Preparation method and application of two-dimensional MOF coated metal oxide composite material

A two-dimensional MOF-coated metal oxide composite addresses the shuttle effect in lithium-sulfur batteries by forming a stable core-shell structure, enhancing conductivity and adsorption, thus improving battery performance.

CN119092705AActive Publication Date: 2024-12-06TONGJI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411150824.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-12-06
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Lithium-ion batteries suffer from poor cycle stability and low energy density due to the shuttle effect of polysulfides between electrodes, leading to capacity decay and reduced coulombic efficiency, and the volume change of sulfur during charge-discharge processes.

Method used

A two-dimensional MOF-coated metal oxide composite material is prepared through a simple method involving surface charge modification, dispersion, and ultrasonication to form a core-shell structure, combining the high adsorption and catalytic properties of MOF with the conductivity of metal oxides, forming a stable composite for lithium-sulfur batteries.

Benefits of technology

The composite material effectively suppresses the shuttle effect, enhances electrical conductivity, and improves the performance of lithium-sulfur batteries by maintaining active metal sites and polysulfide adsorption, resulting in improved cycle stability and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092705A_ABST
    Figure CN119092705A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a two-dimensional MOF (Metal Organic Framework) coated metal oxide composite material. The preparation method comprises the following steps: modifying the surface charge of metal, dispersing the modified metal oxide, preparing the two-dimensional MOF coated metal oxide, and preparing a core-shell composite material (MO (MOF)) with the two-dimensional layered MOF coated metal oxide. Compared with the prior art, the method is simple and easy to implement and good in repeatability, the obtained MOF-coated MOF material is novel in morphology, and combination of MOF and metal oxide is stable. MOF with rich catalytic sites is compounded with polar metal oxide, so that the conductivity of the material and the adsorption catalytic performance of the material on polysulfide are improved. The product can be compounded with a conductive agent and elemental sulfur to serve as a positive electrode material of a lithium-sulfur battery, and has excellent performance of adsorbing and catalyzing conversion of polysulfide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a preparation method of a lithium-sulfur battery catalyst, and in particular to a synthesis method of a two-dimensional MOF-coated metal oxide and a two-dimensional material-coated nanoparticle core-shell composite material and its application in the field of lithium-sulfur battery catalytic materials. Background Art

[0002] In recent years, with society's growing energy demand, the utilization of new clean energy sources such as solar energy and hydropower has received increasing attention. Developing advanced energy storage technologies is an effective way to fully utilize these energy sources. Among the many energy storage technologies, electrochemical energy storage, particularly high-energy-density rechargeable batteries, has become a hotspot for the development of advanced energy storage technologies due to its advantages of high efficiency, stability, cleanliness, flexible configuration, and low cost. Currently, lithium-ion batteries have achieved widespread commercialization, but their disadvantages lie in their poor cycle stability and low energy density, making them difficult to meet the needs of high-density energy storage systems.

[0003] Among various potential new chemical power systems with high specific energy, lithium-sulfur batteries with elemental sulfur and metallic lithium as positive and negative electrodes have attracted much attention from researchers. The reduction of sulfur is based on a multi-electron transfer mechanism, and the theoretical specific capacity of elemental sulfur is as high as 1675 mAh g -1 The lithium-sulfur battery system composed of lithium metal can reach 2600Wh kg -1 The ultra-high theoretical specific energy of elemental sulfur is abundant, inexpensive, and environmentally friendly. Therefore, research on lithium-sulfur batteries with high energy density and high cycle stability is of great significance to meeting society's energy needs and improving energy utilization.

[0004] The low room temperature conductivity of elemental sulfur and Li2S (discharge product) leads to a decrease in the utilization rate of active materials. n (n = 4 to 8) are easily soluble in lithium-sulfur electrolytes. Chain-like polysulfides shuttle back and forth between the positive and negative electrodes. This process leads to the loss of active materials, ultimately causing problems such as battery capacity decay, reduced coulombic efficiency, and shortened cycle life. Due to the difference in density between elemental sulfur and the final product Li2S (2.03 vs. 1.66 g cm -3 ), resulting in a volume change of about 80% during the charge and discharge process.

