Organic room-temperature phosphorescent material based on benzil derivative as well as preparation method and application of organic room-temperature phosphorescent material
By self-assemblying supramolecular self-assembly of room temperature phosphorescence dendrimers based on benzyl derivatives, the problems of short phosphorescence lifetime and low quantum yield of organic room temperature phosphorescence materials in the aqueous phase are solved, and high-efficiency phosphorescence performance in the aqueous phase is achieved. Improved, suitable for fields such as bioimaging and photocatalysis.
Patent Information
- Application Number
- CN202411122948.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-06
AI Technical Summary
There are challenges in achieving organic room temperature phosphorescence emission in aqueous solutions, especially due to the short phosphorescence lifetime and low quantum yield due to the non-radiative transition caused by dissolved oxygen and molecular movement in water.
Supramolecular self-assembly using room temperature phosphorescence dendrimer compound based on benzyl derivatives to form a stable nanoassembly. The compound is prepared by nucleophilic substitution reaction under the action of alkali, and the supramolecular is formed by solvent precipitation. Nanoassembly to improve phosphorescence properties.
The phosphorescence life is extended and the quantum yield is improved in the aqueous phase. The phosphorescence life is 0.63ms, the quantum yield is as high as 51.9%. The preparation process is simple, suitable for mass production, and has a low cost and green and environmentally friendly light capture system. .
Smart Images

Figure CN119080598A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to an organic room temperature phosphorescent material based on a benzil derivative, and a preparation method and application thereof. Background Art
[0002] Organic room temperature phosphorescent materials (RTP) have unique properties such as low toxicity, long emission lifetime and large Stokes shift. They have broad application prospects in the fields of optical functional materials, intelligent anti-counterfeiting, bio-imaging, chemical sensing, information encryption, etc., and have become one of the frontier topics in chemistry and materials science in recent years. However, achieving efficient phosphorescent emission of organic compounds at room temperature is a challenging task. The essential reason is that the spin-orbit coupling of pure organic systems is weak, and the non-radiative transition and quenching of triplet excitons cannot be avoided at room temperature. There are two main ways to achieve room temperature phosphorescence of pure organic materials: 1) Enhance the spin-orbit coupling to increase the minimum excited singlet state (S1) and triplet state (T n ) intersystem crossing between electrons; 2) suppressing the non-radiative transition process of triplet excitons. Currently, researchers have developed a variety of methods to obtain pure organic room temperature phosphorescence, including the introduction of aromatic carbonyl compounds, heteroatoms and heavy atoms to increase spin-orbit coupling, and the suppression of non-radiative transitions of triplet electrons by methods such as crystal construction, host-guest doping, incorporation into rigid polymer matrices, host-guest interactions, and supramolecular self-assembly. In recent years, great progress has been made in organic room temperature phosphorescent materials, but organic room temperature phosphorescent materials with ultra-long luminescence lifetime and high phosphorescence quantum yield are still very challenging.
[0003] Supramolecular self-assembly has become an effective strategy for preparing efficient room temperature phosphorescent materials due to its advantages such as low cost, simple preparation process, and ability to effectively restrict molecular motion and inhibit non-radiative transition processes, and has attracted widespread attention from scientific researchers. Supramolecular self-assembly can construct different types of phosphorescent molecules into assemblies with precise structures and functions, which not only simplifies complex molecular design and time-consuming synthesis. Moreover, supramolecular self-assembly is mainly based on non-covalent bond forces, and can regulate the state of molecular stacking and energy transfer through processes such as assembly-disassembly, giving the assembled phosphorescent materials characteristics such as dynamic adjustability and stimulus responsiveness of luminescence properties, which can achieve the effect of precise luminescence regulation.
