Seamless continuous tubing for hydrogen injection in underground hydrogen storage facilities and its preparation method
By employing seamless processing methods, including slitting of rolled plates, laser welding, and multi-pass hot extrusion, the corrosion and hydrogen embrittlement problems of continuous tubes during hydrogen injection were solved, the hydrogen resistance of the weld area was improved, and the long-term stability and safety of the continuous tubes were ensured.
Patent Information
- Application Number
- CN202311065845.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-22
AI Technical Summary
Conventional continuous tubing is prone to corrosion and hydrogen embrittlement during hydrogen injection, and the weld area is a weak point, leading to hydrogen leakage and easy damage to the weld joint.
The seamless processing method employs a process involving the preparation of rolled steel sheets, longitudinal shearing of steel strips, laser welding, inert gas protection, solution heat treatment, and multi-pass hot extrusion to ensure consistent weld structure and improve durability.
This solved the corrosion and hydrogen embrittlement problems of continuous tubing, improved the hydrogen resistance of the weld area, and ensured the long-term stability and safety of the continuous tubing.
Smart Images

Figure CN119501473B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of continuous tube fabrication technology, and more specifically, to an engineered seamless continuous tube for hydrogen injection in underground hydrogen storage facilities and its fabrication method. Background Technology
[0002] Coiled Tube (CT), also known as flexible tubing, features pressurized operation and continuous lifting and lowering. It is small in size, has a fast operation cycle, and low cost. A single tube can reach tens of thousands of meters in length. It can be repeatedly deformed and carry operating tools. It can carry out all types of operations in well workover, logging, drilling, and well completion. It can also be used in onshore and offshore oil and gas gathering and transportation pipelines. It is an indispensable high-end oil pipe material in today's petroleum industry.
[0003] Using coiled tubing instead of conventional tubing for hydrogen injection into underground hydrogen storage facilities solves the corrosion problem that easily occurs near the casing couplings during hydrogen injection using conventional tubing. It also allows for direct pressurized operation, fully meeting the operating pressure requirements for underground hydrogen storage and significantly reducing operating costs. However, conventional coiled tubing is susceptible to hydrogen embrittlement, as hydrogen molecules easily enter and accumulate in the metal. Simply using coiled tubing for hydrogen injection cannot prevent hydrogen embrittlement. Furthermore, the welding process required during forming creates a weak point in the coiled tubing, and the residual stress in the weld further increases the risk of hydrogen embrittlement.
[0004] Currently, corrosion easily occurs at conventional tubing joints, leading to poor wellbore sealing and hydrogen leakage. Conventional coiled tubing is not resistant to hydrogen embrittlement. The weakest point of the coiled tubing is the welded joint, where high temperatures can cause water and hydrogen atoms to dissolve and enter the weld, resulting in hydrogen corrosion and other problems. Summary of the Invention
[0005] This application aims to solve or improve the aforementioned technical problems.
[0006] Therefore, the primary objective of this application is to provide a method for preparing seamless continuous tubing for hydrogen injection into underground hydrogen storage facilities.
[0007] The second objective of this application is to provide a seamless continuous pipe for hydrogen injection into an underground hydrogen storage facility.
[0008] To achieve the first objective of this application, the technical solution of the first aspect of this application provides a method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility, comprising: preparing a coil; longitudinally shearing the coil to obtain multiple steel strips; welding the multiple steel strips using a first welding method and protecting the weld seam with a first inert gas to obtain butt-jointed steel strips; milling the edges of the butt-jointed steel strips and bending them into shape using rollers, welding them using a second welding method and protecting the weld seam with a second inert gas; welding the longitudinal seam using an I-type nick to form the entire tube; after welding, performing bright solution heat treatment under argon protection using a solution heat treatment unit to obtain a tube blank; coiling the tube blank and performing multiple hot extrusions on the tube blank to obtain a seamless continuous tube.
[0009] According to the method for preparing seamless continuous tubing for hydrogen injection in underground hydrogen storage facilities provided in this application, a coil is first prepared. The coil is then longitudinally sheared to obtain multiple steel strips. These steel strips are welded using a first welding method, and the weld seams are protected with a first inert gas to obtain butt-jointed steel strips. The butt-jointed steel strips are milled, bent into shape using rollers, and then welded using a second welding method, with the weld seams protected with a second inert gas. The longitudinal seam is welded using an I-type weld joint to form the entire tube. After welding, the tube undergoes bright solution heat treatment under argon protection in a solution heat treatment unit to obtain a tube blank. After the tube blank is manufactured, the continuous tubing is coiled and transported to a hot extrusion unit for hot extrusion of the weld seams, ensuring seamless weld seams and obtaining a seamless continuous tubing. This ensures the consistency of the base material structure of the weld seams and improves the durability of the continuous tubing.
[0010] It is understandable that the seamless processing of continuous pipe is considered to be hot extrusion forming. Hot extrusion uses a transmission device to transport the pipe to the extrusion equipment for hot extrusion. Therefore, a certain amount of hot extrusion needs to be considered in the selection of plate thickness. The selection of extrusion amount mainly considers the breakage and growth of the weld structure at the welding position, and ensures that the overall quality of the pipe remains unchanged. The pipe is then cut into steel strips of the specified width by a slitting unit.
[0011] In addition, the technical solution provided in this application may also have the following additional technical features:
[0012] In the above technical solution, the preparation of the coil specifically includes: placing the raw materials into an electric furnace to complete the melting and roughing process to obtain roughed steel; transferring the roughed steel into an argon-oxygen decarburization (AOD) furnace, introducing an oxygen-argon mixed gas into the AOD furnace, and adjusting the oxygen-argon ratio in the mixed gas according to the carbon content in the roughed steel; and removing slag from the roughed steel after the carbon content in the roughed steel reaches the preset carbon content.