[0005] To maximize the lifespan of lithium-sulfur batteries, cathode materials must exhibit strong physical or chemical adsorption for polysulfides, capturing or dispersing them to suppress the "shuttle effect." MOFs are considered promising candidates for cathode support materials in lithium-sulfur batteries due to their controllable pore size, highly ordered structure, ultrahigh porosity, and Lewis acid-base interactions with polysulfides. The presence of pores effectively controls the volume changes of the cathode during cycling. Furthermore, polysulfides are reversibly captured and released within the pores of MOFs, where sulfur atoms interact with coordinatively unsaturated metal sites, enhancing the substrate's polysulfide adsorption capacity and effectively suppressing the "shuttle effect." Furthermore, metal sites on the MOF surface are often also catalytic sites for catalytic reactions. By selecting different organic ligands and metal centers, the catalytic performance of MOF materials can be tuned. However, given the suboptimal electrical conductivity of most pure MOFs, further engineering of MOF composites and MOF derivatives is often necessary to meet the required cathode conductivity. Summary of the Invention

[0006] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a novel method for preparing two-dimensional MOF-coated metal oxide composite materials with simple operation and strong controllability.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] During the conception process, it was believed that sheet-like two-dimensional MOFs have a larger specific surface area than block-like MOFs, can provide more active sites, and have better adsorption and catalytic reaction effects on soluble polysulfides.

[0009] The abundant metal active sites in metal oxides are far more effective at adsorbing lithium polysulfides than non-polar carbon materials. Due to their inherent surface defects and unique band structures, some metal oxides even have good conductivity. Therefore, a strategy can be proposed to combine metal oxides and metal-organic frameworks to construct composite materials and apply them to the positive electrode of lithium-sulfur batteries.

[0010] The first aspect of the present invention provides a method for preparing a two-dimensional MOF-coated metal oxide composite material, comprising the following steps:

[0011] (1) Surface charge modification of metal oxides: Weigh the metal oxide and the surface charge modifier, add the metal oxide to an aqueous solution of the surface charge modifier, and then perform ultrasonic mixing. After mixing, separate the solid from the mixed system, wash it several times with alcohol and water, and discard the liquid portion to obtain the surface charge-modified polar metal oxide;

[0012] (2) Dispersion of surface charge-modified metal oxides in a solution: taking the metal oxide complex prepared in step (1), adding water, alcohol, and N,N-dimethylformamide (DMF), and performing ultrasonic dispersion to obtain a solid-liquid mixture in which polar metals are dispersed;

[0013] (3) adding terephthalic acid and metal salt, adding DMF and stirring to dissolve to obtain a metal salt solution;

[0014] (4) adding the solid-liquid mixture in step (2) to the solution in step (3) and stirring and mixing to obtain a solid-liquid mixture;

[0015] (5) introducing nitrogen into the container of the solid-liquid mixture obtained in step (4) to expel the air in the container;

[0016] (6) adding triethylamine to the mixture in step (5) and stirring and mixing in a sealed state;

[0017] (7) placing the container of step (6) into an ultrasonic instrument for ultrasonication, and controlling the temperature of the mixture in the bottle during ultrasonication;

[0018] (8) centrifuging the solid-liquid mixture obtained in step (7), washing with water and alcohol, and drying the solid in a vacuum oven to obtain a MOF-coated metal oxide;

[0019] Furthermore, the metal oxide in step (1) is a polar transition metal oxide having good electrical conductivity and strong adsorption properties for polysulfides, and the surface charge modifier is one of sodium polyvinylbenzenesulfonate (PSS), polyethyleneimine (PEI), and polyvinylpyrrolidone (PVP);

[0020] Furthermore, the mass concentration of the aqueous solution of the surface modifier is 0.1-1%.

[0021] More preferably, the mass concentration of the aqueous solution of the surface modifier is 0.3%.

[0022] Further preferably, the metal oxide is selected from one of Fe3O4, MnO2, Co2O3, Co2O3, and NiO.

[0023] Furthermore, the volume ratio of water, alcohol and DMF in step (2) is 1:1:4-16.

[0024] In step (3), the volume of N,N-dimethylformamide added is the same as that in step (2);

[0025] Furthermore, in step (3), the ratio of terephthalic acid, metal salt and DMF is: 32.5 mg: 170-200 mg: 8-12 ml.