[0004] At present, researchers have achieved efficient room temperature phosphorescence emission of pure organic compounds in the solid state through strategies such as co-crystallization, incorporation into rigid polymer matrices, and host-guest doping. However, in the solution state, especially in the aqueous solution state, it is still a huge challenge to achieve organic room temperature phosphorescence emission, because the dissolved oxygen in water and the non-radiative transitions caused by molecular motion will significantly quench triplet excitons. Therefore, it is of great significance and challenge to use supramolecular self-assembly strategies to construct aqueous organic room temperature phosphorescent materials with long phosphorescence lifetime and high quantum yield. Summary of the invention
[0005] In view of the above technical problems, the present invention provides an organic room temperature phosphorescent material based on benzil derivatives and a preparation method and application thereof. The organic room temperature phosphorescent material in the present invention uses a room temperature phosphorescent dendrimer compound based on benzil derivatives as an assembly unit, which can self-assemble into a stable nano-assembly in an aqueous solution as an organic room temperature phosphorescent material. The organic room temperature phosphorescent material provided by the present invention overcomes the technical problems of short phosphorescence lifetime and low phosphorescence quantum yield of room temperature phosphorescent materials in aqueous phase.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In one aspect, the present invention provides a room temperature phosphorescent dendrimer compound based on a benzil derivative, having a structure shown in formula (1):
[0008]
[0009] In formula (1), Z1 and Z2 are each isolated and selected from any one of the structures represented by formula (2), formula (3) and formula (4):
[0010]
[0011]
[0012] In formula (2), formula (3) and formula (4), R1 to R 12 Each is independently selected from any one of -COOMe, -F, -Cl, -Br, -CF3, -CH3 and -OCH3.
[0013] On the other hand, the present invention provides a method for preparing the above-mentioned room temperature phosphorescent dendrimer compound based on benzil derivatives, comprising the following steps: reacting 4,4'-dihydroxybenzil, Z1CH2Br and / or Z2CH2Br in a solvent at 80-100°C under the action of a base to obtain the room temperature phosphorescent dendrimer compound based on benzil derivatives.
[0014] In the technical solution of the present invention, the structural formula of the 4,4'-dihydroxybenzil is:
[0015]
[0016] In the technical solution of the present invention, 4,4'-dihydroxybenzil can undergo a nucleophilic substitution reaction with Z1CH2Br / Z2CH2Br to prepare the room temperature phosphorescent dendrimer compound based on the benzil derivative.
[0017] As a preferred embodiment, the base is potassium carbonate and / or cesium carbonate;
[0018] Preferably, the ratio of the amount of the 4,4'-dihydroxybenzil, the total amount of Z1CH2Br and Z2CH2Br to the amount of potassium carbonate is 1:(2-2.2):(2.5-3), more preferably 1:2.2:3;
[0019] Preferably, the solvent is N,N-dimethylformamide (DMF) and / or acetonitrile;
[0020] Preferably, the reaction time is 12 to 24 hours;
[0021] Preferably, the reaction is carried out in an inert gas atmosphere;
[0022] In certain specific embodiments, the preparation method further comprises post-treatments of cooling and purification.
[0023] In another aspect, the present invention provides an organic room temperature phosphorescent material, which is a supramolecular nanoassembly formed by self-assembly of the room temperature phosphorescent dendrimer compound based on benzil derivatives.
[0024] As a preferred embodiment, the organic room temperature phosphorescent material is a supramolecular nanoassembly formed by self-assembly of the above-mentioned room temperature phosphorescent dendrimer compound based on benzil derivatives through a solvent precipitation method.
[0025] As a preferred embodiment, the solvent precipitation method comprises the following steps: adding a solution containing the room temperature phosphorescent dendrimer compound based on the benzil derivative into a poor solvent, and obtaining the supramolecular nanoassembly by ultrasonic oscillation;
[0026] Preferably, the solvent in the solution containing the dendrimer phosphorescent molecule based on benzil derivatives is at least one selected from tetrahydrofuran, acetonitrile, 1,4-dioxane, dimethyl sulfoxide and N,N-dimethylformamide;
[0027] Preferably, the poor solvent is water;
[0028] Preferably, the ultrasonic oscillation time is 1 to 5 minutes;
[0029] In some specific embodiments, the supramolecular nanoassembly obtained by the above preparation method shows excellent aggregation-induced phosphorescence phenomenon, with a phosphorescence lifetime of up to 0.63 ms and a phosphorescence quantum yield of up to 51.9%.