[0013] In this technical solution, the preparation of steel coils involves first melting and rough refining raw materials such as scrap steel in an electric furnace. Then, the molten steel is transferred to an argon-oxygen decarburization (AOD) furnace, where a certain proportion of oxygen-argon mixed gas is introduced. The oxygen-argon ratio in the mixed gas is continuously adjusted according to the carbon content of the molten steel. Once the carbon content meets the requirements for the steel grade, slag removal is performed. Using a full-process ultra-high-efficiency electric furnace and a clean argon-oxygen decarburization (AOD) furnace smelting technology, deep degassing, decarburization, desulfurization, and dephosphorization can be achieved.
[0014] The above technical solution for preparing coils also includes: transferring the rough molten steel after slag removal into the LF furnace of the ladle for refining to obtain refined molten steel; when the composition and temperature of the refined molten steel reach the preset composition and preset temperature, transporting the refined molten steel to the continuous casting platform for casting to obtain ingots; and after the ingots cool, mechanically polishing the oxide scale on the surface of the ingots.
[0015] In this technical solution, the preparation of the coil also includes transferring the rough molten steel after slag removal into a ladle LF furnace for refining to obtain refined molten steel. Once the composition and temperature of the refined molten steel reach the preset values, it is transported to a continuous casting platform for casting to obtain ingots. After the ingots cool, the oxide scale on their surface is mechanically polished. Using a full-process ultra-electric furnace, a clean argon-oxygen decarburization AOD furnace smelting technology, and a ladle LF refining process, deep degassing, decarburization, desulfurization, and dephosphorization can be achieved.
[0016] In the above technical solution, the rough molten steel after slag removal is transferred to the LF furnace of the ladle for refining to obtain refined molten steel. Specifically, this includes adjusting the composition of the rough molten steel after slag removal by adding reducing agents and slag-forming materials to obtain refined molten steel.
[0017] In this technical solution, the rough molten steel after slag removal is transferred to the LF furnace in the ladle for refining to obtain refined molten steel. Specifically, reducing agents and slag-forming materials are added to adjust the composition of the rough molten steel after slag removal to obtain refined molten steel.
[0018] In the above technical solution, the preparation of the coil also includes: placing the polished ingot into a continuous rolling mill for multi-pass hot continuous rolling to obtain an initial coil, and performing online solution treatment on the initial coil at 1050℃-1100℃ to obtain a rolled finished plate.
[0019] In this technical solution, the preparation of the coil also includes placing the polished ingot into a continuous rolling mill for multi-pass hot continuous rolling to obtain an initial coil. The initial coil is then subjected to online solution treatment at 1050℃-1100℃ to obtain the rolled finished plate.
[0020] The above technical solution includes preparing the coil by pickling and phosphating the rolled product plate, and then coiling the rolled product plate to obtain the coil.
[0021] In this technical solution, the preparation of the coil also includes pickling and phosphating the rolled product plate, and then coiling the rolled product plate to obtain the coil.
[0022] In the above technical solution, the reducing agent includes one or a combination of the following: ferrosilicon, chromium silicon, and aluminum.
[0023] In this technical solution, the reducing agent includes ferrosilicon, silicon chromium, and aluminum.
[0024] In the above technical solution, the slag-forming materials include lime and / or fluorite.
[0025] In this technical solution, the slag-forming material includes lime or fluorite.
[0026] In the above technical solution, the chemical composition of the coiled plate by mass percentage is as follows: C: ≤0.02%; Si: ≤0.7%; Mn: ≤2.0%; P: ≤0.009%; S: ≤0.003%; Cr: 16%-26%; Ni: 10%-30%; N: 0.05%-1.0%; Mo: 1.6%-3.0%, with the remainder being Fe and unavoidable impurities.
[0027] In this technical solution, the chemical composition of the coil is characterized by low C, high Cr, high Ni, low Mo, low Mn, and low nitrogen. The high Cr and high Ni chemical composition is key to ensuring that the continuous tube has a high resistance to hydrogen environment. The selection of Cr and Ni content mainly depends on parameters such as hydrogen partial pressure and temperature in the hydrogen environment.
[0028] In the above technical solution, multiple steel strips are welded using a first welding method, and the weld is protected by a first inert gas to obtain butt-jointed steel strips. Specifically, this includes: connecting multiple steel strips using a 40°-50° oblique joint method, and welding the multiple steel strips using the first welding method; protecting the weld with a first inert gas, and performing solution heat treatment on the butt-joint weld at 1050℃-1100℃; and grinding and non-destructive testing on the weld area to obtain butt-jointed steel strips.
[0029] In this technical solution, multiple steel strips are welded using a first welding method, and the weld is protected by a first inert gas to obtain butt-jointed steel strips. Specifically, welding methods such as laser welding, resistance spot welding, friction stir welding, and plasma filler wire are used. The weld is protected by inert gases such as helium and argon. The steel strips are connected by a 40°-50° bevel joint method, and the butt weld is subjected to solution heat treatment at 1050℃-1100℃. The weld area is then ground and subjected to non-destructive testing. Multiple steel strips are then beveled, solution heat treated, and ground to the target length.
[0030] In the above technical solution, the first welding method includes one or a combination of the following: laser welding, resistance spot welding, friction stir welding, and plasma filler wire welding.
[0031] In this technical solution, the first welding method includes laser welding, resistance spot welding, friction stir welding, and plasma filler wire welding.
[0032] In the above technical solution, the first inert gas includes helium and / or argon.
