Metal foil for electrode foil production, method for producing electrode foil for electrolytic capacitor, electrode foil for electrolytic capacitor, and electrolytic capacitor

By etching the multiple recesses in the main surface opening of the electrode foil, the porous part is formed, which solves the problem of foil breakage and insufficient fold resistance strength during the winding process of the electrode foil, and achieves higher fold resistance strength and lower risk of foil breakage.

CN119631153APending Publication Date: 2025-03-14PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380055926.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-29
Filing Date
2023-07-27
Publication Date
2025-03-14

AI Technical Summary

Technical Problem

The existing electrode foil is prone to foil breakage during winding, and the fold resistance strength is insufficient, making it difficult to effectively suppress foil breakage.

Method used

A metal foil containing a valve-acting metal is used, and a plurality of recesses with a main surface opening and dispersed in a dot-like shape. The opening diameter of the recess is 2 μm or more. The porous portion is formed by etching and the opening diameter of the fine pores is less than 2 μm.

Benefits of technology

The foil breakage of the electrode foil for electrolytic capacitors during the winding process is significantly suppressed, and the fold resistance strength of the electrode foil is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119631153A_ABST
    Figure CN119631153A_ABST
Patent Text Reader

Abstract

This method for manufacturing an electrode foil for an electrolytic capacitor comprises: a step for preparing a raw material foil; and a step in which the raw material foil is etched. The raw material foil contains a valve action metal, and has a plurality of recesses that are open in the main surface thereof and are arranged so as to be dispersed in dots in the direction of the main surface thereof. The opening diameter of the recess is 2 [mu] m or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a metal foil for producing an electrode foil, a method for producing an electrode foil for an electrolytic capacitor, an electrode foil for an electrolytic capacitor, and an electrolytic capacitor. Background Art

[0002] As the electrode foil of the electrolytic capacitor, a metal foil (etched foil) having a porous portion formed on the surface by etching is used. This makes the electrode foil have a large surface area, and the capacity of the electrolytic capacitor is improved.

[0003] Patent document 1 discloses: "An electrode foil, characterized in that it is formed by a strip-shaped foil and comprises: an expanded portion formed on the surface of the aforementioned foil, a core portion which is the remainder of the aforementioned foil excluding the aforementioned expanded portion, and a plurality of dividing portions extending along the width direction of the strip on the aforementioned expanded portion and dividing the aforementioned expanded portion, wherein the aforementioned dividing portions have a groove width of 50 μm or less, including 0, when the aforementioned foil is in a flat state."

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-224844 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] In Patent Document 1, by providing a split portion, the indentation depth (Erickson value) in the Erickson test is increased. However, the split portion extends in the width direction of the electrode foil, and the folding strength in the width direction of the electrode foil is low. Due to the stress generated when the electrode foil is wound, cracks are formed in the width direction of the electrode foil along the split portion, and cracks extending linearly from one end to the other end in the width direction of the electrode foil are generated. As a result, foil breakage is likely to occur. The suppression of foil breakage when winding the electrode foil is still insufficient.

[0009] Solutions for solving problems

[0010] One scheme of the present disclosure relates to a metal foil for manufacturing an electrode foil, which is a metal foil used in the manufacture of an electrode foil for an electrolytic capacitor. The metal foil contains a valve-acting metal and has a plurality of recesses that are open on a main surface of the metal foil and are dispersed in a dotted manner in the direction of the main surface, and the opening diameter of the recesses is greater than 2 μm.

[0011] Another aspect of the present disclosure relates to a method for producing an electrode foil for an electrolytic capacitor, the method comprising: preparing the metal foil for producing the electrode foil; and etching the metal foil.

[0012] Still another aspect of the present disclosure relates to an electrode foil for an electrolytic capacitor obtained by the above-mentioned method for producing an electrode foil for an electrolytic capacitor.

[0013] Still another scheme of the present disclosure relates to an electrode foil for an electrolytic capacitor, which contains a metal foil containing a valve-acting metal, wherein the metal foil has a plurality of recesses that are open on the main surface of the metal foil and are arranged in a dot-like manner in the direction of the main surface, and the metal foil includes a porous portion, wherein the porous portion has pores that are open on the main surface of the metal foil and on the inner wall surfaces of the plurality of recesses, wherein the opening diameter of the recess is greater than 2 μm, and the opening diameter of the pores of the porous portion is less than 2 μm.

[0014] Still another aspect of the present disclosure relates to an electrolytic capacitor including the above-mentioned electrode foil for an electrolytic capacitor.

[0015] Effects of the Invention

[0016] According to the present disclosure, it is possible to suppress foil breakage when winding an electrode foil for an electrolytic capacitor.

[0017] The novel features of the present invention are described in the appended claims, but the present invention, both about the configuration and content, together with other objects and features of the present invention, should be further fully understood from the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a main part front view schematically showing an example of the electrode foil for electrolytic capacitor according to one embodiment of the present disclosure.

[0019] Figure 2 This is a front view schematically showing a main part of another example of the electrode foil for an electrolytic capacitor according to an embodiment of the present disclosure.

[0020] Figure 3 for Figure 2 III-III sectional view.

[0021] Figure 4 This is a diagram schematically showing an example of a wound body viewed from the end surface side.

[0022] Figure 5 It is a cross-sectional view schematically showing an electrolytic capacitor according to an embodiment of the present disclosure.

[0023] Figure 6 It is a perspective view schematically showing the structure of a wound body.

[0024] Figure 7 This is a SEM image showing a state after winding of the electrode foil for electrolytic capacitor according to one embodiment of the present disclosure.

[0025] Figure 8 This is a SEM image showing a main part of an electrode foil for an electrolytic capacitor according to an embodiment of the present disclosure.

[0026] Fig. 9 The SEM image shows the main part of the electrode foil when the recessed portion group is provided after etching the metal foil. Fig. 9 (a) shows the case where the depth of the concave portion is small. Fig. 9 (b) shows a case where the depth of the recess is large.

[0027] Fig.10 Specific examples of the shape of the opening of the recess are shown. Fig.10 (a)~ Fig.10 (c) shows the cases where the opening shapes of the recessed portion are circular, quadrilateral, and hexagonal, respectively. Fig.10 (d) shows a case where the opening shape of the recessed portion is a quadrilateral with all corners having arcs. Fig.10 (e)~ Fig.10 (g) shows the case where the opening shape of the recessed portion is a teardrop shape. Fig.10 (h) shows a case where the opening shape of the recess is a hexagonal star. DETAILED DESCRIPTION

[0028] Hereinafter, examples are given to illustrate the embodiments of the present disclosure, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials are sometimes exemplified, but other numerical values ​​and materials may also be applied as long as the effects of the present disclosure are obtained. In this specification, the so-called "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read interchangeably as "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values ​​related to specific physical properties, conditions, etc. are exemplified, as long as the lower limit does not become above the upper limit, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be combined and used.

[0029] The present disclosure includes a combination of matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the attached claims. That is, matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the attached claims may be combined as long as no technical contradiction occurs.

[0030] The method for producing an electrode foil for an electrolytic capacitor according to an embodiment of the present disclosure includes a first step and a second step.

[0031] In the first step, the metal foil for producing the electrode foil according to the embodiment of the present disclosure is prepared as the metal foil used for producing the electrode foil for an electrolytic capacitor (hereinafter also referred to as “raw material foil”).

[0032] The metal foil used for manufacturing the electrode foil of the embodiment of the present disclosure contains a valve-acting metal and has a plurality of recesses opening on its main surface. The plurality of recesses are arranged in a point-dispersed manner in the direction of the main surface of the metal foil (when the metal foil is observed from the normal direction of its main surface). That is, the plurality of recesses are arranged away from each other. The plurality of recesses each have an opening diameter of more than 2 μm (hereinafter also referred to as "opening diameter D"). The point-dispersed arrangement of the recesses may be uniform, uneven, regular, or irregular.

[0033] It should be noted that the opening diameter of the recess refers to the maximum diameter of the opening of the recess. Hereinafter, a plurality of recesses with an opening diameter of 2 μm or more, which are open on the main surface of the metal foil and are arranged in a dotted manner in the direction of the main surface, are also referred to as a "recess group". The recess group may be provided on one main surface of the metal foil or on both main surfaces of the metal foil.

[0034] In the second step, the metal foil is etched to form a porous portion on the surface of the metal foil. The above-mentioned production method may further include a third step of forming a dielectric layer on the surface of the etched metal foil by chemical conversion treatment or the like.

[0035] The electrode foil for electrolytic capacitors of the embodiment of the present disclosure is obtained by the above-mentioned manufacturing method. That is, it is obtained by etching the above-mentioned metal foil (further chemical conversion treatment, etc. as needed). Hereinafter, the metal foil formed with a porous portion by etching treatment is also referred to as "etched foil". The metal foil that is further chemically converted after etching treatment is also referred to as "chemical conversion foil".

[0036] The etched foil obtained by the above-mentioned manufacturing method contains a metal foil containing a valve-acting metal, and the metal foil has a plurality of recesses that are open on the main surface of the metal foil and are dispersed and arranged in a point-like manner in the direction of the main surface. The etched foil includes a porous portion, and the porous portion has pores that are open on the main surface of the metal foil and the inner wall surface of the plurality of recesses. The opening diameter of the recess is greater than 2 μm, and the opening diameter of the pores of the porous portion is less than 2 μm. It should be noted that the opening diameter of the pores of the porous portion refers to the maximum diameter of the opening of the pores. The opening diameter of the recess is greater than the opening diameter of the pores of the porous portion. The chemical conversion foil also has: a dielectric layer covering the metal skeleton constituting the above-mentioned porous portion.