[0030] On the other hand, the present invention provides a light harvesting system, wherein the light harvesting system uses the above-mentioned room temperature phosphorescent dendrimer compound based on benzil derivatives as a light collection antenna and energy donor, and uses a fluorescent dye as an energy acceptor, and the room temperature phosphorescent dendrimer compound based on benzil derivatives and the fluorescent dye are co-assembled in an aqueous solution to form a light harvesting system.
[0031] As a preferred embodiment, the fluorescent dye is Nile Red (NiR) and / or Eosin Y (ESY);
[0032] Preferably, the concentration ratio of the room temperature phosphorescent dendrimer compound based on benzil derivatives to the fluorescent dye in the aqueous solution is 50-2000:1.
[0033] In another aspect, the present invention provides a method for preparing the above light harvesting system, comprising the following steps:
[0034] The room temperature phosphorescent molecular compound based on benzyl derivatives and fluorescent dye are dissolved in solvent I, then added into a poor solvent, and the light harvesting system is obtained by ultrasonic oscillation.
[0035] As a preferred embodiment, the solvent I is a hydrophilic organic solvent, selected from at least one of tetrahydrofuran, 1,4-dioxane, dimethyl sulfoxide, N,N-dimethylformamide (DMF) and acetonitrile;
[0036] Preferably, the poor solvent is water;
[0037] Preferably, the ultrasonic oscillation time is 1 to 5 minutes.
[0038] In another aspect, the present invention provides applications of the light-harvesting system in the fields of biological imaging, photocatalysis, and luminescent materials.
[0039] The above technical solution has the following advantages or beneficial effects:
[0040] The invention provides an organic room temperature phosphorescent material based on benzil derivatives. The organic room temperature phosphorescent material uses a room temperature phosphorescent dendrimer compound based on benzil derivatives as an assembly unit, can self-assemble into a stable nano assembly in an aqueous solution, has a long phosphorescence lifetime and a high phosphorescence quantum yield.
[0041] Compared with the prior art, the present invention has the following advantages:
[0042] (1) The preparation process of the room temperature phosphorescent dendrimer compound based on benzyl derivatives in the present invention is simple, the reaction conditions are mild, the reaction yield is high, the post-treatment is convenient, and it is suitable for mass production;
[0043] (2) The room temperature phosphorescent dendrimer compound based on benzyl derivatives in the present invention can form a stable supramolecular nanoassembly in a variety of organic solvents or aqueous solutions, and can be assembled into a supramolecular nanoassembly with good water dispersibility in aqueous phase. The nanoassembly has excellent aggregation-induced room temperature phosphorescence performance, a phosphorescence lifetime of up to 0.63 ms, and a phosphorescence quantum yield of up to 51.9%;
[0044] (3) The light-harvesting system prepared by the room temperature phosphorescent dendrimer compound based on benzil derivatives can be constructed in an aqueous phase, and has the advantages of low cost, green environmental protection, and suitability for application in biological systems;
[0045] (4) The light-harvesting system provided by the present invention can still transfer energy well at a higher donor / acceptor ratio. A unit acceptor can receive energy transferred by hundreds or even thousands of times the amount of the donor, while having high-efficiency energy transfer capabilities, with the best energy transfer efficiency reaching 82%. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The phosphorescence spectrum (a) and phosphorescence intensity variation trend diagram (b) of the compound BZL-G0 in Example 4 of the present invention in solvents with different water contents.
[0047] Figure 2 The phosphorescence spectrum (a) and phosphorescence intensity variation trend diagram (b) of the compound BZL-G1 in Example 4 of the present invention in solvents with different water contents.
[0048] Figure 3 It is a phosphorescence spectrum diagram (a) and a phosphorescence intensity variation trend diagram (b) of the compound BZL-AB3-G1 in Example 4 of the present invention in solvents with different water contents.