[0033] In this technical solution, the first inert gas includes helium or argon.
[0034] In the above technical solution, the second welding method includes one or a combination of the following: laser welding, carbon dioxide gas shielded welding, and plasma welding.
[0035] In this technical solution, the second welding method includes laser welding, carbon dioxide gas shielded welding, and plasma welding.
[0036] In the above technical solution, the second inert gas includes helium with a purity of 100%; and / or the second inert gas includes argon with a purity of ≥99.7% and nitrogen with a purity of 2%.
[0037] In this technical solution, the second inert gas includes 100% helium or ≥99.7% argon and 2% nitrogen.
[0038] In the above technical solution, the heat treatment temperature for bright solution heat treatment is 1050℃-1100℃.
[0039] In this technical solution, the heat treatment temperature for bright solution heat treatment is 1050℃-1100℃.
[0040] In the above technical solution, the tube blank is coiled and subjected to multiple hot extrusions to obtain a seamless continuous tube. Specifically, this includes: conveying the tube blank through rollers adapted to its size and feeding it into an online heat treatment furnace and hot extrusion equipment; subjecting the tube blank to multiple online heat treatments and hot extrusions to obtain a seamless continuous tube. The temperature of the online heat treatment needs to be higher than the sensitization temperature range of the material.
[0041] In this technical solution, the tube blank is coiled and subjected to multiple hot extrusions to obtain a seamless continuous tube. Specifically, the tube blank is first extruded and transported by rollers adapted to its dimensions, and then enters an online heat treatment furnace for online heat treatment. The tube blank after online heat treatment is then subjected to multiple hot extrusions to obtain a seamless continuous tube with a high surface finish. This multi-pass hot extrusion process is used to process high-performance seamless continuous tubes for hydrogen injection into hydrogen storage facilities. A novel rear-drive method is employed to move the continuous tube, and the lower pushing speed ensures uniform thrust during hot extrusion. Uniform hot extrusion of the continuous tube ensures the consistency of the base material microstructure of the weld seam. The consistency of the coiling and extrusion speeds eliminates slippage and dislocations generated during hot rolling, welding, and stretching. The online heat treatment temperature is higher than the sensitization temperature range of the material, with the specific temperature range determined based on the specific material.
[0042] In the above technical solution, the tube blank undergoes multiple online heat treatments and hot extrusions to obtain a seamless continuous tube for engineering applications. Specifically, this includes: performing online heat treatment on the tube blank; transferring the tube blank after online heat treatment to a hot extrusion unit to perform hot extrusion on the tube blank segments; immediately cooling the tube blank segments after hot extrusion, and then coiling the tube blank onto a large coil; reversing the hot extrusion conveyor to perform a second hot extrusion on the tube blank to obtain a seamless continuous tube for engineering applications.
[0043] In this technical solution, the tube blank undergoes multiple online heat treatments and hot extrusions to obtain a seamless continuous tube. Specifically, the tube blank is first subjected to online heat treatment, and then fed into a hot extrusion unit for hot extrusion of the tube blank sections. After hot extrusion, the tube blank sections are water-cooled, and then coiled onto a large coil. Finally, the hot extrusion conveyor is reversed for a second hot extrusion to obtain a seamless continuous tube. The water cooling method ensures that the tube material is rapidly cooled from the austenitic temperature range to room temperature after hot extrusion, effectively avoiding the formation of low-temperature precipitates, thereby further ensuring that the tube material and welds have good resistance to hydrogen embrittlement.
[0044] In the above technical solution, the transmission speed is less than or equal to 15 mm / s.
[0045] In this technical solution, the transmission speed is less than or equal to 15 mm / s.
[0046] In the above technical solution, the temperature of the online heat treatment is greater than or equal to 950℃.
[0047] In this technical solution, the online heat treatment temperature is greater than or equal to 950℃.
[0048] To achieve the second objective of this application, the technical solution of the second aspect of this application provides a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility. It is prepared using the preparation method of the seamless continuous tube for hydrogen injection in an underground hydrogen storage facility as described in any of the technical solutions of the first aspect of this application, and therefore has the technical effects of any of the technical solutions of the first aspect, which will not be repeated here.
[0049] Additional aspects and advantages of this application will become apparent in the following description or may be learned by practice of this application. Attached Figure Description
[0050] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0051] Figure 1 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0052] Figure 2 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0053] Figure 3 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0054] Figure 4 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0055] Figure 5 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0056] Figure 6 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0057] Figure 7 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0058] Figure 8 This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application.
[0059] Figure 9This is a schematic flowchart illustrating the steps of a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility, according to one embodiment of this application. Detailed Implementation
[0060] To better understand the above-mentioned objectives, features, and advantages of this application, the application will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.
[0061] Many specific details are set forth in the following description in order to provide a full understanding of this application. However, this application may also be implemented in other ways different from those described herein. Therefore, the scope of protection of this application is not limited to the specific embodiments disclosed below.
[0062] The following reference Figures 1 to 9 This application describes some embodiments of seamless continuous tubing for hydrogen injection into underground hydrogen storage facilities and its preparation method.
[0063] like Figure 1 As shown, an embodiment of the first aspect of this application provides a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage reservoir, comprising the following steps:
[0064] Step S102: Prepare the rolled plate;
[0065] Step S104: Slit the coil to obtain multiple steel strips;
[0066] Step S106: Weld multiple steel strips using a first welding method, and protect the weld seam with a first inert gas to obtain butt-jointed steel strips;
[0067] Step S108: After milling the edges of the butt steel strip, it is bent into shape by rollers, welded by the second welding method, and the weld is protected by the second inert gas.