[0026] Furthermore, the metal salt is one or any two selected from: CoCl2·6H2O, NiCl2·6H2O, SrCl2·6H2O, CuCl2·6H2O, ZnCl2·6H2O, and MnCl2·6H2O.

[0027] Furthermore, the volume ratio of the triethylamine added in step (6) to the DMF added in the entire preparation step is 1:60-120.

[0028] Further preferably, the volume ratio of the triethylamine added in step (6) to the DMF added in the entire preparation step is 1:80-100.

[0029] The ultrasonic time in step (7) is 6 to 12 hours. During the ultrasonication, the container of the reactants is sealed and filled with nitrogen. During the ultrasonication, the temperature of the ultrasonic liquid in the ultrasonic machine is kept below 25°C.

[0030] The drying temperature in step (8) is 50-80° C., and the drying time is 12-18 hours.

[0031] The second aspect of the present invention provides a two-dimensional MOF-coated metal oxide obtained by the above preparation method, characterized in that the MOF-coated metal oxide has a shell-core structure of a two-dimensional layered MOF-coated granular metal oxide.

[0032] Furthermore, a composite material of a core-shell structured two-dimensional MOF coated with a metal oxide is prepared, and the thickness of the two-dimensional MOF is 10 to 30 nm.

[0033] A third aspect of the present invention provides a use of the above-mentioned two-dimensional MOF-coated metal oxide in the preparation of positive electrode materials for lithium-sulfur batteries.

[0034] Compared with the existing technology, the present invention has the following technical advantages:

[0035] 1) The composite method utilizes the different electrical properties of the materials to electrostatically assemble a core-shell composite structure of a two-dimensional MOF and nanometal oxide. This simple preparation process eliminates the need for high-temperature sintering, resulting in low energy consumption. The resulting product exhibits consistent composition and excellent stability. Compared to single MOF and metal oxide materials, the resulting composite material exhibits superior performance improvements for lithium-sulfur batteries.

[0036] 2) The amount of surface charge modifier, DMF, triethylamine used in the preparation process of the present invention, whether nitrogen is introduced into the reaction vessel to isolate the air, the time and temperature of ultrasonication, the drying temperature and other parameters will affect the structure and properties of the synthesized material. The type of surface charge modifier directly determines whether MOF can be composited with metal oxides. The greater the difference in electronegativity between the MOF and metal oxide surfaces, the stronger the attraction for mutual binding. The amount of DMF used will determine whether the metal salt can be completely dissolved and the number of metal sites in the MOF material. The use of terephthalic acid can stabilize the metal ions in the solution, forming metal coordination structures with the metal ions as the center and terephthalic acid as the ligand; triethylamine plays a role in connecting the metal coordination structures dispersed in the solution to form a metal organic framework. Its amount used will directly determine whether a two-dimensional MOF can be formed in the later stage. Excessive use of triethylamine will result in too many metal-terephthalic acid linkages, making it difficult to separate the two-dimensional layered MOF by ultrasonication in the later stage. The ultrasonic time will determine the exfoliation effect of the layered MOF, the temperature during ultrasonication will affect the morphology of the MOF, and too high a temperature during ultrasonication will cause the two-dimensional MOF to curl up; sealing the container and filling it with nitrogen during the reaction and ultrasonication process can reduce the oxidation of divalent metal ions by oxygen during the MOF formation process, so that the metal active sites in the MOF maintain an unsaturated coordination structure.

[0037] 3) The composite metal oxide and two-dimensional MOF material prepared by this invention exhibits a stable bond, maintaining a large number of active metal sites within the MOF structure. The resulting composite two-dimensional MOF is coated onto the nanometal oxide to form one or more layers of a coating structure. This material combines the high catalytic activity of the two-dimensional MOF with the strong conductivity and adsorption capacity of the polar metal oxide, resulting in a significantly improved performance for lithium-sulfur batteries compared to single MOF materials and metal oxides. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a transmission electron microscope (TEM) photograph of the Fe3O4@MOF composite material prepared in Example 1;

[0039] Figure 2 This is a scanning electron microscope (SEM) photograph of the Fe3O4@MOF composite material prepared in Example 2;

[0040] Figure 3 These are the rate performance diagrams of lithium-sulfur batteries prepared from the Fe3O4@MOF composite sulfur material, MOF composite sulfur material, and Fe3O4 composite sulfur material prepared in Example 6. DETAILED DESCRIPTION

