Pretreatment methods and applications for impurity element analysis of high-purity silicon materials

By employing a pretreatment process involving ultrasound, pyrolysis, grinding and polishing, and acid treatment, the problem of removing EVA adhesive layer and impurities from the surface of waste photovoltaic silicon materials was solved, ensuring the accuracy and sensitivity of DSIMS detection and achieving efficient analysis of impurity elements.

CN119618768BActive Publication Date: 2026-11-17YONGJIANG LAB +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411765827.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-04
Publication Date
2026-11-17
Estimated Expiration
2044-12-04

AI Technical Summary

Technical Problem

Existing technologies cannot effectively remove EVA adhesive layers and impurities from the surface of waste photovoltaic silicon materials, resulting in uneven sample surfaces, which affects the accuracy and sensitivity of DSIMS detection, and may also damage the sample.

Method used

The pretreatment process employs ultrasonication, pyrolysis, polishing, and acid treatment, including ultrasonic pretreatment, pyrolysis treatment, polishing, and acid treatment, to ensure a smooth and glossy sample surface and remove EVA adhesive layer and impurities.

Benefits of technology

This method achieves a smooth and flat sample surface, meeting the requirements of DSIMS detection, improving detection sensitivity and accuracy, and shortening detection time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005168916010000101
    Figure BDA0005168916010000101
  • Figure BDA0005168916010000111
    Figure BDA0005168916010000111
  • Figure HDA0005168916020000011
    Figure HDA0005168916020000011
Patent Text Reader

Abstract

This invention relates to the field of photovoltaic module recycling technology, and particularly to a pretreatment method for impurity element analysis of high-purity silicon materials and its application. The pretreatment method includes the following steps: providing a crude sample; subjecting the crude sample to ultrasonic pretreatment; subjecting the ultrasonically pretreated crude sample to pyrolysis and polishing; subjecting the pyrolysis and polishing crude sample to acid treatment to obtain the sample to be tested; and transferring the sample to be tested to a dynamic secondary ion mass spectrometer for impurity element analysis. The crude sample is a composite layer structure of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass. Through the above series of pretreatment processes, the EVA adhesive layer can be effectively separated without damaging the sample, and the surface smoothness and gloss of the silicon material can be significantly improved, making it well-suited for impurity element analysis using DSIMS.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic module recycling technology, and in particular to a pretreatment method for analyzing impurity elements in high-purity silicon materials and its application. Background Technology

[0002] Photovoltaic silicon materials are exposed to various working environments for extended periods, making them susceptible to performance degradation due to the introduction of impurities. Using DSIMS (Dynamic Secondary Ion Mass Spectrometry) to determine the distribution of impurities in waste photovoltaic silicon materials is crucial for understanding and optimizing device lifespan. DSIMS testing requires samples with a smooth and flat surface; however, waste photovoltaic silicon materials are often treated with coatings and etching processes to improve their photoelectric conversion efficiency or performance, resulting in a non-smooth surface with grid lines. Furthermore, they are often contaminated with various organic substances in the working environment, such as EVA (ethylene-vinyl acetate copolymer) adhesives. Directly introducing these substances into the DSIMS equipment can adversely affect the equipment, prolong testing time, and reduce accuracy. Therefore, appropriate sample pretreatment is necessary to ensure suitability for DSIMS testing. Summary of the Invention

[0003] Existing technologies use lasers, grinding, ultrasonication, and embedding techniques to purify and recycle waste photovoltaic materials. However, these technologies either fail to completely remove the adhesive layer and impurities from the silicon wafer surface or damage the sample, rendering the processed sample unsuitable for DSIMS analysis. This invention employs a series of pretreatment processes—ultrasonication, pyrolysis, polishing, and acid treatment—to effectively separate the EVA adhesive layer without damaging the sample, significantly improving the smoothness and gloss of the silicon surface. This allows the sample to be well-suited for DSIMS impurity element analysis, solving the technical problem that existing pretreatment methods cannot prepare samples that meet DSIMS requirements.