[0068] Step S110: The longitudinal seam is welded into a whole pipe using a type I break. After welding, the pipe blank is subjected to bright solution heat treatment under argon protection in a solution heat treatment unit to obtain the pipe blank.
[0069] Step S112: The tube blank is coiled and subjected to multiple hot extrusions to obtain a seamless continuous tube.
[0070] According to the method for preparing seamless continuous tubing for hydrogen injection in underground hydrogen storage facilities provided in this application, a rolled sheet is first prepared. The rolled sheet is then longitudinally sheared to obtain multiple steel strips. These steel strips are welded using a first welding method, and the weld seam is protected with a first inert gas to obtain butt-jointed steel strips. The butt-jointed steel strips are milled, bent into shape using rollers, and then welded using a second welding method, with the weld seam protected with a second inert gas. The longitudinal seam is welded using a type I weld joint. After welding, the tubing undergoes bright solution heat treatment under argon protection in a solution heat treatment unit to obtain a tube blank. After the tube blank is manufactured, the continuous tubing is coiled and transported to a hot extrusion unit for hot extrusion of the weld seam to ensure seamless weld treatment, resulting in a seamless continuous tubing. This ensures the consistency of the microstructure of the base material in the weld seam of the continuous tubing and improves its durability.
[0071] It is understandable that, considering the seamless processing of continuous tubes as hot extrusion forming, the hot extrusion transmission device uses a four-jaw transmission device to drive the tube to the extrusion equipment for hot extrusion. Therefore, a certain amount of hot extrusion needs to be considered in the selection of plate thickness. The selection of extrusion amount mainly considers the breakage and growth of the weld structure at the welding position, and ensures that the overall quality of the tube remains unchanged. The tube is then cut into steel strips of the specified width by a slitting unit.
[0072] like Figure 2 As shown, according to an embodiment of this application, a method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility includes the following steps:
[0073] Step S202: Place the raw materials into an electric furnace to complete the melting and rough refining process, and obtain rough steel.
[0074] Step S204: Transfer the crude steel to the argon-oxygen decarburization AOD furnace, introduce the oxygen-argon mixed gas into the argon-oxygen decarburization AOD furnace, and adjust the ratio of oxygen and argon in the mixed gas according to the carbon content in the crude steel.
[0075] Step S206: When the carbon content of the crude steel reaches the preset carbon content, the crude steel is subjected to slag removal treatment.
[0076] In this embodiment, the preparation of the coil involves first melting and rough refining raw materials such as scrap steel in an electric furnace, then transferring the molten steel to an argon-oxygen decarburization (AOD) furnace. A certain proportion of oxygen-argon mixed gas is introduced into the furnace, and the oxygen-argon ratio in the mixed gas is continuously adjusted according to the carbon content of the molten steel. Once the carbon content meets the requirements for the steel grade, slag removal is performed. Using the full-process ultra-high-efficiency electric furnace and clean argon-oxygen decarburization (AOD) furnace smelting technology, deep degassing, decarburization, desulfurization, and dephosphorization can be achieved.
[0077] like Figure 3As shown, the method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application, including the preparation of the coil, further comprises the following steps:
[0078] Step S302: Transfer the rough molten steel after slag removal to the LF furnace in the ladle for refining to obtain refined molten steel;
[0079] Step S304: When the composition and temperature of the refined molten steel reach the preset composition and preset temperature, the refined molten steel is transported to the continuous casting platform for casting to obtain ingots;
[0080] Step S306: After the ingot cools, the oxide scale on the surface of the ingot is mechanically polished.
[0081] In this embodiment, the preparation of the coil also includes transferring the rough molten steel after slag removal into a ladle LF furnace for refining to obtain refined molten steel. Once the composition and temperature of the refined molten steel reach the preset values, it is transported to a continuous casting platform for casting to obtain ingots. After the ingots cool, the oxide scale on their surface is mechanically polished. Using a full-process ultra-electric furnace, a clean argon-oxygen decarburization AOD furnace smelting technology, and a ladle LF refining process, deep degassing, decarburization, desulfurization, and dephosphorization can be achieved.
[0082] like Figure 4 As shown, according to an embodiment of this application, a method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility involves transferring the rough molten steel after slag removal into an LF furnace for refining to obtain refined molten steel. The method specifically includes the following steps:
[0083] Step S402: Adjust the composition of the crude steel after slag removal by adding reducing agent and slag-forming material to obtain refined steel.
[0084] In this embodiment, the rough molten steel after slag removal is transferred to an LF furnace for refining to obtain refined molten steel. Specifically, this is achieved by adding reducing agents and slag-forming materials to adjust the composition of the rough molten steel after slag removal. The reducing agents include ferrosilicon, silicon chromium, and aluminum. The slag-forming materials include lime or fluorite.
[0085] like Figure 5 As shown, the method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application, including the preparation of the coil, further comprises the following steps:
[0086] Step S502: The polished ingot is placed into a continuous rolling mill for multi-pass hot continuous rolling to obtain an initial coil. The initial coil is then subjected to online solution treatment at 1050℃-1100℃ to obtain a rolled finished plate.
[0087] In this embodiment, the preparation of the coil also includes placing the polished ingot into a continuous rolling mill for multi-pass hot continuous rolling to obtain an initial coil. The initial coil is then subjected to online solution treatment at 1050℃-1100℃ to obtain a rolled finished plate.
[0088] like Figure 6 As shown, the method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to an embodiment of this application, including the preparation of the coil, further comprises the following steps:
[0089] Step S602: Pickling and phosphating are performed on the rolled finished plate, and the rolled finished plate is coiled to obtain a coil plate.