[0037] In a metal foil having a recess group, the folding strength is improved. Due to the presence of the recess group, high-quality cracks can be formed between the recesses when the metal foil is wound, and the stress generated by the winding is relieved, thereby suppressing the breakage of the foil. By designing the recess group to form high-quality cracks, the generation of large cracks extending in a straight line from one end of the foil in the width direction to the other end, which is the cause of the foil breakage, is suppressed. In particular, in the case of etching foil and chemical conversion foil, the foil breakage during winding is prone to occur, so the effect of suppressing the foil breakage based on the formation of the recess group can be significantly obtained. In addition, in a chemical conversion foil with a large chemical conversion voltage, the stress relaxation effect based on the formation of the recess group can be significantly obtained. It should be noted that the winding of the metal foil is carried out, for example, by winding the metal foil (raw material foil, etching foil, chemical conversion foil) based on a roller, cutting the electrode foil, and forming a winding body containing the electrode foil.

[0038] The above-mentioned high-quality cracks are formed in a manner extending from the inner wall of the recess when viewed from the main surface side of the metal foil, and are formed in a manner that the cracks extending from the recesses are connected to each other. The length and shape of the cracks, the direction in which the cracks extend, etc. can be controlled by the recess group. According to the arrangement of the recess group, cracks can be formed in a slightly curved manner between the recesses on the main surface of the metal foil.

[0039] Here, Figure 7 This is a SEM image showing a wound state of the electrode foil for electrolytic capacitor according to one embodiment of the present disclosure, and shows a part of the surface of the electrode foil. Figure 7 The longitudinal direction of the SEM image is the length direction (winding direction) of the strip-shaped electrode foil, and is also the rolling direction of the electrode foil. Figure 7 The recessed portion group is configured in a sawtooth shape, Figure 2 The recessed portion group shown in the figure shows that L1 is larger than L3, L1 and L2 are almost the same size, and L3 is the interval L. Figure 7 As shown, by winding the electrode foil, high-quality cracks can be formed between the recessed portions in a direction perpendicular to the winding direction (rolling direction).

[0040] During the manufacturing process of electrolytic capacitors, metal foil (sheet) contacts with treatment liquid (e.g., etching solution, chemical conversion solution) and rollers, which may produce bumps (or scratches). When winding the electrode foil, stress concentrates on the bumps, and sometimes the foil breaks when winding the electrode foil. In addition, rolled foil (Al raw foil) is usually used as the raw foil, which has rolling marks generated during its manufacturing process. Due to the influence of the rolling marks, etching pits are unevenly formed, the folding strength is locally reduced, and sometimes the foil breaks when winding the electrode foil. In contrast, in the electrode foil with a recessed portion group, the above-mentioned foil breakage can be suppressed.

[0041] In addition, when using an electrolytic capacitor with a wound body, the foil may break due to vibration. In contrast, the electrode foil with a recessed portion group can also suppress the foil breakage caused by vibration when using the electrolytic capacitor, and can be suitably used for electrolytic capacitors for vehicles and the like that require high reliability against vibration.

[0042] In addition, in the above-mentioned manufacturing method, the metal foil (raw foil) having the recessed portion group is etched. In this case, a porous portion having pores (etching pits) opening on the main surface of the metal foil and the inner wall surface of the recessed portion is formed. As a result, the surface area of ​​the metal foil is increased, and the capacity can be increased.

[0043] When a metal foil is etched and then a recess group is set on the etched foil, the pores (etching pits) located near the inner wall surface of the recess are easily blocked when the recess group is formed, and the pores opening on the inner wall surface of the recess are not easily formed, and the surface area of ​​the metal foil is reduced accordingly. In the case of forming a recess by pressing a fixture with a protrusion on the metal foil, the etching pit is blocked due to the deformation of the porous part caused by the pressing. In the case of forming a recess by laser processing, the etching pit is blocked due to the melting of the laser irradiated part. In the case of forming a recess with a large depth (for example, a recess with a depth H of more than 5μm), the energy irradiated during processing (or the pressure during pressing) is large, and the etching pit is easily blocked due to melting (deformation). When the influence of the occlusion of the etching pit caused by melting (deformation) is large, the capacity is sometimes reduced and the strength is also reduced. The above-mentioned occlusion includes not only the case where the etching pit is completely blocked, but also the case where the etching pit is partially blocked.

[0044] In contrast, in the manufacturing method of this embodiment, the etching process of the second step is performed after the recessed portion group is formed, so that the reduction in capacity and strength caused by the melting (deformation) of the porous portion when the recessed portion group is formed can be avoided. When the recessed portion with a depth H of 20 μm or more is formed, the improvement effect of strength and capacity based on the manufacturing method of this embodiment can be significantly obtained.

[0045] Here, Figure 8 FIG. 1 is a SEM image showing a main part of the electrode foil produced by the above-mentioned production method.

[0046] like Figure 8 As shown, the electrode foil has a mortar-shaped recess 1 opened on the main surface S. The electrode foil is an etched foil, and a porous portion 2 is formed on the main surface S and the inner wall surface of the recess 1. The porous portion 2 has pores opened on the main surface S and pores opened on the inner wall surface of the recess 1.

[0047] Here, Fig. 9 The SEM image shows the main part of the electrode foil when the recessed portion group is provided after etching the metal foil. Fig. 9(a) shows the case where the depth of the concave portion is as small as 5 μm. Fig. 9 (b) shows the case where the depth of the recess is as large as 45 μm. In any case, the recess is formed by laser processing, and the etching pit is observed to be blocked due to the melting of the inner wall surface of the recess accompanying the laser irradiation. Fig. 9 The greater the effect of laser processing on the electrode foil of (b), the greater the degree of occlusion of the etching pits.

[0048] (First process)

[0049] (Metal foil having recessed portions)

[0050] The metal foil prepared in the first step (metal foil used in the step of forming the recessed portion group described later) does not have a porous portion formed by etching, a dielectric layer formed by chemical conversion treatment or the like, and a cover layer described later formed in the case of a cathode foil.

[0051] The metal foil prepared in the first step contains a valve metal. The valve metal includes, for example, aluminum (Al), tantalum (Ta), niobium (Nb), titanium (Ti), zirconium (Zr), etc. The metal foil may contain the valve metal as an alloy or compound containing the valve metal.

[0052] When the metal foil contains aluminum (Al) as a valve metal, the Al content in the metal foil may be 98% by mass or more, or 99% by mass or more (or 99.5% by mass or more). From the viewpoint of increasing the capacity of the electrode foil, the metal foil is preferably a soft foil (Al content: 98% by mass or more). Among them, from the viewpoint of increasing the capacity, the Al content in the metal foil is preferably 99.8% by mass or more.

[0053] The metal foil may also contain trace amounts of other elements other than the valve action metal. As other elements, silicon (Si), copper (Cu), iron (Fe) and the like can be listed. The Si content in the metal foil is, for example, preferably 1 mass ppm or more and 100 mass ppm or less, and more preferably 5 mass ppm or more and 80 mass ppm or less. The Cu content in the metal foil is, for example, preferably 5 mass ppm or more and 100 mass ppm or less, and more preferably 5 mass ppm or more and 80 mass ppm or less. The Fe content in the metal foil is, for example, preferably 5 mass ppm or more and 200 mass ppm or less, and more preferably 5 mass ppm or more and 100 mass ppm or less. In the metal foil, the total content of Si, Cu and Fe is preferably 0.1 mass % or less, and more preferably 0.05 mass % or less.

[0054] The tensile strength of the metal foil having the recessed portion group is preferably 25 N / mm 2 More than 40N / mm 2More than, more preferably 60N / mm 2 In addition, the tensile strength can be, for example, 120 N / mm 2 The elongation of the metal foil having the recessed portion group is preferably 1% to 16%, and more preferably 2% to 14%.

[0055] The metal foil having the recessed portion group has a tensile strength of 25 N / mm 2 Above (or 40N / mm 2 In the case of a thickness of 0.1% or more (or an elongation of 1% or more (or an elongation of 2%) or more (or an elongation of 1% or more (or an elongation of 2%) or more (or an elongation of 2%) or more (or an elongation of 1%) or more (or an elongation of 2%) or more (or an elongation of 2%) or more (or an elongation of 1%) or more (or an elongation of 2%) or more (or an elongation of 2%) or more (or an elongation of 2%) or more (or an elongation of 3%) or more (or an elongation of 1%) or more (or an elongation of 2%) or more (or an elongation of 3 ...

[0056] Rolled foil is usually used as metal foil, and tensile strength and elongation refer to the tensile strength and elongation in the rolling direction, respectively. The rolling direction of the strip-shaped metal foil is usually substantially consistent with the length direction of the metal foil. The tensile strength and elongation of the metal foil are obtained, for example, according to JIS Z 2241 (tensile test of metal materials).

[0057] In the depth direction of the recess, the number N of crystal grains of the metal foil exposed on the inner wall surface of the recess is preferably 2 or more (or 3 or more), and can be 2 or more (or 3 or more) and 10 or less. In this case, it is easy to ensure the strength (tensile strength, folding strength) of the metal foil (etched foil, chemical conversion foil). For more than 40% (or more than 60%) of the plurality of recesses constituting the recess group, the number N is preferably within the above range.