[0004] The first aspect of this invention provides a pretreatment method for impurity element analysis of high-purity silicon materials, the pretreatment method comprising the following steps:

[0005] Provide a crude sample and perform ultrasonic pretreatment on the crude sample;

[0006] The crude sample after ultrasonic pretreatment is subjected to pyrolysis and polishing.

[0007] The crude sample after pyrolysis and polishing is subjected to acid treatment to obtain the sample to be tested;

[0008] The sample to be tested was transferred to a dynamic secondary ion mass spectrometer for impurity element analysis.

[0009] In some preferred embodiments, the crude sample is a composite layer structure of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass.

[0010] The pretreatment method of this invention is for composite layer structures of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass (e.g.) Figure 1 As shown in the image, this material is typically waste photovoltaic silicon. While impurity element analysis of silicon materials can remove the outer glass layer through heat treatment combined with physical removal methods, the EVA layer has extremely high adhesion to the intermediate photovoltaic silicon wafer, making it difficult to completely peel off the EVA layer without damaging the intermediate photovoltaic silicon wafer. DSIMS, as an ion source-based solid-state material elemental analysis device, has extremely high requirements for the sample being tested. This is mainly because the working principle of DSIMS is to use a focused primary ion beam to sputter the sample surface, bombarding it with trace amounts of various particles. A mass analyzer collects the positively or negatively charged secondary ions, and selectively separates the charged secondary ions according to their charge-to-mass ratio, thereby obtaining the secondary ions of the analyte element and matrix element ions. Finally, these are collected and analyzed by a detector to obtain information about the composition and concentration distribution of the analyte element on the sample surface with depth. This process requires the sample surface to be flat and smooth so that the focused ion beam and the sample test micro-area maintain the same incident angle and ion yield during sputtering, minimizing the impact on data accuracy. If the sample surface is uneven or has defects, it will inevitably affect the focusing and sputtering effect of the ion beam, thereby reducing the accuracy and sensitivity of the analysis. Meanwhile, waste photovoltaic silicon materials, due to their rough surface, numerous pores, and large specific surface area, may suffer irreversible damage to DSIMS from the attached EVA adhesive layer and other contaminants. The core technology of this invention lies in using pyrolysis combined with polishing to effectively remove the EVA adhesive layer from the surface of the photovoltaic silicon wafer sample while ensuring its integrity. This also ensures that the sample surface is smooth and its gloss meets the analytical requirements of DSIMS, thereby enabling the detection and analysis of impurity elements in silicon materials.

[0011] In some preferred embodiments, before ultrasonic pretreatment of the crude sample, the initial sample is first split into pieces to obtain an initial sample with the required size; the initial sample is then marked and its surface is cleaned to obtain the crude sample, which is ready for use in the next step.

[0012] More preferably, the size of the crude sample is 5 mm. 2 -100mm 2 The sample holder can be flexibly configured according to its specifications. For example, a 4-well sample holder can be used to cut rough samples into 8mm x 8mm pieces.

[0013] This invention does not impose any particular limitation on the tool used for splitting the fragments, as long as it can achieve the purpose of splitting; for example: fragment splitting pliers.

[0014] In some preferred embodiments, the ultrasonic pretreatment includes: placing the crude sample in an organic solvent for ultrasonic treatment.

[0015] The ultrasonic waves generated by a high-frequency oscillator act on waste photovoltaic silicon materials. Firstly, the cavitation effect of the ultrasound in the organic solvent disrupts the microstructure of the crude sample surface, making it easier for impurities to dissolve and disperse in the solvent. Secondly, the disturbance effect of the ultrasound promotes mixing and dispersion between the organic solvent and the sample, thereby improving impurity removal efficiency. Thirdly, the high acceleration and abrasive action of the ultrasound directly act on the impurity particles, breaking them down and dispersing them in the organic solvent. The synergistic effect of these three aspects further promotes solvent penetration and cleaning of the crude sample surface, further enhancing the impurity removal effect.

[0016] More preferably, the organic solvent includes one or more combinations of acetone, ethanol, isopropanol, chlorinated hydrocarbons, and xylene.

[0017] In some preferred embodiments, the ultrasonic pretreatment includes: placing the crude sample in organic solvent one and organic solvent two in sequence for ultrasonic treatment.