[0090] In this embodiment, the preparation of the coil also includes pickling and phosphating the rolled product plate, and coiling the rolled product plate to obtain the coil.
[0091] In the above embodiments, the chemical composition of the coil, by mass percentage, is as follows: C: ≤0.02%; Si: ≤0.7%; Mn: ≤2.0%; P: ≤0.009%; S: ≤0.003%; Cr: 16%-26%; Ni: 10%-30%; N: 0.05%-1.0%; Mo: 1.6%-3.0%, with the remainder being Fe and unavoidable impurities. It can be understood that the chemical composition of the coil is characterized by low C, high Cr, high Ni, low Mo, low Mn, and low nitrogen. The high Cr and high Ni chemical composition is key to ensuring the continuous tube has high resistance to hydrogen environments. The selection of Cr and Ni content mainly depends on parameters such as hydrogen partial pressure and temperature in the hydrogen environment.
[0092] like Figure 7 As shown, according to an embodiment of this application, a method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility involves welding multiple steel strips using a first welding method and protecting the weld seam with a first inert gas to obtain butt-jointed steel strips. The method specifically includes the following steps:
[0093] Step S702: Connect multiple steel strips by a 40°-50° oblique splice method, and weld the multiple steel strips by a first welding method;
[0094] Step S704: Protect the weld with a first inert gas and perform solution heat treatment on the butt weld at 1050℃-1100℃.
[0095] Step S706: Grind and perform non-destructive testing on the weld area to obtain the butt-jointed steel strip.
[0096] In this embodiment, multiple steel strips are welded using a first welding method, and the weld is protected by a first inert gas to obtain butt-jointed steel strips. Specifically, welding methods such as laser welding, resistance spot welding, friction stir welding, and plasma filler wire are used. The weld is protected by inert gases such as helium and argon. The steel strips are connected by a 40°-50° bevel joint method, and the butt weld is subjected to solution heat treatment at 1050℃-1100℃. The weld area is then ground and subjected to non-destructive testing. Multiple steel strips are then beveled, solution heat treated, and ground to the target length.
[0097] In some embodiments, the first welding method includes laser welding, resistance spot welding, friction stir welding, and plasma filler wire welding. The first inert gas includes helium or argon. The second welding method includes laser welding, carbon dioxide gas shielded welding, and plasma welding. The second inert gas includes 100% pure helium or argon with a purity of ≥99.7% and nitrogen with a purity of 2%.
[0098] In the above embodiments, the heat treatment temperature for bright solution heat treatment is 1050℃-1100℃.
[0099] like Figure 8 As shown, according to an embodiment of this application, a method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility involves coiling a tube blank and subjecting it to multiple hot extrusions to obtain a seamless continuous tube. The method specifically includes the following steps:
[0100] Step S802: The tube blank is conveyed by rollers adapted to the size of the tube blank and enters the online heat treatment furnace and hot extrusion equipment;
[0101] Step S804: Perform multiple online heat treatments and hot extrusions on the tube blank to obtain a seamless continuous tube. The temperature of the online heat treatment is higher than the sensitization temperature range of the material.
[0102] In this embodiment, the tube blank is coiled and subjected to multiple hot extrusions to obtain a seamless continuous tube. Specifically, the tube blank is first extruded and transported by rollers adapted to its dimensions, and then enters an online heat treatment furnace for online heat treatment. The tube blank after online heat treatment is then subjected to multiple hot extrusions to obtain a seamless continuous tube. This multi-pass hot extrusion process is used to process high-performance seamless continuous tubes for hydrogen injection into hydrogen storage facilities. A novel rear-drive method is employed to move the continuous tube, and the lower pushing speed ensures uniform thrust during hot extrusion. Uniform hot extrusion of the continuous tube ensures the consistency of the microstructure of the weld seam base material. The consistency of the coiling and extrusion speeds eliminates slippage and dislocations generated during hot rolling, welding, and stretching. The online heat treatment temperature is higher than the sensitization temperature range of the material, and the specific temperature range is determined based on the specific material.
[0103] like Figure 9 As shown, according to an embodiment of this application, a method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility involves subjecting a tube blank to multiple online heat treatments and hot extrusions to obtain a seamless continuous tube. The method specifically includes the following steps:
[0104] Step S902: Perform online heat treatment on the tube blank;
[0105] Step S904: The tube blank after online heat treatment is fed into the hot extrusion unit to hot extrude the tube blank into tube sections;
[0106] Step S906: After hot extrusion, the tube section of the billet is cooled immediately, and after cooling, the billet is coiled onto a large coil.
[0107] Step S908: Reverse the hot extrusion conveyor to perform secondary hot extrusion on the tube blank to obtain a continuous tube with seamless engineering treatment.
[0108] In this embodiment, the tube blank undergoes multiple online heat treatments and hot extrusions to obtain a seamless continuous tube. Specifically, the tube blank is first subjected to online heat treatment, and then fed into a hot extrusion unit for hot extrusion of the tube blank segments. After hot extrusion, the tube blank segments are water-cooled, and then coiled onto a large coil. Finally, the hot extrusion conveyor is reversed for a second hot extrusion to obtain a seamless continuous tube. The water cooling method ensures that the tube material is rapidly cooled from the austenitic temperature range to room temperature after hot extrusion, effectively avoiding the formation of low-temperature precipitates, thereby further ensuring that the tube material and welds have good resistance to hydrogen embrittlement.
[0109] The transmission speed is less than or equal to 15 mm / s. The online heat treatment temperature is greater than or equal to 950℃.