[0058] The number N of crystal grains mentioned above can also be said to be the number of crystal grains exposed on the side wall surface of the recess (the inner wall surface from the deepest part of the recess to the opening). The number N of crystal grains mentioned above is calculated using the following method. Using a scanning electron microscope (SEM), a cross-sectional SEM image of the thickness direction of the metal foil is obtained. At this time, the contours of the side wall surfaces of two recesses are observed for one recess. The two contours are set as C1 and C2 (for example, Figure 3 C1 and C2 in the figure correspond to two contours of the side wall surface provided in the concave portion of the raw foil. ). The number N1 of grain boundaries extending from the contour C1 of one side wall surface to the inside of the metal foil is counted. The number N2 of grain boundaries extending from the contour C2 of the remaining side wall surface to the inside of the metal foil is counted. The average value of (N1+1) and (N2+1) is obtained as the number N of the above-mentioned crystal grains.

[0059] The average grain diameter of the metal foil is preferably greater than 18 μm (or greater than 20 μm) and less than 60 μm. In this case, the metal foil (electrode foil) has a moderate hardness and is easy to fully ensure strength. Damage to the metal foil (electrode foil) is suppressed during cutting, winding, and connection of the electrode foil to the lead member of the metal foil. When the average grain diameter is greater than 18 μm, grain boundaries exist moderately. When there are many grain boundaries, the distribution of pits near the grain boundaries in the porous portion and other parts can be suppressed from becoming uneven, resulting in reduced capacity.

[0060] The average grain diameter is obtained by arbitrarily selecting a region with a length of 2×F in the plane direction in a cross-sectional SEM image of a metal foil (electrode foil) with a thickness of F, measuring the maximum diameters of multiple crystals contained in the region, and calculating the average values.

[0061] The thickness F of the metal foil (electrode foil) can be 50 μm or more and 200 μm or less, or 80 μm or more (or 100 μm or more) and 200 μm or less. When the thickness F of the metal foil is 80 μm or more (or 100 μm or more), the stress generated during winding is large, so the stress relaxation effect based on the cracks between the recesses can be significantly obtained. The thickness F of the metal foil is measured at any 10 points using a cross-sectional SEM image in the thickness direction of the metal foil, and these measured values ​​are averaged to obtain the thickness.

[0062] (Concave part group)

[0063] From the viewpoint of improving the folding strength of the metal foil and ensuring the tensile strength, the opening diameter of the recess is preferably 5 μm or more and 100 μm or less, and more preferably 5 μm or more and 70 μm or less. In addition, from the viewpoint of further improving the folding strength of the metal foil, the opening diameter D of the recess is further preferably 5 μm or more and 50 μm or less, and particularly preferably 5 μm or more and 40 μm or less. Furthermore, from the viewpoint that pores (pits) opening on the inner wall surface of the recess are easily formed in the deep part of the recess, the opening diameter D of the recess is preferably 8 μm or more, and more preferably 18 μm or more. In the case of increasing the effect of improving the folding strength, it is desired that the opening diameter of the recess is small and the number of recesses is large.

[0064] The ratio of the opening diameter D (μm) of the recessed portion to the thickness F (μm) of the metal foil: D / F is preferably less than 0.5, more preferably less than 0.25 (or less than 0.2).

[0065] The depth H of the concave portion is preferably, for example, 4 μm or more and 74 μm or less. The depth H of the concave portion may be 5 μm or more (or 20 μm or more). It should be noted that the “depth H of the concave portion” refers to the distance from the opening of the concave portion to the deepest part.

[0066] The ratio of the depth H (μm) of the concave portion of the metal foil to the thickness F (μm): H / F is preferably 0.05 or more and 0.55 or less, more preferably 0.26 or more and 0.47 or less, and further preferably 0.3 or more and 0.43 or less. When H / F is within the above range, it is easy to ensure the folding strength of the electrode foil and the strength of the electrode foil (core).

[0067] From the viewpoint of ensuring the tensile strength of the electrode foil and suppressing foil breakage caused by winding of the electrode foil, etc., the main surface of the metal foil has a thickness of 1 mm. 2 The number of recessed portions in the area may be 7 or more and 570 or less, 7 or more and 120 or less, or 7 or more (or 15 or more) and 80 or less.

[0068] The recesses adjacent to each other can be arranged at intervals L. It should be noted that "the recesses adjacent to each other" refers to the recesses adjacent to each other and closest to each other. "Interval L" refers to the length of the line segment when the line segment between the recesses adjacent to each other on the main surface of the metal foil is drawn in the shortest possible connection. The interval L can be greater than 4μm, greater than 9μm, or greater than 15μm. In addition, the interval L can be less than 2000μm, less than 1000μm, less than 320μm, or less than 250μm. For example, the interval L can be greater than 9μm and less than 320μm. When the opening diameter of the recess is greater than 5μm and less than 50μm, the interval L is preferably greater than 4μm and less than 320μm, and more preferably greater than 9μm and less than 250μm.

[0069] When adjacent concave portions have opening diameters of D1 (μm) and D2 (μm), respectively, D1 and D2 may be the same or different. It should be noted that the so-called "same" here means that D1 / D2 is in the range of 6 / 10 or more and 10 / 6 or less. D1 / D2 may be 8 / 10 or more and 10 / 8 or less, and may be 1. Hereinafter, "opening diameter D1" and "opening diameter D2" are sometimes collectively referred to as "opening diameter D".

[0070] The opening diameter D1 (μm) and the interval L (μm) preferably satisfy the relationship of 2≤D1 and 2≤L / D1≤50. The opening diameter D2 (μm) and the interval L (μm) preferably satisfy the relationship of 2≤D2 and 2≤L / D2≤50.

[0071] When L / D is 2 or more, it is easy to ensure the strength of the metal foil. From the viewpoint of ensuring strength, L / D may be 5 or more. When L / D is 50 or less, it is easy to obtain the effect of the concave portion. L / D may be 10 or less.

[0072] The above-mentioned D1, D2 and L are calculated as follows.

[0073] An image of the main surface of the metal foil (electrode foil) is obtained by scanning electron microscopy (SEM). Using this image, an opening with a maximum diameter of 2 μm or more is regarded as an opening of a recess, and two recesses adjacent to each other and closest to each other are regarded as recesses adjacent to each other. For the two recesses, the maximum diameters of the openings are calculated as D1 and D2, respectively. Draw a line segment connecting the adjacent recesses, and calculate the length of the shortest line segment in the line segment as L.

[0074] In the direction perpendicular to the winding direction when the metal foil (electrode foil) is wound, adjacent recesses may be arranged at intervals L. The so-called "direction perpendicular to the winding direction" here refers to a direction within the range of 65° to 115° relative to the winding direction. In the direction perpendicular to the winding direction, all recesses may not be along a prescribed direction, and recesses in different directions may coexist within the above-mentioned angle range.

[0075] The plurality of recesses may be arranged in a zigzag shape. In this case, the plurality of recesses are arranged at intervals L1 (μm) in the winding direction when the metal foil (electrode foil) is wound, at intervals L2 (μm) in the direction perpendicular to the winding direction, or at intervals L3 (μm) in the direction inclined relative to the winding direction. In this case, the smallest interval among the intervals L1 to L3 is the interval L mentioned above.

[0076] The adjacent recesses have circular openings of the same size, and one of the adjacent recesses may be arranged relative to the other recess in the winding direction when the metal foil (electrode foil) is wound. In this case, the interval L may be greater than 15 μm and less than 250 μm. It should be noted that "arranged in the winding direction" not only includes the case where adjacent recesses are arranged along the winding direction when the metal foil (electrode foil) is wound, but also includes the case where one recess is arranged relative to another recess in a direction perpendicular to the winding direction within a range of one amount of the other recess from the winding direction. The above-mentioned "same size" means that D1 / D2 is within the range of 6 / 10 to 10 / 6. D1 / D2 may be greater than 8 / 10 and less than 10 / 8, and may be 1.

[0077] Regarding the diameter of the concave portion, the diameter of the opening side of the concave portion may be larger than the diameter of the deep side of the concave portion. For example, when the opening diameter of the concave portion is set to D, the diameter of the concave portion in the same direction as the opening diameter D when traveling a distance D from the opening of the concave portion in the depth direction thereof may be 0.8D or less, or may be greater than 0.05D and less than 0.8D.

[0078] From the viewpoint of improving tensile strength and folding strength, the recess may extend obliquely relative to the main surface of the metal foil. From the viewpoint of facilitating the formation of the recess, the recess may also extend perpendicularly relative to the main surface of the metal foil. It should be noted that perpendicularly relative to the main surface of the metal foil means that the recess extends at an angle of 80° to 100° relative to the main surface of the metal foil.

[0079] The opening of one recess has a maximum diameter D L and minimum diameter D S When the minimum diameter D S Relative to the maximum diameter D L Ratio: D S / D L For example, it is preferably 0.1 or more and 1 or less, and more preferably 0.2 or more and 0.8 or less. From the viewpoint of improving the tensile strength in the longitudinal direction and the folding strength in the width direction of the strip-shaped metal foil, the recessed portion may be provided in such a manner that the direction of the maximum diameter DL of the opening of the recessed portion is substantially parallel to the longitudinal direction of the strip-shaped metal foil. L The same meaning as the opening diameter D. In addition, "substantially parallel to the longitudinal direction of the metal foil" means that the maximum diameter D L The angle formed by the direction of the longitudinal direction is in the range of -20° to 20°.

[0080] The plurality of recesses are preferably arranged regularly in the surface direction of the metal foil. The plurality of recesses are preferably arranged at equal intervals in the surface direction of the metal foil. In the surface direction of the metal foil, the plurality of recesses may be arranged in a zigzag shape or in a square lattice shape.

[0081] As the opening shape of the recess, for example, a circle, an ellipse, a polygon, a star, and a teardrop shape can be listed. At least a part of the angle of the polygon is preferably curved, and more preferably all the angles of the polygon are curved. The shapes of the openings of the multiple recesses arranged in the porous portion can be the same type as each other, or they can be different types from each other. Polygons include triangles, quadrilaterals, hexagons, etc. Stars include shapes with internal angles of more than 180 degrees, and representative shapes are polygonal stars such as pentagrams and hexagonal stars. The multiple sides constituting the polygon and the star can be the same length as each other, or they can be different lengths. The quadrilateral may not be a square, and may be a rectangular, rhombus, or an elongated shape.