[0018] More preferably, the organic solvent one and organic solvent two are independently selected from acetone or ethanol.

[0019] More preferably, the organic solvent is acetone; before using the organic solvent for ultrasonication, the surface of the crude sample is wiped with a cotton swab soaked in acetone.

[0020] More preferably, the second organic solvent is ethanol; before using the second organic solvent for ultrasonication, the surface of the crude sample is wiped with a cotton swab soaked in ethanol.

[0021] In some preferred embodiments, the pyrolysis treatment includes: taking the crude sample after ultrasonic pretreatment and performing pyrolysis treatment; the temperature of the pyrolysis treatment is 520℃-550℃, and the time of the pyrolysis treatment is 5min-10min.

[0022] By subjecting the crude sample to high-temperature pyrolysis at 520℃-550℃, the EVA film on its surface and other impurities (such as residual materials from the photovoltaic backsheet layer, copper strips, etc.) undergo a series of physical and chemical changes. The EVA film gradually decomposes at high temperatures, its polymer chains break down, thus achieving separation from the silicon material. This invention has found that when the pyrolysis temperature is below 520℃, the EVA layer in the waste photovoltaic silicon material carbonizes under high temperatures, but complete pyrolysis is not achieved; even with extended high-temperature treatment time, the EVA layer remains on the silicon material surface. However, when the pyrolysis temperature is 520-550℃, only 5-10 minutes of pyrolysis is needed for the adhesive layer on the photovoltaic silicon wafer surface to significantly disappear, indicating complete EVA pyrolysis. Metallographic microscopy characterization shows no EVA adhesive layer on the photovoltaic silicon wafer surface; this demonstrates that the pyrolysis conditions ensure complete separation of the EVA adhesive layer from the silicon material, facilitating subsequent sample testing and recycling.

[0023] The temperatures for the pyrolysis treatment can be listed as 520℃, 525℃, 530℃, 535℃, 540℃, 545℃, and 550℃.

[0024] The pyrolysis treatment time can be listed as 5 min, 6 min, 7 min, 8 min, 9 min, and 10 min.

[0025] In some preferred embodiments, the grinding and polishing process includes: sequentially grinding, polishing and buffing the pyrolysis-treated sample rough to obtain a sample rough with a bright surface.

[0026] More preferably, during the smoothing process, the surface of the rough sample is polished using sandpaper of 1000-1600 mesh; examples include 1000 mesh, 1100 mesh, 1200 mesh, 1300 mesh, 1400 mesh, 1500 mesh, and 1600 mesh; the most preferred is 1200 mesh.

[0027] More preferably, during the polishing process, the surface of the rough sample is polished using sandpaper of 2000-2800 mesh; examples include 2000 mesh, 2100 mesh, 2200 mesh, 2300 mesh, 2400 mesh, 2500 mesh, 2600 mesh, 2700 mesh, and 2800 mesh; the most preferred is 2400 mesh.

[0028] More preferably, during the polishing process, a polishing agent and a polishing cloth are used together to polish the surface of the rough sample under the rotation of the polishing machine; the polishing agent includes one or more combinations of adhesive-type polishing agents, metal oxide-type polishing agents, alloy-type polishing agents, and diatomaceous earth-type polishing agents.

[0029] Examples of adhesive-type polishing agents include waxes, greases, paraffin wax, and resins.

[0030] Examples of metal oxides include aluminum oxide or iron oxide.

[0031] Examples of alloy-type polishing agents include stainless steel polishing agents, magnesium alloy polishing agents, and aluminum alloy polishing agents.

[0032] In some preferred embodiments, the polishing agent comprises aluminum oxide; more preferably, the particle size of the polishing agent is 0.5µm-2µm.

[0033] In some preferred embodiments, the polishing machine rotates at a speed of 100 r / min to 200 r / min and the polishing time is 30 min to 60 min.

[0034] Examples of polishing machine speeds include 100 r / min, 110 r / min, 120 r / min, 130 r / min, 140 r / min, 150 r / min, 160 r / min, 170 r / min, 180 r / min, 190 r / min, and 200 r / min.