[0110] The second aspect of this application provides a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility, which is prepared using the same method as described in any of the first aspects above. Therefore, it has the technical effects of any of the first aspects above, which will not be repeated here.
[0111] According to a specific embodiment of this application, a seamless continuous pipe for hydrogen injection in an underground hydrogen storage facility is used. It is formed into a continuous pipe through welding using a specialized hydrogen-resistant material. The finished continuous pipe undergoes hot extrusion to ensure the consistency of the weld seams, including the oblique weld seams, straight weld seams, and base material, guaranteeing the uniformity of the weld seam and base material microstructure. The chemical composition of the coiled steel, by mass percentage, is: C: ≤0.02%; Si: ≤0.7%; Mn: ≤2.0%; P: ≤0.009%; S: ≤0.003%; Cr: 16-26%; Ni: 10-30%; N: 0.05-1.0%; Mo: 1.6-3.0%, with the remainder being Fe and unavoidable impurities.
[0112] The seamless continuous tubing used for hydrogen injection in the aforementioned underground hydrogen storage facility includes the following steps:
[0113] (1) Coil preparation: First, raw materials such as scrap steel are put into EAF (electric furnace) for melting and roughing. Then, the smelted molten steel is transferred to argon-oxygen decarburization AOD furnace. A certain proportion of oxygen-argon mixed gas is introduced into the furnace, and the oxygen-argon ratio in the mixed gas is continuously adjusted according to the carbon content of the molten steel. When the carbon content meets the requirements of the steel grade, slag removal is performed. Finally, it is put into the ladle LF furnace for refining. During the refining process, a certain amount of reducing agents such as ferrosilicon, silicon chromium, and aluminum, as well as slag-forming materials such as lime and fluorite, can be added according to the composition of the molten steel. When the composition and temperature meet the requirements, the molten steel is transported to the continuous casting platform for casting. After the ingot cools, the oxide scale on the surface of the ingot is mechanically polished. After polishing, it is put into the continuous rolling mill for multi-pass hot continuous rolling. The coil is subjected to online solution treatment at a temperature of 1050℃-1100℃. After rolling, the coil is pickled and phosphated, and the rolled product is coiled.
[0114] (2) Slitting and welding of rolled plates: Considering that the continuous tube is made seamless by hot extrusion, the hot extrusion uses a transmission device to drive the tube to the extrusion equipment and hot extrudes the tube. Therefore, a certain amount of hot extrusion needs to be considered in the selection of plate thickness. The selection of extrusion amount mainly considers the breakage and growth of the weld structure at the welding position, and ensures that the overall quality of the tube remains unchanged. The tube is cut into steel strips of the specified width by the slitting unit.
[0115] (3) Welding methods such as laser welding, resistance spot welding, friction stir welding, and plasma filler are adopted. The weld is protected by inert gas such as helium and argon. The steel strips are connected by a 40°-50° bevel joint. The butt weld is subjected to solution heat treatment at 1050℃-1100℃. The weld area is ground and non-destructive tested. Multiple steel strips are beveled, solution heat treated and ground to the target length.
[0116] (3) Tube blank preparation: After the steel strip is milled, it is bent into shape by rollers and welded by laser welding, carbon dioxide gas shielded welding, plasma welding and other methods. The entire welding process is protected by 100% pure helium or ≥99.7% pure argon + 2% nitrogen for laser welding protection of the weld. The longitudinal seam is welded by I-type break. After welding, it is subjected to bright solution heat treatment under the protection of argon in the solution heat treatment unit. The heat treatment temperature is 1050℃-1100℃. After the tube blank is manufactured, the continuous tube is coiled and transported to the hot extrusion equipment unit to perform hot extrusion of the weld to ensure seamless treatment of the weld.
[0117] (5) Hot extrusion process: The hot extrusion equipment uses rollers adapted to the size of the continuous tube to extrude and transport the continuous tube. The transport speed is consistent with the rolling speed of the continuous tube finished tube coiling equipment. The continuous tube is driven forward by the rollers and then enters the online heat treatment furnace for online heat treatment. The heat treatment temperature is ≥ the austenitic forming temperature. After passing through the online heat treatment furnace, the tube enters the hot extrusion unit to perform hot extrusion on the tube section. After hot extrusion, the tube section is water-cooled and then coiled onto a large coil. The hot extrusion transport equipment is reversed to perform two hot extrusions on the tube. After multiple extrusions, the entire tube body of the continuous tube is completed through multiple hot extrusions to ensure the consistency of the weld, heat-affected zone, and base material structure, making the continuous tube a seamless continuous tube. This process requires a low transport speed (≤15mm / s) to eliminate voids and defects generated by hot extrusion and ensure that the tube has good resistance to hydrogen embrittlement.
[0118] The wall thickness of the seamless continuous tubing used for hydrogen injection in underground hydrogen storage facilities ranges from 1.0 to 6.0 mm, and the length ranges from 100 to 8000 m. It can be wound onto a drum of appropriate core diameter for transportation and use.
[0119] Specifically, the chemical composition of the board by mass percentage is as follows: C: 0.02%; Si: 0.5%; Mn: 2%; P: 0.003%; S: 0.0001%; Cr: 21.5%; Ni: 23.5%; Mo: 1.0%; N: 0.12%; the remainder is Fe and unavoidable impurities.