[0041] The invention relates to a method for preparing a two-dimensional metal organic framework compound (MOF) coated metal oxide (MO) composite material and its application, including surface charge modification of the metal, dispersion of the modified metal oxide, preparation of two-dimensional MOF coated metal oxide, and preparation of a core-shell composite material (MO@MOF) having two-dimensional layered MOF coated metal oxide. The present invention is simple and easy to implement, with good reproducibility. The obtained MO@MOF material has a novel morphology, and the combination of MOF and metal oxide is stable. The combination of MOF with rich catalytic sites and polar metal oxide is beneficial to improving the material's electrical conductivity and polysulfide adsorption catalytic performance. This product can be combined with a conductive agent and elemental sulfur as a positive electrode material for lithium-sulfur batteries, and has excellent adsorption catalytic performance in polysulfide conversion.

[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that those skilled in the art may make several variations and improvements without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.

[0043] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed to be common technical features disclosed in the prior art.

[0044] Example 1

[0045] Preparation of Fe3O4@MOF composite materials

[0046] Step 1: Add 150mg of Fe₃O₄ to 20mL of a 0.3% PSS solution, sonicate for 30 minutes, separate using a magnet, and wash twice with alcohol and water. Step 2: Add the Fe₃O₄-PSS to a solution of 1mL of H₂O, 1mL of alcohol (a 99.5% ethanol-water solution is used in all examples), and 8mL of DMF, and sonicate for 30 minutes. Step 3: Add 32.5mg of terephthalic acid, 89.25mg of CoCl₂·6H₂O, and 89.25mg of NiCl₂·6H₂O to 8mL of DMF and stir to dissolve. Step 4: Add the Fe₃O₄-PSS dispersion to the bottle from Step 3 and stir thoroughly with a glass rod. Step 5: After purging the air through the bottle from Step 4 with nitrogen, add 0.2mL of triethylamine, seal, and mix thoroughly. Sonicate for 8 hours, controlling the liquid temperature in the sonicator to not exceed 25°C. After ultrasonication, centrifuge and wash with water and alcohol for 3 to 4 times. The obtained solid was placed in a vacuum oven and dried in vacuum at 60℃ for 12 hours to obtain Fe3O4@MOF. The obtained Fe3O4@MOF material was characterized by TEM, as shown in FIG. Figure 1, showing the morphology of two-dimensional MOF-coated granular Fe3O4.

[0047] Example 2

[0048] Preparation of Fe3O4@MOF composite materials

[0049] Step 1: Add 150mg of Fe₃O₄ to 20mL of a 0.3% PEI solution, sonicate for 30 minutes, separate using a magnet, and wash twice with alcohol and water. Step 2: Add Fe₃O₄-PEI to a solution of 1mL of H₂O, 1mL of alcohol, and 8mL of DMF, and sonicate for 30 minutes. Step 3: Add 32.5mg of terephthalic acid, 89.25mg of CoCl₂·6H₂O, and 89.25mg of NiCl₂·6H₂O to 8mL of DMF and stir to dissolve. Step 4: Add the Fe₃O₄-PSS dispersion to the vial from Step 3 and stir thoroughly with a glass rod. Step 5: Purge the vial from Step 4 with nitrogen, then add 0.2mL of triethylamine, seal, and mix thoroughly. Sonicate for 8 hours, maintaining the liquid temperature in the sonicator above 25°C. After ultrasonication, centrifuge and wash with water and alcohol for 3 to 4 times. The obtained solid was placed in a vacuum oven and dried in vacuum at 60℃ for 12 hours to obtain Fe3O4@MOF. The obtained Fe3O4@MOF material was characterized by scanning electron microscopy, as shown in FIG. Figure 2 , showing the morphology of two-dimensional MOF-coated granular Fe3O4.