[0082] A specific example of the opening shape of the concave portion is as follows: Fig.10 The circles, quadrilaterals and hexagons shown in (a) to (c) can be as follows Fig.10 A quadrilateral with all its angles curved, as shown in (d), can be Fig.10 The water drop shape shown in (e) to (g) can also be Fig.10 The hexagonal star shown in (h). Fig.10 The dotted lines in (b) to (h) indicate the maximum diameter D L direction. Fig.10 The recesses shown in (b) to (h) can be arranged in such a way that the direction of the dotted line is almost parallel to the length direction of the strip-shaped metal foil. It should be noted that "almost parallel to the length direction of the metal foil" means that the angle formed by the direction of the dotted line and the length direction is in the range of -20° to 20°.

[0083] The shape of the recessed portion may be a columnar shape (e.g., a cylindrical shape, an elliptical column shape, a quadrangular column shape, etc.), a cone shape (e.g., a cone shape, a quadrangular pyramid shape, etc.), a truncated cone shape (e.g., a truncated cone shape, a quadrangular pyramid shape, etc.), a hemispherical shape, a mortar shape, etc. From the viewpoint of ease of processing, a cone shape, a triangular pyramid shape, and a quadrangular pyramid shape are preferred.

[0084] A first recess group may be provided on one main surface of the metal foil, and a second recess group may be provided on the other main surface of the metal foil. In this case, the opening diameter D, interval L, shape, and arrangement of the recesses of the first recess group and the second recess group may be the same or different. When the metal foil is observed from the normal direction of its main surface, the recesses constituting the first recess group and the recesses constituting the second recess group are preferably arranged in a staggered manner so as not to overlap each other.

[0085] The metal foil is a rolled foil, and the winding direction when the metal foil is wound can be parallel to the rolling direction of the rolled foil. In this case, compared with the case where the metal foil is wound in a direction perpendicular to the rolling direction, the influence of the rolling mark during winding can be reduced. It should be noted that "the winding direction is parallel to the rolling direction of the rolled foil" means that the angle formed by the winding direction and the rolling direction is in the range of -20° to 20°.

[0086] (Step of Forming Recessed Portion Group)

[0087] The first step may include a step of forming a recess group in a metal foil. As the metal foil used in the step of forming the recess group. A plain foil containing a valve-acting metal (for example, an arithmetic mean roughness Ra of 3 μm or less) is used. It should be noted that the arithmetic mean roughness Ra is calculated in accordance with JIS B 0601:2001. In the step of forming the recess group, a clamp having a plurality of protrusions may be pressed onto the metal foil to form the recess group. In addition, the metal foil may be conveyed between a pair of rollers having a plurality of protrusions while pressing the pair of rollers, thereby forming a recess group on both sides of the metal foil. The recess group may also be formed by laser processing, sandblasting, etching, etc. The metal foil in which the recess group is formed by etching in the first step is not included in the above-mentioned etching foil (metal foil in which a porous portion is formed by etching).

[0088] (Second process)

[0089] In the second step, the raw foil having the recessed portion group is etched to form a porous portion on the main surface of the raw foil and the inner wall surface of the recessed portion group. The etching process in the second step is performed to form the porous portion. The surface of the raw foil is made porous by etching, but the recessed portions are sufficiently large compared to the pores of the porous portion, and even after the etching process, the size and shape of the plurality of recessed portions provided in the raw foil are almost unchanged, so that the recessed portion group is maintained.

[0090] Depending on the size and shape of the concave diameter, an etching pit (porous portion) is sometimes formed on the bottom surface of the concave portion. In this case, in the area where the concave portion is arranged, the porous portion is formed on the core side, and in the area where the concave portion is not arranged, the thickness of the core is ensured to be larger. Therefore, it is possible to improve the electrostatic capacitance while minimizing the reduction in strength.

[0091] The etching process can be electrolytic etching or chemical etching. Electrode foil having a porous portion including pores with a diameter (opening diameter) less than 2 μm can be mass-produced by electrolytic etching. In the case of AC etching, an electrode foil having a porous portion including sponge-like pits with a diameter of less than 1.0 μm can be produced, and a high-capacity foil can be produced when the diameter is less than 0.5 μm. In the case of DC etching, an electrode foil having a porous portion including tunnel-shaped pits with a diameter less than 2 μm can be produced. From the viewpoint of easily increasing the difference between the opening diameter of the pores of the porous portion and the opening diameter of the recessed portion, AC etching is preferred.

[0092] (Third process)

[0093] The manufacturing method of the electrode foil may also include a step of forming a dielectric layer, the dielectric layer covering the metal skeleton of the porous portion constituting the electrode foil. In the step of forming the dielectric layer, for example, an oxide film containing a valve action metal may be formed on the surface of the porous portion by chemical conversion treatment (anodization). The chemical conversion voltage when the Al foil is subjected to chemical conversion treatment may be, for example, 4V or more, or 40V or more. In the case of manufacturing the electrode foil by AC etching, the chemical conversion voltage is preferably 200V or less.

[0094] (other)

[0095] The manufacturing method of the electrode foil may also include a step of cutting the electrode foil. For example, a strip of electrode foil with a width of 500 mm is cut into a width of 1.5 mm or more and 40 mm or less. The electrode foil after cutting may also be rolled up. By providing a recessed portion group, when the cutting width is as small as 10 mm or less, the foil breakage due to the rolling may also be suppressed.

[0096] [Electrode foil for electrolytic capacitors]

[0097] The electrode foil is a metal foil having a group of recesses that is subjected to an etching treatment. The metal foil after the etching treatment has a porous portion and a core portion connected to the porous portion. The porous portion is the outer portion of the metal foil that has been made porous by etching, and the inner portion of the metal foil, i.e., the remainder, is the core portion. The porous portion is formed on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses. By etching, at least a portion of the opening side of the inner wall surfaces of the plurality of recesses is made porous together with the main surface of the metal foil, and it is preferred that almost the entire inner wall surfaces of the plurality of recesses are made porous. A portion of the deep side of the inner wall surfaces of the plurality of recesses may not be made porous, and the core portion may be exposed on the inner wall surfaces of the deep side of the plurality of recesses.

[0098] The porous portion has pores opening on the main surface of the metal foil and the inner wall surface of the plurality of recesses. The opening diameter of the pores of the porous portion is less than 2 μm. It should be noted that the opening diameter of the pores of the porous portion refers to the maximum diameter of the opening of the pores. The opening diameter of the recess is larger than the opening diameter of the pores of the porous portion. When the opening diameter D of the recess is greater than 2 μm, high-quality cracks are formed during winding, which can inhibit the breakage of the foil.

[0099] If the opening diameter D of the recess is less than 2 μm, even if the opening diameter D of the recess is larger than the opening diameter of the pores of the porous portion, the above-mentioned high-quality cracks are not easily formed, and the flexural strength tends to decrease.

[0100] As the electrode foil, for example, a strip-shaped metal foil is used, and the width thereof is, for example, not less than 1.5 mm and not more than 520 mm.

[0101] The ratio of the depth H (μm) of the recess to the thickness T (thickness of each single side) (μm) of the porous portion: H / T is preferably greater than 0.1 and less than 1.35, more preferably greater than 0.2 and less than 1.1, and further preferably greater than 0.3 and less than 1. When H / T is within the above range, it is easy to ensure the folding strength of the electrode foil and the strength of the electrode foil (core). In addition, H / T is greater than 1 and can be less than 1.35 (or less than 1.1). That is, within the range of ensuring the strength of the electrode foil (core), the recess can be further extended from the porous portion to the core. In this case, the depth of the recess in the core is, for example, less than 10 μm, and can be less than 7 μm (or less than 5 μm). When the diameter of the deep side of the recess is very small, the inner wall surface of the deep part of the recess is sometimes not easy to be etched.

[0102] It should be noted that the thickness T of the porous portion refers to the thickness of the porous portion of the portion without the concave portion of the metal foil. The thickness T of the porous portion is obtained by measuring the thickness of any 10 points of the porous portion using a cross-sectional SEM image of the electrode foil in the thickness direction, and averaging these measured values.

[0103] The porous portion may be formed on one main surface of the metal foil or on both main surfaces of the metal foil. The porous portion is preferably formed on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses on at least the main surface of the metal foil having the recessed portion group.

[0104] There is no particular limitation on the thickness T of the porous portion, and it can be appropriately selected according to the purpose of the electrolytic capacitor, the required withstand voltage, etc. The thickness T of the porous portion can be, for example, 1 / 10 or more and less than 5 / 10 (or less than 2 / 5) of the thickness F of the metal foil on each single side. In the case of the anode foil, the thickness T of the porous portion can be, for example, 10 μm or more and 160 μm or less, and can be 50 μm or more and 160 μm or less.

[0105] The metal foil includes a metal skeleton constituting the porous portion. The metal skeleton refers to a metal portion having a microstructure in the porous portion. The porous portion has a plurality of pores (pits) surrounded by the metal skeleton. From the viewpoint of increasing the surface area and forming a dielectric layer in the deep part of the porous portion, the range of the pore diameter (opening diameter) is less than 2000 nm and can be greater than 100 nm and less than 1500 nm.