[0120] 1. Coil preparation: First, the raw materials such as scrap steel are calculated according to the percentage of elements in the finished product and put into EAF (electric furnace) for melting and rough refining. Then, 110t of molten steel is transferred to argon-oxygen decarburization AOD furnace. A certain proportion of oxygen-argon mixed gas is introduced into the furnace, and the oxygen-argon ratio in the mixed gas is continuously adjusted according to the carbon content in the molten steel. When the carbon content reaches the steel grade requirements, slag removal is performed, and finally, it enters the ladle LF furnace for secondary refining. During the refining process, a certain amount of reducing agents such as ferrosilicon, silicon chromium, and aluminum, as well as slag-forming materials such as lime and fluorite, can be added to adjust the composition of the molten steel. When the composition and temperature meet the requirements, the molten steel is transported to the continuous casting platform for casting. After the ingot cools, the oxide scale on the surface of the ingot is mechanically polished. After polishing, it is placed in the continuous rolling mill for multi-pass hot continuous rolling. The coil is subjected to online solution treatment at a solution temperature of 1070℃. After rolling, the coil is pickled and phosphated, and the rolled product is sawed and coiled.
[0121] 2. Slitting and splicing of rolled steel sheets:
[0122] Since the final pipe size is 63*4.0mm and the pipe injection length is 1500m, and because the extrusion process involves internal and external hot extrusion, the welded pipe needs to have a certain amount of extrusion allowance on both the inner and outer diameters. 4.8mm sheet metal is used for welding and forming, and the formed pipe size is 63.4*4.8mm. According to the principle of volume conservation, 1258 meters of continuous tubing with a wall thickness of 63.4mm*4.8mm is required. According to the calculation, the continuous pipe requires a slitting width of 204mm for the rolled plate. The rolled plate is then slitted to a width of 204mm.
[0123] The sheet metal is uncoiled, and the head is beveled at 45°. The beveled sheet metal is placed in a vacuum laser welding heat treatment device to perform laser butt welding on the beveled sheet metal. The butt welded sheet metal is then subjected to vacuum solution heat treatment and rapidly cooled with argon gas.
[0124] 3. Preparation of tube blank:
[0125] After milling the edges of the butt steel strip, it is bent into shape by rollers and then welded into a pipe blank by laser welding. Argon gas with a purity of ≥99.7% is used to protect the straight seam of the pipe during the welding process.
[0126] 4. Heat treatment of the entire tube:
[0127] The continuous tube is subjected to online solution heat treatment using a whole-tube heat treatment equipment. The solution heat treatment temperature is 1080℃ and the solution treatment time needs to be ≥1min.
[0128] 5. Hot extrusion process of tube blank:
[0129] A Φ63.4×4.8mm continuous tube is moved to the hot extrusion equipment by an overhead crane for hot extrusion at 1080℃. After unfolding, the tube is directly fed into the hot extrusion die by conveyor rollers. A 63.2mm fixed outer diameter die with a 54.4mm internal expansion head is used to push the Φ63.4×4.8mm continuous tube into the hot extrusion die at a speed of 8mm / s. -2 After extrusion, the tube diameter is 63.2 mm and the wall thickness is 4.5 mm. After hot extrusion, the extruded tube is driven by the conveyor extrusion rollers. After one hot extrusion, the direction of the drive rollers is changed, the hot extrusion die is replaced, and the continuous tube is subjected to a second hot extrusion. The second hot extrusion uses a 63 mm outer extrusion die and a 55 mm inner bulging head to perform a second hot extrusion on the continuous tube. The extrusion speed is 6 mm / s. -2 .
[0130] 6. Main performance:
[0131] The above method produces a high-performance seamless continuous pipe for hydrogen injection in underground hydrogen storage facilities and a manufacturing method thereof. The pipe can withstand an internal pressure of ≥35MPa, and the weld and base material are not sensitive to hydrogen environment at 15MPa.
[0132] In summary, the beneficial effects of the embodiments of this application are as follows:
[0133] 1. The chemical composition of low C, high Cr, high Ni, low Mo, low Mn, and low nitrogen, with high Cr and high Ni, is key to ensuring that the continuous tube has a high resistance to hydrogen environment.
[0134] 2. The entire process of ultra-EAF (electric furnace), clean argon-oxygen decarburization AOD furnace smelting technology and ladle LF refining process is adopted to achieve deep degassing, decarburization, desulfurization and dephosphorization.
[0135] 3. High-performance seamless continuous tubes for hydrogen injection in hydrogen storage tanks are processed through a multi-pass hot extrusion process. The innovative use of a rear-drive method to move the continuous tube ensures uniform thrust during hot extrusion, and uniform hot extrusion of the continuous tube ensures the consistency of the microstructure of the weld base material. The consistency of the coiling and extrusion speeds eliminates slippage and dislocations generated during hot rolling, welding and stretching.
[0136] 4. The water cooling method ensures that the pipe is rapidly cooled from the austenitic temperature range to room temperature after hot extrusion, effectively avoiding the generation of low-temperature precipitates, thereby further ensuring that the pipe and weld have good resistance to hydrogen embrittlement.
[0137] In this application, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance; the term "multiple" refers to two or more unless otherwise expressly defined. The terms "install," "connect," "link," and "fix" should be interpreted broadly. For example, "connect" can mean a fixed connection, a detachable connection, or an integral connection; "link" can mean a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.