[0049] Figure 4 It is a fluorescence spectrum diagram of the light harvesting system with different donor / acceptor concentration ratios prepared by compound BZL-AB3-G1 in Example 6 of the present invention.
[0050] Figure 5 It is a fluorescence spectrum diagram of the light harvesting system with different donor / acceptor concentration ratios prepared by the compound BZL-AB3-G1 in Example 7 of the present invention. DETAILED DESCRIPTION
[0051] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0052] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0053] Example 1 Room temperature phosphorescent dendrimer compound BZL-G0 based on benzyl derivatives
[0054] This embodiment provides a room temperature phosphorescent dendrimer compound BZL-G0 based on a benzil derivative, and its preparation process is as follows:
[0055]
[0056] The specific steps are:
[0057] In a 250 mL double-necked flask equipped with a stirring magnet, 4,4'-dihydroxybenzil (1.0 g, 4.1 mmol), 3,5-dichlorobenzyl bromide (2.18 g, 9.1 mmol), K2CO3 (1.71 g, 12.4 mmol) and ultra-dry DMF (30 mL) were added in sequence; the mixture was reacted in a metal bath at 80°C under nitrogen protection for 12 h, during which the reaction progress was monitored by TLC;
[0058] After the reaction was completed, 200 mL of water was added to the reaction system to precipitate the product, which was filtered and washed with a large amount of water. The crude solid product was dried and then purified by silica gel flash column chromatography to obtain a white solid BZL-G0 with a yield of 90%.
[0059] The H NMR spectrum of BZL-G0 prepared in this example 1 H NMR (400MHz, CDCl3, δ): 5.27 (s, ArCH2O, 4H), 7.21-7.24 (m, ArH, 4H), 7.54 (d, J = 1.9Hz, ArH, 4H), 7.61 (t, J = 1.9Hz, ArH, 2H), 7.87-7.90 (m, ArH, 4H). 13 C NMR (100MHz, CDCl3, δ): 193.9, 163.8, 141.0, 134.7, 132.6, 128.2, 126.8, 126.3, 116.1, 68.6.
[0060] High resolution mass spectrum (HRMS-ESI) of BZL-G0 prepared in this example: 28 H 19 O4Cl4 + ([M+H] + ); calculated molecular ion peak value: m / z 559.00320, measured value: m / z 559.00305.
[0061] Example 2 Room temperature phosphorescent dendrimer compound BZL-G1 based on benzil derivatives
[0062] This embodiment provides a room temperature phosphorescent dendrimer compound BZL-G1 based on a benzil derivative, and the preparation process thereof is as follows:
[0063]
[0064] The specific steps are:
[0065] In a 250 mL double-necked flask equipped with a stirring magnet, 4,4'-dihydroxybenzil (0.80 g, 3.3 mmol), AB2-G1CH2Br (3.79 g, 7.3 mmol), K2CO3 (1.37 g, 9.9 mmol) and ultra-dry DMF (30 mL) were added in sequence; the mixture was reacted in a metal bath at 80°C under nitrogen protection for 24 h, during which the reaction progress was monitored by TLC;
[0066] After the reaction was completed, 200 mL of water was added to the reaction system to precipitate the product, which was then filtered and washed with a large amount of water. The solid crude product was dried and then purified by silica gel flash column chromatography to obtain a white solid BZL-G1 with a yield of 92%.
[0067] The H NMR spectrum of BZL-G1 prepared in this example 1 H NMR (400MHz, CDCl3, δ): 4.99 (s, ArCH2O, 8H), 5.09 (s, ArCH2O, 4H), 6.51 (t, J = 2.3Hz, ArH, 2H), 6. 63(d,J=2.2Hz,ArH,4H),6.98-7.02(m,ArH,4H),7.29-7.31(m,ArH,12H),7.92-7.95(m,ArH,4H). 13 C NMR (100MHz, CDCl3, δ): 193.3, 163.7, 159.7, 140.0, 138.8, 135.3, 132.4, 128.2, 126.6, 125.5, 115.1, 106.5, 101.8, 69.9, 68.6.