[0106] The shape of the pores (pits) may be sponge-like or tunnel-like. Tunnel-shaped pits include pits extending from the surface side of the porous portion toward the core side. In the case of sponge-like pits, the range of the pore diameter (opening diameter) is preferably, for example, less than 600nm, and more preferably greater than 50nm and less than 500nm. In the case of sponge-like pits, the average pore diameter Dp is preferably greater than 80nm and less than 400nm, and further preferably greater than 100nm and less than 300nm. Electrode foils with sponge-like pits are used, for example, in low-voltage type electrolytic capacitors. Specifically, they are used in electrolytic capacitors using chemical conversion foils below 200V. In the case of tunnel-shaped pits, the range of the pore diameter (opening diameter) is, for example, less than 1900nm, and may be greater than 100nm and less than 1800nm. In the case of tunnel-shaped pits, the average pore diameter Dp is preferably greater than 200nm and 1700nm, and more preferably greater than 400nm and less than 1400nm. The electrode foil having tunnel-shaped pits is used in, for example, a medium- and high-voltage type electrolytic capacitor using a chemical conversion foil of 180 V or more.

[0107] The average pore diameter Dp of the porous portion is obtained by measuring the pore diameter distribution of the electrode foil (porous portion) using a mercury pressure porosimeter. Specifically, the pore diameter (mode particle size) corresponding to the vertex of the peak (the maximum peak in the case of multiple peaks) appearing in the pore distribution curve (vertical axis: log differential pore volume, horizontal axis: pore diameter) obtained by the measurement is obtained as the average pore diameter Dp. As a measuring device, for example, the AutoPore V series manufactured by Micromeritics is used. The above-mentioned pore distribution curve shows the distribution of pores in the porous portion within the range of pore diameters less than 2μm. Usually, the diameter (opening diameter) of the recessed portion is much larger than the pores of the porous portion, and it is difficult to measure the diameter of the recessed portion using a mercury pressure porosimeter under the same conditions as the measurement of the porous portion.

[0108] (Dielectric layer)

[0109] The electrode foil may include a dielectric layer covering the metal skeleton constituting the porous part. In this case, the electrode foil may be used as an anode foil. The dielectric layer covers the main surface of the metal foil, the inner wall surface of the concave part, and the inner wall surface of the pores of the porous part.

[0110] The thickness of the dielectric layer can be 2 nm or more, 4 nm or more, 12 nm or more, or 24 nm or more. An electrode foil having a dielectric layer having a thickness of 24 nm or more can be used as an anode foil of an electrolytic capacitor having a rated voltage of 20 V or more. In particular, when used for a hybrid capacitor, it is preferred to form a dielectric layer of 50 nm or more, and the chemical conversion voltage during chemical conversion treatment is preferably 30 V or more. When the chemical conversion voltage is as high as 30 V or more, the dielectric layer also becomes thicker, which easily leads to the problem of the strength of the electrode foil, so the effect of stress relaxation based on the formation of cracks between the recesses is large. The thickness of the dielectric layer can be obtained as follows: the thickness of any 10 points of the dielectric layer is measured using an SEM or TEM image of a cross section in the thickness direction of the electrode foil, and these measured values ​​are averaged to obtain the thickness.

[0111] The electrode foil for electrolytic capacitors of the present embodiment can be used for at least one of the anode foil and the cathode foil of a wound-type electrolytic capacitor, or can be used for an anode body of a stacked-type electrolytic capacitor.

[0112] Here, Figure 1 This is a main part front view showing an example of the electrode foil according to one embodiment of the present disclosure. Figure 1 In the figure, the X direction and the Y direction respectively represent the length direction (winding direction) and the width direction of the strip-shaped electrode foil. The electrode foil 351 has a group of recesses on its main surface S (X direction and Y direction). Figure 1 A partial region including recessed portions arranged along the X direction of electrode foil 351 is shown.

[0113] like Figure 1 As shown, adjacent recesses 381 and 382 are provided on the main surface S of the electrode foil 351, and have circular openings with the same opening diameter D. The opening diameter D is 2 μm or more. The electrode foil 351 has a porous portion 361 formed on the main surface S and the inner wall surfaces of the recesses 381 and 382. The porous portion 361 has pores (opening diameter less than 2 μm) opened on the main surface S and the inner wall surfaces of the recesses 381 and 382.

[0114] The recessed portions 381 and 382 are separated by a distance L. 11 One recess 381 may be arranged slightly offset from the other recess 382 in the Y direction (direction perpendicular to the winding direction) within a range of one amount of the recess 381 (less than the opening diameter D) from the X direction. For example, one recess 381 may be arranged with a spacing L relative to the other recess 382. 12 The recess 381 is provided so as to be offset from the X direction to a position indicated by a dotted circle (only one portion of one recess 381 is along the Y direction).

[0115] L 11 / D(or L12 / D) can be 2 or more and 50 or less. 11 (or L 12 ) can be 15 μm or more and 250 μm or less. 11 (or L 12 ) is 15 μm or more, when the metal foil is a rolled foil and the X direction is the rolling direction, even if the recessed portion group is arranged along the rolling direction, the strength in the rolling direction is ensured. In addition, in this case, cracks are easily formed along the Y direction by winding, and the cracks formed along the Y direction can be appropriately distributed in the X direction.

[0116] in addition, Figure 2 This is a front view schematically showing another example of the electrode foil for electrolytic capacitors according to the embodiment of the present disclosure. Figure 2 The strip-shaped electrode foil 350 (metal foil) has a first main surface S1 and a second main surface S2 opposite to the first main surface S1. Figure 2 A portion of the electrode foil 350 is shown when viewed from the first major surface S1 side. Figure 2 In the figure, the X direction and the Y direction respectively indicate the length direction and the width direction of the strip-shaped electrode foil. Figure 3 for Figure 2 III-III sectional view. Figure 3 For schematic illustration Figure 2 The cross-section of the electrode foil 350 in the thickness direction and the Y direction is shown in FIG. It should be noted that the electrode foil for electrolytic capacitors disclosed in the present invention is not limited to Figure 2 and Figure 3 The respective figures are schematic diagrams, and the shapes and features of the respective components (for example, the opening diameter D of the recesses, the interval L, etc.) in the respective figures do not necessarily reflect the actual dimensions, nor are they necessarily represented in the same proportion ratio.

[0117] The strip-shaped electrode foil 350 (metal foil) has a plurality of cylindrical recesses 380a opened in the first main surface S1. The plurality of first recesses 380a are provided at intervals and are dispersedly arranged in dots in the surface direction (X direction and Y direction) of the electrode foil 350.

[0118] A first porous portion 360a is formed on the main surface S1 of the electrode foil 350 and the inner wall surface of the recess 380a. The first porous portion 360a has pores (not shown) opening on the first main surface S1 and the inner wall surface of the first recess 380a. The opening diameter of the pores of the first porous portion 360a is less than 2μm. The electrode foil 350 has a core portion 370 connected to the first porous portion 360a. When the electrode foil 350 is a rolled foil, the X direction is preferably the rolling direction.

[0119] like Figure 2As shown, a plurality of first recesses 380a are arranged in a zigzag shape at equal intervals. The first recesses 380a adjacent to each other are arranged at intervals L from each other. The plurality of first recesses 380a have circular openings with an opening diameter D (μm). The opening diameter D of the first recess 380a is greater than 2 μm. In this case, when the electrode foil is wound with the X direction set as the winding direction, high-quality cracks are formed between the first recesses 380a, the stress generated by the winding is relieved, the folding strength in the Y direction is improved, and the foil breakage during winding is suppressed.

[0120] A plurality of first recesses 380a are arranged at intervals of L1 (μm) along the winding direction (X direction) when the metal foil is wound, at intervals of L2 (μm) along the direction perpendicular to the winding direction (Y direction), and at intervals of L3 (μm) along the direction inclined relative to the winding direction (X direction). L1 and L3 are the same as each other, smaller than L2, and are intervals L. L1 / D and L3 / D are greater than 2 and less than 50. Interval L1 and interval L2 satisfy the relationship of 2<L2 / L1. In this case, the folding strength in the Y direction is greatly improved. In particular, when a large stress is generated in the Y direction, the effect of stress relaxation based on the formation of cracks between the recesses can be significantly obtained. As such a situation, for example, when the electrode foil is cut, when the electrode foil is bent during the conveyance of the electrode foil and when the travel angle is changed, when the winding body is formed, and when the electrode foil and the lead member are connected by riveting.

[0121] Figure 2 In the embodiment, L1 and L3 are almost the same size, but the configuration of the recessed portion can be adjusted in a way that L1 is smaller than L3, or in a way that L1 is larger than L3. It is desirable that the relationship is L1>L3. In this case, L1 and L2 can be almost the same size, and L3 can be the interval L.

[0122] By winding the metal foil in the X direction, it is easy to Figure 2 The cracks are formed in the direction of L2 (Y direction). Figure 2 A crack is formed in the direction of L2 (Y direction) and at the same time Figure 2 Cracks are also formed in a certain proportion in the direction of L3. Thus, the stress generated by winding can be effectively alleviated. From the above viewpoint, L1 can be, for example, 15 μm or more and 250 μm or less. The cracks are formed, for example, in a manner that connects 50 to 500 first recesses 380a.

[0123] The electrode foil 350 has a thickness F (μm), the first porous portion 360a has a thickness T (μm), and the first recessed portion 380a has a depth H (μm). H / F and H / T are within the above-described ranges, for example.

[0124] Figure 2 The opening shape of the first recess shown is circular, but not limited to this. The shape of the opening of the recess may also be elliptical, quadrilateral, hexagonal, etc. The shape of the first recess is cylindrical, but not limited to this, and may also be a columnar or hammer shape other than a cylindrical shape. The shapes and sizes of the multiple first recesses are the same, but the shapes and / or sizes of the multiple first recesses may also be different. The configuration of the first recess is not limited to Figure 2 The configuration shown may be, for example, a square grid.