[0138] In the description of this application, it should be understood that the terms "upper", "lower", "front", "rear", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or module referred to must have a specific orientation or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0139] In the description of this specification, the terms "one embodiment," "some embodiments," "specific embodiment," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0140] The above are merely preferred embodiments of this application and are not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage reservoir, characterized in that, include: Prepare a rolled sheet, wherein the chemical composition of the rolled sheet by mass percentage is: C: ≤0.02%; Si: ≤0.7%; Mn: ≤2.0%; P:≤0.009%; S: ≤0.003%; Cr: 16%-26%; Ni: 10%-30%; N: 0.05%-1.0%; Mo: 1.6%-3.0%, with the remainder being Fe and unavoidable impurities; The coil is longitudinally sheared to obtain multiple steel strips; Multiple steel strips are welded using a first welding method, and the weld is protected by a first inert gas to obtain butt-jointed steel strips. The butt steel strip is milled and then bent into shape by rollers, then welded by a second welding method, and the weld is protected by a second inert gas. The longitudinal seam is welded into a whole tube using a type I break. After welding, the tube blank is subjected to bright solution heat treatment under argon protection in a solution heat treatment unit. The tube blank is coiled and subjected to multiple hot extrusions to obtain a seamless continuous tube. Specifically, the coiling and hot extrusion of the tube blank to obtain a seamless continuous tube includes: conveying the tube blank through rollers adapted to its size at a speed of 15 mm / s or less; subjecting the tube blank to online heat treatment in an online heat treatment furnace at a temperature greater than or equal to 950°C; transferring the heat-treated tube blank to a hot extrusion unit for hot extrusion of tube sections; immediately cooling the tube sections after hot extrusion; coiling the cooled tube blank onto a large coil; and reversing the hot extrusion conveyor for a second hot extrusion to obtain a seamless continuous tube.
2. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 1, characterized in that, The preparation of the rolled plate specifically includes: The raw materials are placed in an electric furnace to complete the melting and rough refining process, and then the rough steel is obtained. The crude steel is transferred into an argon-oxygen decarburization AOD furnace, and an oxygen-argon mixed gas is introduced into the argon-oxygen decarburization AOD furnace. The ratio of oxygen to argon in the mixed gas is adjusted according to the carbon content in the crude steel. Once the carbon content of the crude steel reaches the preset carbon content, the crude steel is subjected to slag removal treatment.
3. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 2, characterized in that, The preparation of the rolled plate also includes: The rough molten steel after slag removal is transferred to the LF furnace in the ladle for refining to obtain refined molten steel. Once the composition and temperature of the refined molten steel reach the preset composition and temperature, the refined molten steel is transported to the continuous casting platform for casting to obtain ingots. After the ingot cools, the oxide scale on the surface of the ingot is mechanically polished.
4. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 3, characterized in that, The process of transferring the rough molten steel after slag removal into the LF furnace for refining to obtain refined molten steel specifically includes: The composition of the crude molten steel after slag removal is adjusted by adding reducing agents and slag-forming materials to obtain refined molten steel.
5. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 3, characterized in that, The preparation of the rolled plate also includes: The polished ingot is placed into a continuous rolling mill for multi-pass hot rolling to obtain an initial coil. The initial coil is then subjected to online solution treatment at 1050℃-1100℃ to obtain a rolled finished plate.
6. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 5, characterized in that, The preparation of the rolled plate also includes: The rolled finished plate is pickled and phosphated, and then coiled to obtain a coil plate.
7. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 4, characterized in that, The reducing agent includes one or a combination of the following: ferrosilicon, chromium silicon, and aluminum.
8. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 4, characterized in that, The slag-forming materials include lime and / or fluorite.
9. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The process of welding multiple steel strips using a first welding method and protecting the weld seam with a first inert gas to obtain butt-jointed steel strips specifically includes: Multiple steel strips are connected by a 40°-50° oblique splice method, and the multiple steel strips are welded by a first welding method; The weld is protected by a first inert gas and the butt weld is subjected to solution heat treatment at 1050℃-1100℃. The weld area was ground and subjected to non-destructive testing to obtain the butt-jointed steel strip.
10. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The first welding method includes one or a combination of the following: laser welding, resistance spot welding, friction stir welding, and plasma filler wire welding.
11. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The first inert gas includes helium and / or argon.
12. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The second welding method includes one or a combination of the following: laser welding, carbon dioxide gas shielded welding, and plasma welding.
13. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The second inert gas includes 100% pure helium; and / or The second inert gas includes argon with a purity of ≥99.7% and nitrogen with a purity of 2%.
14. The method for preparing a seamless continuous tube for hydrogen injection into an underground hydrogen storage facility according to any one of claims 1 to 8, characterized in that, The heat treatment temperature for the bright solution heat treatment is 1050℃-1100℃.
15. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 14, characterized in that, The tube blank undergoes multiple online heat treatments and hot extrusions to obtain a seamless continuous tube for engineering applications, specifically including: The tube blank is subjected to online heat treatment; The tube blank, after online heat treatment, is fed into a hot extrusion unit to hot extrude the tube blank into tube sections; After hot extrusion, the tube section of the tube blank is cooled immediately, and after cooling, the tube blank is coiled onto a large coil. The tube blank is subjected to secondary hot extrusion using a reverse hot extrusion conveyor to obtain a continuous tube with seamless engineering treatment.
16. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 14, characterized in that, The transmission speed is less than or equal to 15 mm / s.
17. The method for preparing a seamless continuous tube for hydrogen injection in an underground hydrogen storage facility according to claim 14, characterized in that, The temperature of the online heat treatment is greater than or equal to 950℃.
18. A seamless continuous pipe for hydrogen injection into an underground hydrogen storage facility, characterized in that... It is prepared using the method for preparing seamless continuous tubes for hydrogen injection in underground hydrogen storage facilities as described in any one of claims 1 to 17.
Citation Information
Patent Citations
Method for smelting very-low carbon and high silicon stainless steel by AOD
CN101338396A
Desulfurization method for smelting two-phase stainless steel
CN102181609A
High-performance seamless continuous pipe and manufacturing method thereof
CN110184542A
Low magnetism steel resisting sea water corrosion
CN1974829A