute; take 50 μl of solution B and spin-coat it on the lead iodide film at 2500 rpm for 30 seconds, and anneal it at 150°C for 10 minutes to obtain a perovskite film.

[0051] 72 mg of Spiro-OMeTAD and 39 microliters of 4-tert-butylpyridine were dissolved in 1 mL of chlorobenzene, and 23 microliters of 520 mg / mL bis(trifluoromethanesulfonyl)imide lithium acetonitrile solution were added, mixed evenly, and spin-coated at 3000 rpm for 30 seconds on the perovskite layer. Finally, a 70 nm thick silver electrode was prepared on the surface of the hole transport layer by vacuum evaporation, with a vacuum degree of less than 10-4 Pa and a deposition rate of 1.5 %. Get solar cells.

[0052] In the perovskite solar cell prepared in Example 1, the thickness of the SnO2 layer is 20 nm, the thickness of the perovskite film is 400 nm, the thickness of the hole transport layer is 200 nm, and the thickness of the silver electrode is 70 nm.

[0053] Example 2

[0054] A perovskite film was prepared according to the method of Example 1, except that the amount of PMMA in solution A was 0.015 mmol.

[0055] Example 3

[0056] A perovskite film was prepared according to the method of Example 1, except that PMMA was not added to solution A.

[0057] Performance Testing

[0058] The morphology of the perovskite films prepared in Examples 1 to 3 was characterized by scanning electron microscopy. Figure 1 , Figure 3 and Figure 5 As shown, it can be seen that the surface of the perovskite film prepared in Example 1 is smooth and no lead iodide remains; a small amount of lead iodide remains on the surface of the perovskite film prepared in Example 2; and a large amount of lead iodide remains on the surface of the perovskite film prepared in Example 3.

[0059] At room temperature, using a 3A solar simulator, at 100mW / cm 2 The photoelectric conversion efficiency of the perovskite solar cell prepared in the embodiment was tested under a light intensity of , and the effective area of ​​the perovskite solar cell was 0.09 cm 2 ; Test results such as Figure 2 , Figure 4 and Figure 6 as shown; Figure 2 As shown in Figure 1, the short-circuit current density of the perovskite solar cell prepared in Example 1 is 25.73 mA / cm 2 , the open circuit voltage is 1.137V, the fill factor is 80.33%, and the photoelectric conversion efficiency is 23.50%; Figure 4 As shown in Figure 2, the short-circuit current density of the perovskite solar cell prepared in Example 2 is 25.68 mA / cm 2 , the open circuit voltage is 1.128V, the fill factor is 80.27%, and the photoelectric conversion efficiency is 23.23%; Figure 6 As shown in Figure 2, the short-circuit current density of the perovskite solar cell prepared in Example 3 is 25.60 mA / cm 2 , the open circuit voltage is 1.067V, the fill factor is 77.93%, and the photoelectric conversion efficiency is 21.29%.

[0060] In order to solve the problem of incomplete reaction between the bottom lead iodide and the organic amine salt, the present invention introduces an organic sacrificial material into the lead iodide layer to prepare porous lead iodide, which provides a channel for the diffusion and reaction of the organic amine salt and promotes the complete conversion of the lead iodide into perovskite.

[0061] Although the present invention has been described and illustrated with reference to specific embodiments of the present invention, these descriptions and illustrations do not limit the present invention. It will be clearly understood by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention as defined by the appended claims, so that specific circumstances, materials, material compositions, materials, methods or processes are suitable for the goals, spirit and scope of the present application. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it should be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless specifically indicated herein, the order and grouping of operations are not limitations of the present application.

Claims

1. A method for preparing a perovskite film, comprising: After the lead iodide solution is deposited on the substrate, annealing is performed once to obtain a lead iodide film; The lead iodide film is immersed in an anti-solvent and then subjected to secondary annealing to obtain a porous lead iodide film; reacting the porous lead iodide film with an organic amine salt solution to obtain a perovskite film; The lead iodide solution contains polymethyl methacrylate.

2. The preparation method according to claim 1, characterized in that: The lead iodide solution comprises: lead iodide, polymethyl methacrylate and a solvent; The concentration of lead iodide in the lead iodide solution is selected from 0.5 to 1.5 mol / L.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the polymethyl methacrylate to lead iodide is selected from (0.5% to 10%):

1.

4. The preparation method according to claim 2, characterized in that: The solvent is selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone and γ-butyrolactone.

5. The preparation method according to claim 1, characterized in that: The temperature of the primary annealing is selected from 50 to 100° C., and the time of the primary annealing is selected from 30 to 300 seconds.

6. The preparation method according to claim 1, characterized in that: The anti-solvent is selected from at least one of chloroform, chlorobenzene, toluene and dichloroethane.

7. The preparation method according to claim 1, characterized in that: The soaking time is selected from 30 to 300 seconds.

8. The preparation method according to claim 1, characterized in that: The temperature of the secondary annealing is selected from 50 to 100° C.; the time of the secondary annealing is selected from 1 to 5 minutes.

9. The preparation method according to claim 1, characterized in that: The organic amine salt solution comprises: a solute and a solvent; The solute is selected from at least one of formamidine hydroiodide, formamidine hydrobromide, methylamine hydroiodide, and methylamine hydrobromide; The solvent is selected from isopropanol; The concentration of the solute in the organic amine salt solution is selected from 60 to 90 mg / mL.

10. A perovskite solar cell, comprising: The perovskite film prepared by the method according to claim 1.

Citation Information

Patent Citations

  • Perovskite solar cell capable of regulating and controlling growth of lead iodide passivation layer and preparation method

    CN111640872A

  • Perovskite thin film and preparation method of solar cell thereof

    CN115207220A

  • Method for reconstructing lead iodide structure by polar solvent and application

    CN115548221A

  • Method for preparing high-performance perovskite thin film from ordered porous lead iodide and application of high-performance perovskite thin film

    CN115605063A