[0125] like Figure 3 As shown, the strip-shaped electrode foil 350 (metal foil) includes a second porous portion 360b and a core portion 370 connected to the second porous portion 360b. That is, the first porous portion 310a and the second porous portion 360b are arranged so as to sandwich the core portion 370. The electrode foil 350 has a second main surface S2 where the pores (not shown) of the second porous portion 360b are open.

[0126] The porous portion 360b has a plurality of second recesses 380b opened in the second main surface S2. The second recesses 380b have the same shape, size, interval and arrangement as the first recesses 380a, but the shapes of the first and second recesses may be different.

[0127] [Electrolytic capacitors]

[0128] The electrolytic capacitor of the embodiment of the present disclosure has the above-mentioned electrode foil. The electrolytic capacitor includes, for example, a winding body and an electrolyte. The winding body is formed by sandwiching a separator between the anode foil and the cathode foil and winding the anode foil and the cathode foil. The winding body and the electrolyte are also collectively referred to as a capacitor element. At least one of the anode foil and the cathode foil has the above-mentioned electrode foil.

[0129] In the wound body, high-quality cracks can exist between the recessed portions of the electrode foil. The cracks are formed by winding the metal foil having the recessed portion group and are formed so as to connect the recessed portions.

[0130] Preferably, the crack extends in a direction perpendicular to the winding direction of the metal foil (width direction) so as to connect at least two or more recesses. Such a crack is easily formed when the recess group is arranged with an L / D of 2 or more and 50 or less. For example, the crack is formed by connecting 2 to 100 recesses.

[0131] The height of the winding body Lc ( Figure 5 The height Lc of the winding body is, for example, 50 mm or less, 20 mm or less, or 15 mm or less. The height Lc of the winding body is substantially the same as the width dimension of the electrode foil, or slightly longer than the width dimension of the electrode foil.

[0132] When the product size is large (for example, when the height Lc of the winding body is 30 mm or more), an electrode foil with a large width (for example, less than 30 mm) is used. In the case of an electrode foil with a large width, the foil is easily broken due to the distortion of the electrode foil. Therefore, by providing a recess group on the electrode foil with a large width, the foil fracture caused by the distortion of the electrode foil can be significantly suppressed, and the reliability of large-sized products (for example, large capacitors of screw terminal type or lead terminal type) is improved.

[0133] On the other hand, when the product size is small (for example, when the height Lc of the winding body is less than 20 mm), an electrode foil with a small width (for example, less than 20 mm) is used. The electrode foil with a small width is obtained by cutting an electrode foil with a large width (for example, more than 125 mm and less than 500 mm) into a desired small width (less than 20 mm). Due to the presence of the recess group, the stress applied to the electrode foil during the cutting process is dispersed, the occurrence of cracks caused by the stress and the foil breakage caused by it are suppressed, and the quality of the electrode foil with a small width dimension is greatly improved. In addition, in the manufacturing process of the capacitor, due to the presence of the recess group, the foil breakage caused by the tension generated during the roller-based transportation of the electrode foil with a small width dimension is significantly suppressed. As a result, the aging (repair chemical conversion) during the capacitor manufacturing is carried out stably, the characteristics such as the leakage current of the capacitor can be stably obtained, and the reliability of the product with a small size is improved.

[0134] Here, Figure 4 This is a diagram schematically showing an example of a wound body viewed from the end face side. The wound body 400 is formed by winding the anode foil and the cathode foil around the winding core 410 via a separator. The "region P" refers to a region where the radial distance from the innermost circumference E1 of the wound body 400 to the outermost circumference E2 is less than (1 / 4) t when the radial thickness from the innermost circumference E1 to the outermost circumference E2 of the wound body 400 is t.

[0135] The high-quality cracks may be present at least in the region P of the wound body. The cracks may be present more in the region P than in regions other than the region P. Foil breakage during winding of the electrode foil tends to occur easily in the region P where the stress generated by winding tends to be large. On the other hand, high-quality cracks that relieve the stress are easily formed in the region P by winding the electrode foil. The presence of the cracks in the region P can effectively suppress foil breakage during winding of the electrode foil.

[0136] The recess group may also be provided on one main surface of the electrode foil. In addition, the recess group is provided on both main surfaces of the electrode foil, and the number of recesses per unit area of ​​the main surface of the electrode foil may be larger in the recess group provided on one main surface of the electrode foil than in the recess group provided on the other main surface of the electrode foil. As the stress generated by winding the electrode foil is more likely to increase on the main surface on the outer peripheral side than on the main surface on the inner peripheral side of the winding body, in the above case, in the winding body, it is preferred that the electrode foil is wound in a manner such that one main surface of the recess group of the electrode foil is provided facing the outer peripheral side of the winding body.

[0137] When the stress generated by winding is large, the recessed portion groups may be provided on both main surfaces of the electrode foil. In the region P of the wound body, the stress generated by winding is large, and it is desirable to provide the recessed portion groups on both main surfaces of the electrode foil.

[0138] (Anode Foil)

[0139] As the anode foil, the electrode foil obtained by the first step to the third step can also be used. The thickness of the anode foil can be, for example, 60 μm or more and 200 μm or less, or 80 μm or more (or 100 μm or more) and 200 μm or less. There is a tendency to use an anode foil with a larger capacity and a larger thickness. For example, in the case of a high-capacity anode foil with a thickness of 100 μm or more, a stress relaxation effect based on crack formation between recesses can be significantly obtained.

[0140] (Cathode Foil)

[0141] The electrode foil obtained by the first step and the second step may also be used as the cathode foil. In the case of the cathode foil, a covering layer may be further formed on the surface of the metal foil (porous portion). Examples of the covering layer include a metal oxide layer, a metal nitride layer, a metal carbide layer, and a conductive layer (for example, a layer containing at least one of a metal and carbon). The thickness of the cathode foil is, for example, not less than 10 μm and not more than 70 μm.

[0142] (Separator)

[0143] The separator is not particularly limited, and for example, nonwoven fabrics containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide (for example, aliphatic polyamide, or aromatic polyamide such as aramid) may be used.

[0144] (Electrolytes)

[0145] The electrolyte covers at least a portion of the anode foil (dielectric layer) and is sandwiched between the anode foil (dielectric layer) and the cathode foil. The electrolyte is a solid or liquid electrolyte. The electrolytic capacitor may also contain a liquid component (electrolyte or non-aqueous solvent) together with the solid electrolyte.

[0146] The solid electrolyte includes a conductive polymer. As the conductive polymer, for example, a π-conjugated polymer can be listed. As the conductive polymer, polypyrrole, polythiophene, polyfuran, polyaniline, etc. can be listed. The conductive polymer can be used alone, or two or more kinds can be used in combination, or it can be a copolymer of two or more monomers. The weight average molecular weight of the conductive polymer is, for example, 1000 to 100000.

[0147] It should be noted that in this specification, polypyrrole, polythiophene, polyfuran, polyaniline, etc. refer to polymers with polypyrrole, polythiophene, polyfuran, polyaniline, etc. as basic skeletons. Therefore, polypyrrole, polythiophene, polyfuran, polyaniline, etc. may also include their respective derivatives. For example, polythiophene includes poly(3,4-ethylenedioxythiophene) and the like.

[0148] The conductive polymer may be doped with a dopant. The solid electrolyte may also contain a dopant together with the conductive polymer. Examples of the dopant include polystyrene sulfonic acid and the like. The solid electrolyte may further contain an additive as required.

[0149] The liquid component may be in direct contact with the dielectric layer or in contact with the dielectric layer via a conductive polymer. The liquid component may be a non-aqueous solvent or an electrolyte. The electrolyte comprises a non-aqueous solvent and an ionic substance (solute (e.g., an organic salt)) dissolved therein. The non-aqueous solvent may be an organic solvent or an ionic liquid.

[0150] As the non-aqueous solvent, a high boiling point solvent is preferred, for example, polyol compounds such as ethylene glycol, sulfone compounds such as sulfolane, lactone compounds such as γ-butyrolactone, ester compounds such as methyl acetate, carbonate compounds such as propylene carbonate, ether compounds such as 1,4-dioxane, ketone compounds such as methyl ethyl ketone, etc. can be used.

[0151] The liquid component may contain an acid component (anion) and an alkaline component (cation). A salt (solute) may also be formed by the acid component and the alkaline component. The acid component contributes to the film repair function. As the acid component, organic carboxylic acids, inorganic acids, etc. may be listed. As inorganic acids, for example, phosphoric acid, boric acid, sulfuric acid, etc. may be listed. As the alkaline component, for example, amine compounds of primary amines to tertiary amines may be listed.

[0152] The organic salt is a salt in which at least one of the anion and the cation contains an organic substance. As the organic salt, for example, trimethylammonium maleate, triethylammonium borodisalicylate, ethyldimethylamine phthalate, mono-1,2,3,4-tetramethylimidazolium phthalate, mono-1,3-dimethyl-2-ethylimidazolium phthalate, etc. can also be used.

[0153] From the viewpoint of suppressing dedoping of dopants from the conductive polymer (deterioration of the solid electrolyte), the liquid component preferably contains more acid components than alkaline components. In addition, the acid component contributes to the film repair function of the liquid component, so it is also preferred to contain more acid components than alkaline components. The molar ratio of the acid component to the alkaline component: (acid component / alkaline component) is, for example, greater than 1.1. From the viewpoint of suppressing dedoping of dopants from the conductive polymer, the pH of the liquid component can be less than 6, or can be greater than 1 and less than 5.