[0068] High resolution mass spectrum (HRMS-ESI) of BZL-G1 prepared in this example: 56 H 39 O8Cl8 + ([M+H] + ); calculated molecular ion peak value: m / z 1119.01477, measured value: m / z 1119.01440.
[0069] Example 3 Room temperature phosphorescent dendrimer compound BZL-AB3-G1 based on benzil derivatives
[0070] This embodiment provides a room temperature phosphorescent dendrimer compound BZL-AB3-G1 based on a benzil derivative, and the preparation process thereof is as follows:
[0071]
[0072] The specific steps are:
[0073] In a 250 mL double-necked flask equipped with a stirring magnet, 4,4'-dihydroxybenzil (0.60 g, 2.5 mmol), AB3-G1CH2Br (3.79 g, 5.5 mmol), K2CO3 (1.03 g, 7.4 mmol) and ultra-dry DMF (30 mL) were added in sequence; the mixture was reacted in a metal bath at 80°C under nitrogen protection for 24 h, during which the reaction progress was monitored by TLC;
[0074] After the reaction was completed, 200 mL of water was added to the reaction system to precipitate the product, which was then filtered and washed with a large amount of water. The solid crude product was dried and then purified by silica gel flash column chromatography to obtain a white solid BZL-AB3-G1 with a yield of 95%.
[0075] The H NMR spectrum of BZL-AB3-G1 prepared in this example 1 H NMR (400MHz, CDCl3, δ): 4.98 (s, ArCH2O, 4H), 5.04 (s, ArCH2O, 12H), 6.66 (s, ArH, 4H), 6.96 -7.00(m,ArH,4H),7.27-7.29(m,ArH,10H),7.30-7.31(m,ArH,8H),7.93-7.97(m,ArH,4H). 13 CNMR (100MHz, CDCl3, δ):193.1,163.6,152.5,140.7,139.9,137.7,135.3,134.9, 132.4,132.3,128.3,128.1,126.6,126.2,125.4,115.1,107.1,73.8,69.9,69.9.
[0076] High resolution mass spectrum (HRMS-ESI) of BZL-AB3-G1 prepared in this example: 70 H 46 O 10 KCl 12 + ([M+K] + ); calculated molecular ion peak value: m / z 1504.89849, measured value: m / z 1504.90198.
[0077] Example 4
[0078] This example tests the phosphorescence intensity of the room temperature phosphorescent molecular compounds based on benzil derivatives prepared in Examples 1-3 in the dissolved state and the aggregated state. Taking compound BZL-G0 as an example, the test process is as follows:
[0079] Take a 100mL volumetric flask and prepare 10 -3 mol / L tetrahydrofuran solution of compound BZL-G0;
[0080] Take 11 10 mL sample bottles, numbered 0 to 10, and add 0.5 mL of the tetrahydrofuran solution of the above compound BZL-G0 into each sample bottle using a pipette;
[0081] Tetrahydrofuran 9.5mL, 8.5mL, 7.5mL, 6.5mL, 5.5mL, 5.5mL, 3.5mL, 2.5mL, 1.5mL, and 0.5mL were added to the sample bottles numbered 0 to 9, respectively; then deionized water 1.0mL, 2.0mL, 3.0mL, 4.0mL, 5.0mL, 6.0mL, 7.0mL, 8.0mL, 9.0mL, and 9.5mL were added to the sample bottles numbered 1 to 10, respectively, to obtain 5×10 - 5 mol / L solution of compound BZL-G0; the prepared solution was sonicated in an ultrasonic instrument for 60 seconds and then the phosphorescence spectrum was tested.