[0050] Example 3

[0051] Preparation of MnO2@MOF composite materials

[0052] Step 1: Add 150mg of MnO2 to 20mL of a 0.3% PSS solution, sonicate for 30 minutes, centrifuge, and wash twice with alcohol and water. Step 2: Add MnO2-PSS to a solution of 1mL of H2O, 1mL of alcohol, and 8mL of DMF and sonicate for 30 minutes. Step 3: Add 32.5mg of terephthalic acid, 90.98mg of CuCl2·6H2O, and 89.25mg of NiCl2·6H2O to 8mL of DMF and stir to dissolve. Step 4: Add the MnO2-PSS dispersion to the vial from Step 3 and stir thoroughly with a glass rod. Step 5: Purge the vial from Step 4 with nitrogen, then add 0.2mL of triethylamine, seal, and mix thoroughly. Sonicate for 8 hours, maintaining the liquid temperature in the sonicator above 25°C. After ultrasonication, the mixture was centrifuged and washed with water and alcohol for 3 to 4 times. The obtained solid was placed in a vacuum oven and dried in vacuum at 60°C for 12 h to obtain MnO2@MOF.

[0053] Example 4

[0054] Preparation of Co2O3@MOF composite materials

[0055] Step 1: Add 120mg of Co2O3 to 20mL of a 0.3% PEI solution, sonicate for 30 minutes, centrifuge, and wash twice with alcohol and water. Step 2: Add the Co2O3-PEI to a solution of 1mL of H2O, 1mL of alcohol, and 8mL of DMF and sonicate for 30 minutes. Step 3: Add 32.5mg of terephthalic acid, 91.67mg of ZnCl2·6H2O, and 89.25mg of NiCl2·6H2O to 12mL of DMF and stir to dissolve. Step 4: Add the Co2O3-PSS dispersion to the vial from Step 3 and stir thoroughly with a glass rod. Step 5: Purge the vial from Step 4 with nitrogen, then add 0.2mL of triethylamine, seal, and mix thoroughly. Sonicate for 12 hours, maintaining the liquid temperature in the sonicator above 25°C. After ultrasonication, the mixture was centrifuged and washed with water and alcohol for 3 to 4 times. The obtained solid was placed in a vacuum oven and dried in vacuum at 60°C for 12 h to obtain Co2O3@MOF.

[0056] Example 5

[0057] Preparation of NiO@MOF composites

[0058] Step 1: Add 90 mg of NiO to 20 mL of a 0.3% PSS solution, sonicate for 30 minutes, centrifuge, and wash twice with ethanol and water. Step 2: Add the NiO-PSS to a solution of 2 mL of H₂O, 2 mL of ethanol, and 8 mL of DMF and sonicate for 30 minutes. Step 3: Add 32.5 mg of terephthalic acid, 89.25 mg of CoCl₂·6H₂O, and 99.98 mg of SrCl₂·6H₂O to 8 mL of DMF and stir to dissolve. Step 4: Add the NiO-PSS dispersion to the vial from Step 3 and stir with a glass rod. Step 5: After purging the vial from Step 4 with nitrogen, add 0.3 mL of triethylamine, seal, and mix thoroughly. Sonicate for 8 hours, maintaining the liquid temperature in the sonicator above 25°C. After sonication, centrifuge, wash 3–4 times with water and ethanol, and place the resulting solid in a vacuum oven at 60°C for 18 hours to obtain NiO@MOF.

[0059] Verification Example 1

[0060] The Fe3O4@MOF prepared in Example 1 was loaded with sulfur (Fe3O4@MOF / S) and prepared into electrode sheets to assemble into lithium-sulfur batteries for rate performance testing.

[0061] Experimental instrument: Xinwei charge and discharge tester

[0062] Battery parameters and assembly: Fe3O4@MOF accounts for 24wt% of the positive electrode material, and sulfur accounts for 48wt%. The positive electrode sheet uses 200μm thick Hesen carbon paper as the current collector, with a diameter of 10mm and a sulfur loading of approximately 1mg / cm 2 The electrode sheet was used as the positive electrode sheet, the 19mm diameter Celgard diaphragm was used as the battery diaphragm, the 0.5mm thick 16mm diameter metal lithium sheet was used as the negative electrode, 20μL of electrolyte was added to each side of the diaphragm, and the battery was assembled using a 2025 battery shell.

[0063] Test parameters: The battery was left to stand for two hours before charging and discharging to allow the electrolyte and electrodes to fully soak into the battery. The discharge cut-off voltage was 1.8V and the charge cut-off voltage was 2.8V. The battery was activated by charging and discharging at a rate of 0.05C for the first cycle. The battery was then charged and discharged at rates of 0.1C, 0.2C, 0.3C, 0.5C, 1C, 1.5C, 2C, and 0.5C, respectively.