[0154] Here, Figure 5 It is a cross-sectional view schematically showing an electrolytic capacitor according to an embodiment of the present disclosure. Figure 6 It is a perspective view schematically showing the structure of a wound body. Figure 6 In FIG. 1 , the X direction indicates the length direction of the strip-shaped anode foil 10 and cathode foil 20 , and the Y direction indicates the width direction of the anode foil 10 and cathode foil 20 .

[0155] The electrolytic capacitor 200 includes a capacitor element, and the capacitor element includes a winding body 100 and an electrolyte (not shown). The winding body 100 is formed by winding an anode foil 10 and a cathode foil 20 with a separator 30 interposed therebetween. The height Lc of the winding body 100 is substantially the same as the dimension of the anode foil 10 and the cathode foil 20 in the width direction (Y direction).

[0156] One end of the tabs 50A and 50B is connected to the anode foil 10 and the cathode foil 20, respectively, and the tabs 50A and 50B are wound to form the winding body 100. The lead wires 60A and 60B are connected to the other end of the tabs 50A and 50B, respectively.

[0157] A winding end tape 40 is disposed on the outer surface of the cathode foil 20 located at the outermost layer of the wound body 100, and the end of the cathode foil 20 is fixed by the winding end tape 40. It should be noted that when the anode foil 10 is prepared by cutting from a wide foil, the wound body 100 may be further subjected to a chemical conversion treatment in order to provide a dielectric layer on the cut surface.

[0158] An electrolyte is interposed between anode foil 10 (dielectric layer) and cathode foil 20 of wound body 100. The capacitor element can be obtained by, for example, impregnating wound body 100 with a treatment solution containing an electrolyte. The impregnation can be performed under reduced pressure, for example, in an atmosphere of 10 kPa to 100 kPa.

[0159] The wound body 100 is housed in the bottomed case 211 so that the leads 60A and 60B are located on the opening side of the bottomed case 211. As the material of the bottomed case 211, a metal such as aluminum, stainless steel, copper, iron, brass, or an alloy thereof can be used.

[0160] A sealing member 212 is disposed at the opening of a bottomed casing 211 housing the wound body 100 , the open end of the bottomed casing 211 is riveted to the sealing member 212 and bent, and a seat plate 213 is disposed at the bent portion, thereby sealing the wound body 100 in the bottomed casing 211 .

[0161] Sealing member 212 is formed so as to penetrate lead wires 60A and 60B. Sealing member 212 may be made of any insulating material, preferably an elastomer, of which silicone rubber, fluororubber, ethylene-propylene rubber, Hypalon rubber, butyl rubber, isoprene rubber, etc., which have high heat resistance, are preferred.

[0162] "appendix"

[0163] The following techniques are disclosed through the description of the above embodiments.

[0164] (Technology 1)

[0165] A metal foil for manufacturing an electrode foil, which is a metal foil used in the manufacture of an electrode foil for an electrolytic capacitor.

[0166] The metal foil contains a valve action metal.

[0167] The metal foil has a plurality of recessed portions which are open on the main surface of the metal foil and are dispersed in a dotted manner in the direction of the main surface.

[0168] The opening diameter of the concave portion is 2 μm or more.

[0169] (Technique 2)

[0170] In the metal foil for electrode foil production according to the first aspect, the opening diameter of the recessed portion is 5 μm or more and 50 μm or less.

[0171] (Technique 3)

[0172] In the metal foil for electrode foil production according to the technique 1 or 2, the mutually adjacent recessed portions are provided at intervals L of 4 μm or more.

[0173] (Technique 4)

[0174] The metal foil for electrode foil production according to any one of techniques 1 to 3 contains 98 mass % or more of aluminum as the valve-acting metal.

[0175] (Technique 5)

[0176] The metal foil for manufacturing the electrode foil according to technique 4 comprises:

[0177] 1 mass ppm or more and 100 mass ppm or less of silicon,

[0178] 5 mass ppm or more and 100 mass ppm or less of copper, and

[0179] 5 mass ppm or more and 200 mass ppm or less of iron.

[0180] (Technique 6)

[0181] The metal foil for electrode foil production according to any one of techniques 1 to 5, which has a strength of 40 N / mm 2 More than tensile strength.

[0182] (Technique 7)

[0183] The metal foil for electrode foil production according to any one of techniques 1 to 6 has an elongation of 1% or more and 16% or less.

[0184] (Technology 8)

[0185] The metal foil for electrode foil production according to any one of techniques 1 to 7, wherein the thickness F μm of the metal foil and the depth H μm of the recessed portion have a relationship of 0.26 ≤ H / F ≤ 0.47.

[0186] (Technique 9)

[0187] The metal foil for electrode foil production according to any one of techniques 1 to 8, wherein a depth H of the recessed portion is 4 μm or more and 74 μm or less.

[0188] (Technology 10)

[0189] The metal foil for electrode foil production according to any one of techniques 1 to 9, wherein a thickness F of the metal foil is 80 μm or more and 200 μm or less.

[0190] (Technology 11)

[0191] The metal foil for electrode foil production according to any one of techniques 1 to 10, wherein the main surface of the metal foil has a thickness of 1 mm 2 The area has 7 or more and 570 or less of the above-mentioned recessed portions.

[0192] (Technology 12)

[0193] The metal foil for electrode foil manufacturing according to any one of techniques 1 to 11, wherein the adjacent recesses have opening diameters of D1 μm and D2 μm, respectively, and are arranged at intervals of L μm.

[0194] The aforementioned opening diameter D1 and the aforementioned interval L satisfy the relationship of 2≤D1 and 2≤L / D1≤50.

[0195] The aforementioned opening diameter D2 and the aforementioned interval L satisfy the relationship of 2≤D2 and 2≤L / D2≤50.

[0196] (Technology 13)

[0197] The metal foil for electrode foil production according to any one of techniques 1 to 12, wherein two or more crystal grains of the metal foil are exposed on the inner wall surface of the recess in the depth direction of the recess.

[0198] (Technology 14)

[0199] The metal foil for electrode foil production according to any one of techniques 1 to 13, wherein the average crystal grain size of the metal foil is 18 μm or more and 60 μm or less.

[0200] (Technology 15)

[0201] A method for manufacturing an electrode foil for an electrolytic capacitor, comprising the following steps:

[0202] A step of preparing a metal foil for electrode foil production according to any one of Techniques 1 to 14; and

[0203] A step of etching the metal foil.

[0204] (Technology 16)

[0205] The method for manufacturing an electrode foil for an electrolytic capacitor according to technique 15, wherein a porous portion is formed on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses by the etching process.

[0206] The porous portion has pores opening on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses.

[0207] The opening diameter of the pores of the porous portion is less than 2 μm.

[0208] (Technology 17)

[0209] In the method for manufacturing an electrode foil for an electrolytic capacitor according to technology 16, the thickness T μm of the porous portion and the depth H μm of the recessed portion have a relationship of 0.2 ≤ H / T ≤ 1.1.

[0210] (Technology 18)

[0211] The method for producing an electrode foil for an electrolytic capacitor according to the sixth aspect includes the step of forming a dielectric layer covering the metal skeleton constituting the porous portion.

[0212] (Technology 19)

[0213] An electrode foil for an electrolytic capacitor obtained by the method for producing an electrode foil for an electrolytic capacitor according to any one of Techniques 15 to 18.

[0214] (Technology 20)

[0215] An electrode foil for an electrolytic capacitor, comprising: a metal foil containing a valve action metal,

[0216] The metal foil has a plurality of recessed portions which are open on the main surface of the metal foil and are arranged in a dotted manner in a direction of the main surface.

[0217] The metal foil includes a porous portion having pores opened on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses.

[0218] The opening diameter of the concave portion is 2 μm or more.

[0219] The opening diameter of the pores of the porous portion is less than 2 μm.

[0220] (Technology 21)

[0221] The electrode foil for an electrolytic capacitor according to Technology 20 includes a dielectric layer covering a metal skeleton constituting the porous portion.

[0222] (Technology 22)

[0223] An electrolytic capacitor comprising the electrode foil for an electrolytic capacitor according to any one of Techniques 19 to 21.

[0224] [Example]

[0225] Hereinafter, the present disclosure will be specifically described based on Examples and Comparative Examples, but the present disclosure is not limited to the Examples.

[0226] 《Examples 1 to 15》

[0227] (First step: Preparation of raw foil)

[0228] First, a strip of Al foil (plain foil, thickness F: 120 μm, average grain size: 40 μm) was prepared. As the Al foil, a rolled foil with a rolling direction parallel to the longitudinal direction (X direction) was used. The Al foil had an Al content of 99.98% by mass, a silicon content of 40 mass ppm, an iron content of 40 mass ppm, and a copper content of 30 mass ppm.

[0229] A plurality of cylindrical recesses were formed on both sides of the Al foil using a predetermined jig, and the Al foil was arranged in a Figure 2The depth H of the recesses was adjusted appropriately, and H / F was set to the value shown in Table 1. For example, in the electrode foil a1, the depth H of the recesses was 45 μm. In this way, a raw foil was obtained.

[0230] The tensile strength of the raw foil obtained by the above method is 65 N / mm 2 The elongation of the raw foil determined by the above method was 10%. The number of crystal grains of the Al foil exposed on the inner wall surface of the recessed portion in the depth direction of the recessed portion determined by the above method was 3.

[0231] Figure 2 The opening diameter D and the interval L (L1=L3) of the concave portion in the metal foil are the values ​​shown in Table 1. 2 The number of recessed portions present in is the value shown in Table 1.