[0035] When performing polishing, apply polishing agent to the polishing cloth or the surface of the rough sample, fix the polishing cloth on the polishing machine, place the rough sample inside the polishing machine so that its surface is parallel to the rotating plane of the polishing machine, and then start the polishing machine to perform a rotary friction polishing operation.

[0036] Through investigation, this invention has found that although specific pyrolysis treatment effectively removes the EVA adhesive layer adhering to the silicon material surface, the roughness of the sample remains relatively high (e.g., Figure 8 (As shown). High sample surface roughness has two main effects. First, the minute undulations and irregular structures on the sample surface significantly affect the scattering characteristics of the incident ion beam, causing multiple reflections and scatterings of the incident ions on the sample surface, thus reducing the effective excitation depth of the ion beam. Second, highly rough sample surfaces tend to more easily adsorb contaminants and form adsorption layers. These contaminants and adsorption layers hinder the effective collision between incident ions and atoms inside the sample, thereby reducing the generation efficiency of secondary ions. They may also cause the incident ion beam to deflect or diffuse, reducing the generation density of secondary ions and the detection sensitivity. This invention effectively reduces the roughness of the sample surface through sequential grinding, polishing, and finishing operations, improving the sample's smoothness and brightness, and further ensuring that the sample meets the requirements for DSIMS detection.

[0037] In some preferred embodiments, the acid treatment is performed two or more times to obtain a sample suitable for DSIMS testing.

[0038] Preferably, the acid selected for the acid treatment includes one or more combinations of hydrofluoric acid, hydrochloric acid, nitric acid, and sulfuric acid.

[0039] More preferably, the acid treatment includes a pre-treatment and a post-treatment, wherein the acid used in the pre-treatment is hydrofluoric acid and the acid used in the post-treatment is aqua regia (a mixed solution of concentrated hydrochloric acid and concentrated nitric acid).

[0040] Preferably, when using hydrofluoric acid for treatment, the crude sample is immersed in hydrofluoric acid for 30-50 minutes; more preferably, for 40 minutes.

[0041] Preferably, when using aqua regia for treatment, the crude sample is immersed in hydrofluoric acid for 3-5 minutes, more preferably 4 minutes.

[0042] Photovoltaic silicon wafers typically have a series of metal lines on the back to form a grid layer, which helps disperse electrons across the entire cell surface. However, the presence of the grid layer creates fine grooves on the back of the silicon wafer, leading to adsorption and negatively impacting the vacuum level of the DSIMS equipment. Furthermore, the grid layer is often very precisely positioned, and strong mechanical removal methods can easily damage the silicon wafer sample. This invention performs acid treatment on the rough sample after polishing, effectively dissolving and eliminating the oxide layer and corrosion on the silicon wafer surface, making the sample surface closer to its original smooth state. Considering the need to effectively remove impurities from the sample surface without excessively corroding the material surface, this invention preferably employs a two-stage acid treatment: first, immersing the rough sample in hydrofluoric acid, followed by immersing it in aqua regia. This thoroughly removes various residual impurities from the rough sample surface, reducing the impact of impurities on the instrument background values ​​and improving the sensitivity and accuracy of DSIMS detection of impurity elements in silicon materials.

[0043] Preferably, before each acid treatment of the crude sample, the crude sample needs to be thoroughly cleaned to ensure that there is no reagent residue on the surface of the crude sample from the previous step; more preferably, ultrasonic cleaning is performed using ultrapure water.

[0044] This invention requires strict adherence to cleaning procedures. After polishing and before acid treatment, ultrapure water rinsing is performed to prevent residual polishing agent from entering the testing equipment and interfering with the test. After soaking in hydrofluoric acid, ultrapure water rinsing is performed to avoid hydrofluoric acid residue causing uneven corrosion and increasing sample roughness. Finally, rinsing with aqua regia prevents residual acid from corroding the sample holder or damaging the equipment during sample transfer, ensuring the safety of the analysis.

[0045] The second aspect of this invention provides an application of the pretreatment method described above in the field of impurity element analysis and detection of high-purity silicon materials.