[0064] The obtained rate performance diagram is shown in Figure 3 As shown in the figure, compared with Fe3O4 / S with the same battery specifications and test parameters, lithium-sulfur batteries with MOF / S as the positive electrode material have higher discharge specific capacity at different rates.

[0065] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various variations or modifications within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a two-dimensional MOF-coated metal oxide composite material, characterized in that: The following steps are involved: (1) Surface charge modification of metal oxides: Weigh the metal oxide and the surface charge modifier, add the polar metal oxide to the aqueous solution of the surface charge modifier, ultrasonically mix, separate the solid in the mixed system, wash it several times with alcohol and water, and discard the liquid to obtain the surface charge-modified polar metal oxide; (2) Dispersion of surface charge-modified metal oxides in a solution: taking the polar metal oxide complex prepared in step (1), adding water, alcohol, and N,N-dimethylformamide (DMF), and performing ultrasonic dispersion to obtain a solid-liquid mixture in which the polar metal is dispersed; (3) adding N,N-dimethylformamide to terephthalic acid and metal salt and stirring to dissolve them to obtain a metal salt solution; (4) adding the solid-liquid mixture in step (2) to the solution in step (3) and stirring and mixing to obtain a solid-liquid mixture; (5) discharging the air in the container of the solid-liquid mixture obtained in step (4); (6) adding triethylamine to the mixture in step (5) and sealing the container; (7) placing the container of step (6) into an ultrasonic instrument for ultrasonication, and controlling the temperature of the mixture in the bottle during ultrasonication; (8) The solid-liquid mixture obtained in step (7) is centrifuged, washed with water and alcohol, and the solid is placed in an oven for vacuum drying to obtain a MOF-coated metal oxide.

2. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: In step (1), the surface charge modifier is one of sodium polyvinylbenzenesulfonate (PSS), polyethyleneimine (PEI), and polyvinylpyrrolidone (PVP); The concentration of the surface charge modifier is 0.1 wt% to 1 wt%.

3. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 2, characterized in that: The surface charge modifier makes the charge-modified polar metal oxide surface have an opposite electronegativity to the MOF surface, thereby generating an electrostatic adsorption effect.

4. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: In step (2), the volume ratio of water, alcohol and N,N-dimethylformamide is 1:1:6-12.

5. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: In step (3), the volume of N,N-dimethylformamide added is the same as that in step (2); In step (3), the ratio of terephthalic acid, metal salt, and DMF is: 32.5 mg: 170-200 mg: 8-12 ml; The metal salt is one or two selected from the group consisting of CoCl2·6H2O, NiCl2·6H2O, SrCl2·6H2O, CuCl2·6H2O, ZnCl2·6H2O and MnCl2·6H2O.

6. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: Step (5) requires introducing a protective gas into the container, and the protective gas can be an inert gas such as nitrogen or argon.

7. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: The volume ratio of triethylamine added in step (6) to the total DMF volume is 1:60-120.

8. The method for preparing a two-dimensional MOF-coated metal oxide composite material according to claim 1, characterized in that: In step (7), the ultrasonic time is 6 to 12 hours, and the temperature of the ultrasonic container is controlled to be lower than 25° C. during the ultrasonication.

9. A two-dimensional MOF-coated metal oxide obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The MOF-coated metal oxide has a core-shell structure in which a two-dimensional layered MOF coats a granular metal oxide.

10. Use of the two-dimensional MOF-coated metal oxide as claimed in claim 9 in the preparation of positive electrode materials for lithium-sulfur batteries.

Citation Information

Patent Citations

  • CuCo bimetal organic framework composite sulfur material and preparation and application thereof

    CN109360960A

  • Molybdenum disulfide nanosheet coated titanium-based MOF derived titanium dioxide composite material as well as preparation method and application thereof

    CN113023778A

  • Lithium-sulfur battery positive electrode material based on catalytic transition metal oxide nanorods and preparation method of lithium-sulfur battery positive electrode material

    CN114497487A

  • Preparation method for iron-cobalt phosphide / carbon composite material having layered structure, and button cell