[0082] Figure 1-3The figures are respectively phosphorescence spectra and phosphorescence enhancement trend diagrams of compounds BZL-G0, BZL-G1 and BZL-AB3-G1 in dissolved state and aggregated state. It can be seen from the figures that the compounds BZL-G0, BZL-G1 and BZL-AB3-G1 synthesized by the present invention have the characteristics of aggregation-induced phosphorescence, among which the luminescence efficiency of BZL-G0 in the aggregated state (tetrahydrofuran-water mixed solution with a water content of 90 vol%) is increased by 16.5 times compared with that in the dissolved state (tetrahydrofuran solution), the luminescence efficiency of BZL-G1 in the aggregated state (tetrahydrofuran-water mixed solution with a water content of 90 vol%) is increased by 60.5 times compared with that in the dissolved state (tetrahydrofuran solution), and the luminescence efficiency of BZL-AB3-G1 in the aggregated state (tetrahydrofuran-water mixed solution with a water content of 90 vol%) is increased by 102 times compared with that in the dissolved state (tetrahydrofuran solution).
[0083] Table 1 shows the test results of the photophysical properties of compounds BZL-G0, BZL-G1 and BZL-AB3-G1 in the dissolved state (tetrahydrofuran solution) and the aggregated state (tetrahydrofuran-water mixed solution with a water content of 90 vol%) (λ ex is the excitation wavelength, λ PL As can be seen from the table, in the dissolved state, the luminescence performance of compounds BZL-G0, BZL-G1 and BZL-AB3-G1 is very poor, among which the phosphorescence lifetime (τ p ) is 0.9~2.55ns, and the phosphorescence quantum yield (Φ PL ) is only 4.36% at most. However, in the aggregated state, the luminescence efficiency of the three compounds has been qualitatively improved, among which the phosphorescence quantum yield of compound BZL-AB3-G1 (Φ PL ) increased from 4.36% in the dissolved state to 51.92%, and the phosphorescence lifetime also increased from 2.55ns to 0.63ms. In addition, the system also showed obvious dendritic molecular effect. As the number of dendritic molecules at both ends increased, the self-assembly effect in the water phase became better, and the best phosphorescence efficiency was also shown.
[0084] Table 1
[0085]
[0086]
[0087] Example 5 Preparation of supramolecular nanoassemblies
[0088] In this example, the above compounds BZL-G0, BZL-G1 and BZL-AB3-G1 were prepared by solvent precipitation method to obtain nanoassemblies. Taking compound BZL-G0 as an example, the preparation process is as follows:
[0089] Step 1: Prepare the compound at a concentration of 1×10 -3 5 mL of mol / L BZL-G0 tetrahydrofuran solution;
[0090] Step 2, take 5 sample bottles with a volume of 10 mL, numbered 1 to 5;
[0091] Step 3, use a pipette to transfer 0.5 mL of the tetrahydrofuran solution of compound BZL-G0 into 5 sample bottles, and place the sample bottles in an oven to completely evaporate the solvent;
[0092] Step 4, add 0.5 mL, 1.0 mL, 1.5 mL, 2.0 mL and 2.5 mL of tetrahydrofuran to bottles 1 to 5 respectively to dissolve the compound;
[0093] Step 5, take another 5 10mL sample bottles (labeled 6 to 10), add 9.5mL, 9.0mL, 8.5mL, 8.0mL and 7.5mL of deionized water respectively; add a small stirring magnet to bottles 6 to 10 respectively and start stirring; use a disposable syringe to slowly drop the tetrahydrofuran solution of compound BZL-G0 in bottles 1 to 5 into the high-speed stirring sample bottles 6 to 10; after the dropwise addition is completed, sample bottles 6 to 10 are ultrasonicated for 5 minutes to obtain uniformly dispersed supramolecular nanoassemblies.
[0094] The concentration of the nanoassembly dispersion prepared in this example is 5×10 -5 mo1 / L.