[0046] Beneficial effects:

[0047] This invention provides a pretreatment method for impurity element analysis of high-purity silicon materials and its application, which has the following advantages:

[0048] (1) The present invention pre-treats waste photovoltaic silicon materials, especially by means of pyrolysis and polishing, so that the surface of the sample to be tested after treatment is smooth and bright and free of adhesive layer and impurity residue, and can be transferred to DSIMS for impurity element testing.

[0049] (2) The present invention preferably uses a pyrolysis temperature of 520℃-550℃ and a pyrolysis time of 5min-10min to ensure that the EVA adhesive layer in the sample is completely separated from the photovoltaic silicon wafer.

[0050] (3) The present invention performs specific grinding, polishing and polishing operations on the crude sample after pyrolysis to ensure that the surface of the silicon material is smooth and flat, so as to improve the sensitivity of DSIMS test and analysis, further shorten the detection time and improve the detection efficiency.

[0051] (4) The present invention performs acid treatment on the rough sample after grinding and polishing to further reduce the roughness of the sample and avoid the negative impact of adsorption caused by the presence of the grid line layer on the back of the photovoltaic silicon wafer on the vacuum degree of DSIMS.

[0052] (5) This method is simple and easy to operate; after pretreatment, the sample can reach the detection limit in about 70 seconds when it is put into DSIMS, and the accuracy and sensitivity of the detection results are significantly improved. Attached Figure Description

[0053] Figure 1 Photos of raw waste photovoltaic silicon material (a is a macroscopic image of the sample, b is a magnified version of the macroscopic image, c is a cross-sectional image of the sample, d is a magnified version of the cross-sectional image of the sample; where 1 is glass, 2 is EVA adhesive layer, and 3 is photovoltaic silicon wafer);

[0054] Figure 2 Initial sample photographs and cross-sectional views (a and b are images of the front of the sample from different positions after the glass bonded to the surface has been peeled off; c is an enlarged version of b; d is a cross-sectional view of the sample);

[0055] Figure 3 Raman spectra of the initial sample;

[0056] Figure 4 Macroscopic morphology of samples R18 and R19 after pyrolysis (left: R18, right: R19);

[0057] Figure 5Microscopic morphology images of samples R18 and R20 after pyrolysis (from left to right: front view at 520℃-5min, front view at 200x magnification, 540℃-5min, front view at 200x magnification, 550℃-5min, front view at 200x magnification);

[0058] Figure 6 Raman spectra of samples R18 and R20 after pyrolysis (A: R18, B: R19);

[0059] Figure 7 Example 1: Microscopic images of samples before and after polishing (left: before polishing, right: after polishing)

[0060] Figure 8 Images of the original photovoltaic material sample, the sample after hydrofluoric acid treatment, and the sample after aqua regia treatment (left: original photovoltaic material sample; middle: sample after hydrofluoric acid treatment; right: sample after aqua regia treatment).

[0061] Figure 9 Images of the original photovoltaic material sample, the sample after hydrofluoric acid treatment, and the sample after aqua regia treatment (a in the image is the front of the original photovoltaic material sample, b is the back of the original photovoltaic material sample; c is the front of the sample after hydrofluoric acid treatment, d is the back of the sample after hydrofluoric acid treatment; e is the front of the sample after aqua regia treatment, and f is the back of the sample after aqua regia treatment). Figure 10 Detailed images of changes in the grid layer of the sample before and after hydrofluoric acid treatment (a: before hydrofluoric acid treatment, 50x magnification; b: before hydrofluoric acid treatment, 200x magnification; c: after hydrofluoric acid treatment, 50x magnification; b: after hydrofluoric acid treatment, 200x magnification).

[0062] Figure 11 . Sample morphology changes during pretreatment in Example 1 (a. Initial sample, b. Sample after pyrolysis treatment, c. Sample after one cleaning; d. Test surface of sample after pretreatment; e. Back side of sample after pretreatment);

[0063] Figure 12 Initial sample test results;

[0064] Figure 13 Example 1: Test results of the pretreated sample. Detailed Implementation

[0065] This invention processes waste photovoltaic silicon materials through a pretreatment process involving ultrasound, pyrolysis, grinding and polishing, and acid treatment. This process effectively removes impurities and yields a smooth, flat, and clean sample for testing, ensuring that the photovoltaic silicon wafer sample is not damaged. This allows the sample to be analyzed for impurity elements using a dynamic secondary ion mass spectrometer, which offers high sensitivity and accuracy, and can obtain accurate DSIMS test results in a short time.