[0232] (Second step: etching treatment (formation of porous portion))

[0233] The raw foil was etched. Thus, a porous portion having sponge-like pits (thickness T: 45 μm, average pore diameter Dp: 0.2 μm) was formed on both main surfaces of the raw foil. The depth H of the recess was appropriately adjusted to set H / T to the value shown in Table 1. In this way, an etched foil was obtained.

[0234] (Third step: chemical conversion treatment)

[0235] The etched foil was then subjected to a chemical conversion treatment to form a dielectric layer having a withstand voltage of 60 V on the surface of the metal portion constituting the porous portion, thereby obtaining a chemical conversion foil. In this manner, electrode foils a1 to a15 were obtained.

[0236] Comparative Example 1

[0237] An electrode foil b1 was produced in the same manner as in Example 1 except that no recessed portion group was formed in the Al foil.

[0238] The following Evaluation 1 was performed on each of the electrode foils (chemical conversion foils) of the Examples and Comparative Examples obtained above.

[0239] [Evaluation 1: Measurement of folding strength]

[0240] The folding strength of the electrode foil in the width direction (Y direction) was measured. The measurement was performed in accordance with the test method for electrode foil for aluminum electrolytic capacitors of the Japanese Electronic Machinery Industry Standard (EIAJ RC-2364A). The measurement was performed using a test piece obtained by cutting the electrode foil into a size of 100 mm in the length direction and 10 mm in the width direction.

[0241] [Evaluation 2: Determination of capacity]

[0242] The capacitance of the electrode foil was measured in accordance with the test method for electrode foil for aluminum electrolytic capacitors of the Electronic Industry Standards of Japan (EIAJ RC-2364A).

[0243] The folding strength and capacity are expressed as relative values ​​when the folding strength and capacity of the electrode foil b1 of Comparative Example 1 are respectively set to 100. Table 1 shows the evaluation results.

[0244] [Table 1]

[0245]

[0246] In the electrode foils a1 to a15, higher folding strength than that of the electrode foil b1 was obtained.

[0247] Comparative Example 2

[0248] (Production of Etched Foil)

[0249] The Al foil was etched to form a porous portion having sponge-like pits (thickness T: 45 μm, average pore diameter Dp: 0.2 μm) on both main surfaces of the Al foil. In this way, an etched foil was obtained. As the Al foil, the same Al foil as in Example 1 was used.

[0250] (Formation of Recessed Portion Group on Etching Foil)

[0251] The recessed portion groups were formed in the same manner as in Example 1, using a predetermined jig to provide recessed portion groups on both main surfaces of the etching foil.

[0252] Except for the above, electrode foil b2 was prepared and evaluated in the same manner as electrode a1 of Example 1. The evaluation results of electrode foils a1, b1, and electrode foil b2 are shown in Table 2. The folding strength and capacity are expressed as relative values ​​when the folding strength and capacity of electrode foil b1 of Comparative Example 1 are set to 100, respectively.

[0253] [Table 2]

[0254]

[0255] The electrode foil b2 has a higher folding strength than the electrode foil b1, but has a lower capacity.

[0256] When a metal foil is etched and then a recess group is provided in the etched foil, the etching pits located near the inner wall surface of the recess are blocked when the recess group is formed, and it is difficult to form etching pits opening on the inner wall surface of the recess, and the surface area of ​​the metal foil is correspondingly reduced, and the capacity is reduced. In addition, in this case, the etching pits near the inner wall surface are blocked when the recess is formed, so that the conductive polymer dispersion (or electrolyte) does not penetrate into the deep part of the etching pit, which is sometimes not conducive to the capacity.

[0257] On the other hand, in the electrode foil a1, higher folding strength and higher capacity were obtained compared with the electrode foil b1.

[0258] When a metal foil (raw material foil) having a group of recesses is etched, etching pits are formed on the main surface of the metal foil and on the inner wall surface of the recess, thereby increasing the surface area of ​​the metal foil and enabling high capacity. The reduction in strength and capacity caused by deformation (melting) of the porous portion during the formation of the recess group can be avoided. In addition, in this case, the etching pits near the inner wall surface are not blocked, so the dispersion (or electrolyte) of the conductive polymer penetrates into the deep part of the etching pits, and the deep part of the etching pits can also be beneficial to the capacity. In a hybrid electrolytic capacitor that uses a combination of a solid electrolyte and an electrolyte, a small amount of electrolyte can effectively penetrate into the deep part of the pit, and the ESR reduction effect based on the electrolyte can be easily obtained.

[0259] Industrial Applicability

[0260] The electrode foil disclosed herein is suitably used for electrolytic capacitors that require high reliability.

[0261] The present invention has been described with respect to currently preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes should be apparent to those skilled in the art in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be construed as including all modifications and changes without departing from the spirit and scope of the present invention.

[0262] Description of Reference Numerals

[0263] 1: recessed portion, 2: porous portion, 10: anode foil, 20: cathode foil, 30: separator, 40: winding end tape, 50A, 50B: tabs, 60A, 60B: leads, 100, 400: winding body, 200: electrolytic capacitor, 211: bottom casing, 212: sealing member, 213: seat plate, 350, 351: electrode foil, 360a: first porous portion, 360b: second porous portion, 361: porous portion, 370: core, 380a: first recessed portion, 380b: second recessed portion, 381, 382: recessed portions, 410: winding core.

Claims

1. A metal foil for manufacturing an electrode foil, which is a metal foil used in the manufacture of an electrode foil for an electrolytic capacitor, The metal foil includes a valve-acting metal and has a plurality of recessed portions that are open on a main surface of the metal foil and are dispersed in a dot pattern in a direction of the main surface. The opening diameter of the concave portion is 2 μm or more.

2. The metal foil for electrode foil production according to claim 1, wherein The opening diameter of the concave portion is greater than or equal to 5 μm and less than or equal to 50 μm.

3. The metal foil for electrode foil production according to claim 1, wherein The adjacent recessed portions are provided at intervals L of 4 μm or more. 4 . The metal foil for producing an electrode foil according to claim 1 , comprising 98 mass % or more of aluminum as the valve-acting metal.

5. The metal foil for electrode foil production according to claim 4, comprising: 1 mass ppm or more and 100 mass ppm or less of silicon, 5 mass ppm or more and 100 mass ppm or less of copper, and 5 mass ppm or more and 200 mass ppm or less of iron.

6. The metal foil for electrode foil production according to claim 1, having a strength of 40 N / mm 2 More than tensile strength. 7 . The metal foil for electrode foil production according to claim 1 , which has an elongation of 1% or more and 16% or less.

8. The metal foil for electrode foil production according to claim 1, wherein The thickness F μm of the metal foil and the depth H μm of the recess have a relationship of 0.26 ≤ H / F ≤ 0.

47.

9. The metal foil for electrode foil production according to claim 1, wherein The depth H of the recess is greater than or equal to 4 μm and less than or equal to 74 μm.

10. The metal foil for electrode foil production according to claim 1, wherein The thickness F of the metal foil is 80 μm or more and 200 μm or less.

11. The metal foil for electrode foil production according to claim 1, wherein The main surface of the metal foil has a thickness of 1 mm 2 The area has 7 or more and 570 or less of the recessed portions.

12. The metal foil for electrode foil production according to claim 1, wherein The adjacent recesses have opening diameters of D1 μm and D2 μm, respectively, and are arranged at intervals of L μm. The opening diameter D1 and the interval L satisfy the relationship of 2≤D1 and 2≤L / D1≤50. The opening diameter D2 and the interval L satisfy the relationship of 2≤D2 and 2≤L / D2≤50.

13. The metal foil for electrode foil production according to claim 1, wherein Two or more crystal grains of the metal foil are exposed on the inner wall surface of the recess in the depth direction of the recess.

14. The metal foil for electrode foil production according to claim 1, wherein The metal foil has an average crystal grain size of 18 μm or more and 60 μm or less.

15. A method for manufacturing an electrode foil for an electrolytic capacitor, comprising the following steps: A step of preparing the metal foil for manufacturing the electrode foil according to claim 1; and A step of etching the metal foil.

16. The method for producing an electrode foil for an electrolytic capacitor according to claim 15, wherein: By the etching process, a porous portion is formed on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses. The porous portion has pores opening on the main surface of the metal foil and the inner wall surfaces of the plurality of recesses. The opening diameter of the pores of the porous portion is less than 2 μm.

17. The method for producing an electrode foil for an electrolytic capacitor according to claim 16, wherein: The thickness T μm of the porous portion and the depth H μm of the recessed portion have a relationship of 0.2 ≤ H / T ≤ 1.

1.

18. The method for manufacturing an electrode foil for an electrolytic capacitor according to claim 16, comprising: A step of forming a dielectric layer covering the metal skeleton constituting the porous portion. 19 . An electrode foil for an electrolytic capacitor obtained by the method for producing an electrode foil for an electrolytic capacitor according to claim 15 .

20. An electrode foil for an electrolytic capacitor, comprising: a metal foil containing a valve action metal, The metal foil has a plurality of recessed portions which are open on a main surface of the metal foil and are arranged in a dotted manner in a direction of the main surface. The metal foil includes a porous portion having pores opening on a main surface of the metal foil and inner wall surfaces of the plurality of recesses. The opening diameter of the concave portion is greater than 2 μm, The opening diameter of the pores of the porous portion is less than 2 μm. 21 . The electrode foil for an electrolytic capacitor according to claim 20 , comprising a dielectric layer, wherein the dielectric layer covers a metal skeleton constituting the porous portion. 22 . An electrolytic capacitor comprising the electrode foil for an electrolytic capacitor according to claim 19 .

Citation Information

Patent Citations

  • Electrode foil, wound capacitor, manufacturing method of electrode foil, and manufacturing method of wound capacitor

    JP2017224844A