[0095] Example 6 Light Harvesting System
[0096] In this example, the above compound BZL-AB3-G1 was used as a donor and Nile red (NiR) was used as a receptor to prepare a light harvesting system. The process is as follows:
[0097] Step 1: Prepare the solution at a concentration of 1×10 -3 5 mL of tetrahydrofuran solution of mol / L compound BZL-AB3-G1;
[0098] Step 2, preparing tetrahydrofuran solutions of Nile red of different concentrations;
[0099] Step 3, mixing a trace amount of donor compound BZL-AB3-G1 solution (D) and a trace amount of Nile red receptor solution (A) at different final concentration ratios (D / A=50 / 1, 100 / 1, 500 / 1, 1000 / 1, 1500 / 1, 2000 / 1) (sample bottles are numbered 1 to 6), and then placing sample bottles numbered 1 to 6 in an oven to completely evaporate the solvent;
[0100] Step 4, add 1.0 mL of tetrahydrofuran to bottles 1 to 6 respectively using a pipette to dissolve the mixture;
[0101] Step 5, the mixed solution was added dropwise to 4.0 mL of deionized water; ultrasonic oscillation was performed for 5 min, and shaking was continued during the period to obtain aqueous solutions of nanoassemblies with different donor / acceptor concentration ratios, wherein the concentration of the donor BZL-AB3-G1 compound was 5×10 - 5 mo1 / L.
[0102] Step 6: Use a fluorescence spectrophotometer to measure the fluorescence of the aqueous solution of the nanoassembly prepared in this example, with an excitation wavelength of 365 nm. The test results are shown in Figure 4 The energy transfer efficiency and antenna efficiency were calculated based on the spectrum data, and the results are shown in Table 2. The energy transfer efficiency of the system with D / A = 2000 / 1 can reach 81%, and the antenna efficiency can reach 37. The antenna efficiency of the system with D / A = 100 / 1 is as high as 48.
[0103] Table 2
[0104]
[0105] Example 7 Light Harvesting System
[0106] In this example, the above compound BZL-AB3-G1 was used as a donor and eosin Y (ESY) was used as an acceptor to prepare a light harvesting system. The process is as follows:
[0107] Step 1: prepare a concentration of 1×10 -3 5 mL of tetrahydrofuran solution of mol / L compound BZL-AB3-G1;
[0108] Step 2, preparing tetrahydrofuran solutions of Eosin Y of different concentrations;
[0109] Step 3, mixing a trace amount of donor compound BZL-AB3-G1 solution (D) and a trace amount of eosin Y acceptor solution (A) at different final concentration ratios (D / A=50 / 1, 100 / 1, 500 / 1, 1000 / 1, 1500 / 1, 2000 / 1) (numbered 1 to 6), and then placing the sample bottles numbered 1 to 6 in an oven to completely evaporate the solvent;
[0110] Step 4, add 1.0 mL of tetrahydrofuran to bottles 1 to 6 respectively using a pipette to dissolve the mixture;
[0111] Step 5, the mixed solution was added dropwise to 4.0 mL of deionized water; ultrasonic oscillation was performed for 5 min, and shaking was continued during the period to obtain aqueous solutions of nanoassemblies with different donor / acceptor concentration ratios, wherein the concentration of the donor BZL-AB3-G1 compound was 5×10 - 5 mo1 / L.
[0112] Step 6: Use a fluorescence spectrophotometer to measure the fluorescence of the aqueous solution of the nanoassembly prepared in this example, with an excitation wavelength of 365 nm. The test results are shown in Figure 5 The energy transfer efficiency and antenna efficiency are calculated based on the spectrum data, and the results are shown in Table 3. As can be seen from Table 3, the energy transfer efficiency of the system with D / A = 2000 / 1 can reach 74%, and the antenna efficiency (Antennaeffect) can reach 51. The antenna efficiency of the system with D / A = 50 / 1 is as high as 58.
[0113] Table 3
[0114]
[0115] As can be seen from the above examples, the room temperature phosphorescent dendrimer compound based on benzil derivatives prepared in the present invention is not only simple to synthesize and has a high yield, but also can form a nanoassembly with good water dispersibility and stability in an aqueous solution, and the supramolecular nanoassembly constructed by self-assembly has excellent aggregation-induced phosphorescence performance. In addition, the dendrimer phosphorescent molecule can also be used as an excellent light-harvesting system to construct a multi-color (from green to yellow or red) luminescent system.