[0066] Example

[0067] This embodiment provides a pretreatment method for impurity element analysis of high-purity silicon materials, including the following steps:

[0068] Step (1) Provide a crude sample;

[0069] Step (2) involves ultrasonic pretreatment of the crude sample;

[0070] Step (3) involves pyrolyzing the pre-treated crude sample.

[0071] Step (4) The crude sample after pyrolysis is subjected to grinding and polishing treatment;

[0072] Step (5) The crude sample after pyrolysis and polishing is subjected to acid treatment to obtain the sample to be tested.

[0073] The sample to be tested was transferred to a dynamic secondary ion mass spectrometer for impurity element analysis.

[0074] Step (1) includes:

[0075] 1.1 Splitting: The initial sample was scribed with a diamond scribing pen and then split into pieces with splitting pliers to prepare an initial sample with a size of 8mm × 8mm;

[0076] 1.2 Marking: Use a diamond scribing pen to mark the back of the initial sample obtained from the cleavage, and then use a lint-free cotton swab dipped in ethanol to wipe the front and back surfaces of the initial sample to remove the silicon powder residue left by the scribing on the surface of the initial sample for the next step.

[0077] The initial sample is waste photovoltaic silicon material, specifically a composite layer structure of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass.

[0078] Step (2) includes: wiping the front and back surfaces of the initial sample prepared in step (1) three times with a cotton swab dipped in acetone, and then sonicating the initial sample in acetone (sonication time is 5 min); then taking out the initial sample, wiping the front and back surfaces of the initial sample three times with a cotton swab dipped in ethanol, and then sonicating the initial sample in ethanol (sonication time is 5 min), and then letting it air dry naturally for use in the next step.

[0079] Step (3) includes: placing the crude sample obtained after ultrasonic treatment in step (2) on a heating table lined with aluminum foil for pyrolysis treatment at a temperature of 550°C for 15 minutes. After pyrolysis, the crude sample is removed and allowed to cool naturally to room temperature on a clean surface for use in the next step.

[0080] The step (4) includes: taking the crude sample obtained after the pyrolysis treatment in step (3), first using 1200-grit sandpaper to smooth its surface, then using 2400-grit sandpaper to polish it, and finally using a polishing cloth and polishing agent to polish it. The polishing agent is 1µm aluminum oxide, the polishing speed is set to 150r / min, and the polishing time is 45min.

[0081] The sandpaper is made of silicon carbide.

[0082] The polishing process is performed using a mechanical polishing machine.

[0083] The acid treatment in step (5) is performed twice to obtain a sample suitable for DSIMS detection; the specific steps include:

[0084] 501 First cleaning: Place the crude sample obtained in step (4) in ultrapure water and sonicate it 3 times (sonicate for 5 minutes each time, and replace the ultrapure water before each sonication); then place the crude sample in ethanol and sonicate it for 5 minutes, then rinse the crude sample with ultrapure water, then put the rinsed sample into ultrapure water and sonicate it once, and take it out for use.

[0085] 502 Pre-acid treatment: Immerse the crude sample after the first cleaning in concentrated hydrofluoric acid (40% by mass) for 40 minutes;

[0086] 503 Secondary cleaning: Immerse the crude sample after the previous acid treatment in ultrapure water for 1 minute, and then rinse the crude sample with ultrapure water; then sonicate the rinsed crude sample in ultrapure water 3 times (5 minutes each time, and replace with fresh ultrapure water before each sonication).

[0087] 504 post-acid treatment: The crude sample after the second cleaning was immersed in aqua regia for 4 minutes; aqua regia is a mixed solution of concentrated hydrochloric acid (mass concentration of 36%) and concentrated nitric acid (mass concentration of 68%) with a volume ratio of 3:1.

[0088] 505 Three-stage cleaning: After the second acid treatment, the crude sample is immersed in ultrapure water for 1 minute, then rinsed with ultrapure water. After rinsing, the crude sample is sonicated three times in ultrapure water (5 minutes each time, with fresh ultrapure water before each sonication). Subsequently, the crude sample is sonicated in ethanol. After sonication, the front and back surfaces of the crude sample are wiped three times with a cotton swab soaked in ethanol, and then air-dried naturally.

[0089] Note: The reagents, tools, and conditions used in this example are described below:

[0090] The ethanol used was an analytical grade product with a concentration of ≥95.0%.

[0091] The acetone used was an analytical grade product with a concentration of ≥99.9%.

[0092] The resistivity of the ultrapure water used should be ≥18MΩ*cm, and the ultrapure water should be used to rinse more than 5 times during the second and third cleaning to ensure no residue remains; and the waste liquid after the first three rinsings should be poured into the acidic waste liquid tank.

[0093] The cotton swabs used were dust-free cotton swabs.

[0094] The sampling fixture used in the pretreatment process is a high-temperature resistant and clean fixture to ensure that the fixture is preheated and melted during the transfer of crude sample, thus preventing contamination of the crude sample.

[0095] The ultrasonic frequency involved in the ultrasonic operation was 40 kHz.

[0096] Unless otherwise specified, the solvent of the solution in this invention is water.

[0097] Performance testing

[0098] 1. Photos of the original and initial samples

[0099] The original sample of waste photovoltaic silicon material was observed using a 3D optical microscope, see... Figure 1 . Figure 1 In the image, a is a macroscopic image of the sample, b is a magnified version of the macroscopic image, c is a cross-sectional image of the sample, and d is a magnified version of the cross-sectional image of the sample. From... Figure 1 As can be seen from the data, the waste photovoltaic silicon material has a composite layer structure of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass.

[0100] The original sample was heated to 150-200℃, and then the glass was removed with tweezers to obtain the initial sample; photographs and cross-sectional views of the initial sample are shown below. Figure 2 The Raman spectrum of the initial sample is shown below. Figure 3 The Raman spectrum clearly shows characteristic peaks of the EVA adhesive layer in the initial sample (e.g., 2600-3000 cm⁻¹). -1 (The location) proves that the initial sample contains an EVA adhesive layer.

[0101] 2. Observation of pyrolysis effect

[0102] The pyrolysis effects of samples under different pyrolysis conditions were compared. The experimental conditions and observation results are recorded in Table 1; photographs of samples R18 and R20 after pyrolysis are shown below. Figure 4 The observation results show that the samples underwent significant pyrolysis after being treated at 520℃ and 550℃ for 5 minutes.

[0103] Samples R18 and R20 were further characterized by metallographic microscopy. Microscopic images at 200x magnification are shown below. Figure 5 .from Figure 5 It can be seen that there is no EVA adhesive layer on the sample surface, proving that the adhesive layer has been completely pyrolyzed.

[0104] Samples R18 and R19 were further characterized by Raman spectra, and the results are shown in [the table below]. Figure 6 .

[0105] Table 1

[0106]

[0107]

[0108] Through Table 1 and Figure 4-6 The experimental results show that waste photovoltaic silicon samples cannot be completely pyrolyzed below 500℃, but the EVA adhesive layer can be effectively removed by pyrolysis for 5 minutes at 520-550℃. However, carbon impurities still remain on the sample surface after removal, and the surface is still relatively rough, making it impossible to perform DSIMS testing. Therefore, further processing is still required.

[0109] 3. Observation of polishing effect

[0110] Metallurgical microscopy was used to observe the samples before and after polishing in Example 1. Microscopic characterization images at 200x magnification are shown below. Figure 7 .from Figure 7 It can be seen that the surface roughness of the sample is significantly reduced after grinding and polishing, making it suitable for DSIMS testing.

[0111] 4. Changes in the back-side grid layer of the sample after acid treatment

[0112] Compare the sample results before and after acid treatment, see... Figure 8-10 .from Figure 10 The results show that hydrofluoric acid treatment significantly reduces the roughness of the sample's back surface, minimizes adsorption caused by the presence of the grid layer on the material surface, avoids negative impacts on the vacuum level of the equipment, and helps protect the detection equipment. During the experiment, hydrochloric acid was also used instead of hydrofluoric acid for treatment; after treatment, the grid layer of the sample showed virtually no reaction.