[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A room temperature phosphorescent dendrimer compound based on a benzil derivative, characterized in that: It has the structure shown in formula (1): In formula (1), Z1 and Z2 are each isolated and selected from any one of the structures represented by formula (2), formula (3) and formula (4): In formula (2), formula (3) and formula (4), R1 to R 12 Each is independently selected from any one of -COOMe, -F, -Cl, -Br, -CF3, -CH3 and -OCH3.
2. The method for preparing a room temperature phosphorescent dendrimer compound based on a benzil derivative according to claim 1, characterized in that: The method comprises the following steps: reacting 4,4'-dihydroxybenzil, Z1CH2Br and / or Z2CH2Br in a solvent at 80-100°C under the action of a base to obtain the room temperature phosphorescent dendrimer compound based on the benzil derivative.
3. The preparation method according to claim 2, characterized in that: The base is potassium carbonate and / or cesium carbonate; Preferably, the ratio of the amount of the 4,4'-dihydroxybenzil, the total amount of Z1CH2Br and Z2CH2Br to the amount of potassium carbonate is 1:(2-2.2):(2.5-3), more preferably 1:2.2:3; Preferably, the solvent is N,N-dimethylformamide and / or acetonitrile; Preferably, the reaction time is 12 to 24 hours; Preferably, the reaction is carried out in an inert gas atmosphere.
4. An organic room temperature phosphorescent material, characterized in that: The organic room temperature phosphorescent material is a supramolecular nanoassembly formed by self-assembly of the room temperature phosphorescent dendrimer compound based on benzil derivatives as claimed in claim 1.
5. The organic room temperature phosphorescent material according to claim 4, characterized in that: The organic room temperature phosphorescent material is a supramolecular nano-assembly formed by self-assembly of the room temperature phosphorescent dendrimer compound based on the benzil derivative by a solvent precipitation method; Preferably, the solvent precipitation method comprises the following steps: adding a solution containing the room temperature phosphorescent dendrimer compound based on the benzil derivative into a poor solvent, and obtaining the supramolecular nanoassembly by ultrasonic oscillation; Preferably, the solvent in the solution containing the dendrimer phosphorescent molecule based on benzil derivatives is at least one selected from tetrahydrofuran, acetonitrile, 1,4-dioxane, dimethyl sulfoxide and N,N-dimethylformamide; Preferably, the poor solvent is water; Preferably, the ultrasonic oscillation time is 1 to 5 minutes.
6. A light harvesting system, characterized in that: The light harvesting system uses the room temperature phosphorescent dendrimer compound based on benzyl derivatives as claimed in claim 1 as a light harvesting antenna and energy donor, and uses a fluorescent dye as an energy acceptor. The room temperature phosphorescent dendrimer compound based on benzyl derivatives and the fluorescent dye are co-assembled in an aqueous solution to form a light harvesting system.
7. The light capture system according to claim 6, characterized in that The fluorescent dye is Nile red and / or eosin Y; Preferably, the concentration ratio of the room temperature phosphorescent dendrimer compound based on benzil derivatives to the fluorescent dye in the aqueous solution is 50-2000:
1.
8. The method for preparing the light harvesting system according to claim 6, characterized in that: The following steps are involved: The room temperature phosphorescent molecular compound based on benzyl derivatives and fluorescent dye are dissolved in solvent I, and then added into a poor solvent, and the light harvesting system is obtained by ultrasonic oscillation.
9. The preparation method according to claim 8, characterized in that: The solvent I is a hydrophilic organic solvent, selected from at least one of tetrahydrofuran, 1,4-dioxane, dimethyl sulfoxide, N,N-dimethylformamide and acetonitrile; Preferably, the poor solvent is water; Preferably, the ultrasonic oscillation time is 1 to 5 minutes.
10. Application of the light-harvesting system of claim 6 in the fields of biological imaging, photocatalysis, and luminescent materials.