[0113] 5. Sample surface morphology

[0114] like Figure 11 The image shows the surface morphology of the sample when the pretreatment method of this embodiment is used to process waste photovoltaic silicon material. Figure 11 a is the initial sample, which shows that there is a grid line layer on the surface of the waste photovoltaic silicon material, as well as residual adhesive and impurities. Figure 11b is the sample to be tested after pyrolysis treatment. At this time, the adhesive residue on the surface of the silicon material has been removed, but it can be seen that there are still impurities on its surface. Figure 11 c is the sample to be tested after one cleaning. At this time, the sample to be tested has undergone polishing treatment, and the impurities on the material surface have been removed, and the surface is bright and clean. Figure 11 d、 Figure 11 e represents the test surface and the back surface of the sample after pretreatment, respectively. It can be seen that after the pretreatment in this embodiment, the grid line layer, residual adhesive and other impurities on the test surface of the sample have been removed, and the grid line layer on the back surface of the test surface of the sample has also been removed. The test sample has achieved a significant cleaning and brightening effect.

[0115] 6. DSIMS On-Machine Test Results

[0116] The initial sample after binder removal and the pretreated sample were subjected to DSIMS analysis to determine the bulk concentration of element B. The test results are shown in [Figure number missing]. Figure 12 , 13 .

[0117] Note: Since silicon materials containing binders cannot be tested on the machine, the initial sample (with rough surface) after removing the binder is used as a control during the machine test.

[0118] from Figure 12 , 13 As can be seen, the initial sample after removing the adhesive only reached the detection limit after 4000 seconds of instrument testing, which was time-consuming, inefficient, and the accuracy of the results could not be guaranteed. However, the sample pretreated according to this invention reached the detection limit in about 70 seconds after testing, allowing for rapid testing and improving both efficiency and accuracy.

Claims

1. A pretreatment method for analyzing impurity elements of high-purity silicon material, characterized by comprising the steps of: The preprocessing method includes the following steps: ​ Provide a crude sample and perform ultrasonic pretreatment on the crude sample; The crude sample after ultrasonic pretreatment is subjected to pyrolysis and polishing. The crude sample after pyrolysis and polishing is subjected to acid treatment to obtain the sample to be tested; The sample to be tested was transferred to a dynamic secondary ion mass spectrometer for impurity element analysis. The crude sample is a composite layer structure consisting of glass-EVA adhesive layer-photovoltaic silicon wafer-EVA adhesive layer-glass. The pyrolysis treatment temperature is 520℃-550℃, and the pyrolysis treatment time is 5min-10min; The acid treatment includes a pre-treatment and a post-treatment. The acid used in the pre-treatment is hydrofluoric acid, and the acid used in the post-treatment is aqua regia. The impurity element is B; When treating with hydrofluoric acid, the crude sample is immersed in hydrofluoric acid for 30-50 minutes; when treating with aqua regia, the crude sample is immersed in hydrofluoric acid for 3-5 minutes. The polishing process includes: taking the crude sample obtained after pyrolysis treatment, first using 1200-grit sandpaper to smooth its surface, then using 2400-grit sandpaper to polish it, and finally using a polishing cloth and polishing agent in combination for polishing. The polishing agent is 1µm alumina, the polishing speed is set to 150r / min, and the polishing time is 45min.

2. The pretreatment method for analysis of impurity elements of high-purity silicon material according to claim 1, characterized by, The ultrasonic pretreatment includes: placing the crude sample in an organic solvent for ultrasonic treatment; the organic solvent includes acetone and / or ethanol.

3. The application of the pretreatment method according to claim 1 or 2 in the field of impurity element analysis and detection of high-purity silicon materials.

Citation Information

Patent Citations

  • Method for detecting content of impurity elements in cobalt

    CN113049671A

  • Separation and recovery method for silicon wafers in waste photovoltaic module

    CN115770780A

  • Photovoltaic module recovery method and device

    CN117046864A