Hollow carbon sphere-perovskite nanoreactor catalysts, their preparation methods and applications

By combining hollow porous carbon spheres with perovskite, the problem of insufficient exposure of active sites and inadequate mass transfer in existing technologies has been solved, achieving efficient oxidative degradation of organic pollutants and improving catalytic performance.

CN119657116BActive Publication Date: 2026-11-17BEIJING UNIV OF CHEM TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411665287.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-20
Publication Date
2026-11-17
Estimated Expiration
2044-11-20

AI Technical Summary

Technical Problem

Existing heterogeneous catalytic ozone oxidation technology is difficult to meet the demand for efficient removal of organic pollutants on an industrial scale, especially due to insufficient exposure of active sites of the catalyst, inadequate ozone mass transfer, and limited mass transfer of reactants.

Method used

A hollow carbon sphere-perovskite nanoreactor catalyst is formed by combining hollow porous carbon spheres with perovskite. The hollow structure enhances the exposure of active sites and mass transfer performance, thereby improving the synergistic effect of adsorption and catalysis of the catalyst.

Benefits of technology

It improves the catalytic performance of the catalyst, enhances the oxidative degradation ability of organic pollutants, avoids the loss of active components, and improves the stability and mass transfer performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119657116B_ABST
    Figure CN119657116B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of wastewater treatment technology and relates to a hollow carbon sphere-perovskite nanoreactor catalyst, which is composed of hollow porous carbon spheres and perovskite components supported on the hollow porous carbon spheres, wherein the molecular structural formula of the perovskite is Ca. 1.1 MnO 3‑δ δ represents oxygen vacancies, with values ​​ranging from 0 to 1. Compared to traditional metal oxide catalysts, the hollow carbon sphere-perovskite nanoreactor catalyst, through the combination of hollow porous carbon spheres and perovskite, forms a catalyst with perovskite as the active center and hollow porous carbon spheres as the synergistic catalytic agents. This catalyst exhibits advantages such as synergistic adsorption and catalysis, and the combination of the carbon layer and perovskite enhances electron transfer at the perovskite active centers. Furthermore, the hollow nanoreactor structure allows the catalyst to fully expose active sites, avoiding the loss of active components, improving mass transfer performance, and thus enhancing catalyst performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wastewater treatment technology, and relates to a hollow carbon sphere-perovskite nanoreactor catalyst for ozone catalytic oxidation deep treatment of organic pollutant wastewater, its preparation method and application. Background Technology

[0002] Over the past decade, advanced oxidation processes (AOPs) have become a powerful technology for removing organic pollutants. Consequently, various AOPs have been developed, such as photocatalysis, photocatalytic peroxymonosulfate (PMS) activation, catalytic ozonation, and Fenton-like processes. Heterogeneous catalytic ozonation is considered a promising method for removing recalcitrant organic pollutants from water. However, the development of heterogeneous catalytic ozonation is still insufficient to meet the needs of practical water and wastewater treatment, especially on an industrial scale. The development of high-performance heterogeneous catalysts is a key step in advancing the engineering application of heterogeneous catalytic ozonation. The catalytic performance of heterogeneous catalysts is significantly affected by three factors: (1) active sites, (2) ozone mass transfer, and (3) reactant mass transfer. Active sites decompose ozone into reactive oxygen species (ROS), which are highly oxidizing and have a high reaction rate constant. High mass transfer between the catalyst and ozone can promote ROS formation. Conversely, higher ROS utilization can be achieved by enhancing mass transfer between the catalyst and reactants. Furthermore, due to the limited lifetime of ROS (approximately 10... -6 -10 -9 Due to the limited diffusion distance (approximately 20 nm) and the s-like properties of the catalyst, driven mass transfer between the catalyst and reactants is crucial for the catalytic performance of heterogeneous catalysts. However, synthesizing heterogeneous catalysts using the aforementioned three elements remains a challenge.

[0003] Perovskite oxides (ABO3) have become candidate materials for heterogeneous catalysis due to their strong tunability and high stability. Compared with transition metal oxides, perovskite oxides can manipulate the redox reactivity and surface chemistry by controlling the A and B elements, thus enabling the manipulation of catalytic reaction performance and showing significant application potential in catalytic ozonation. However, perovskites suffer from problems such as small specific surface area and easy aggregation, which hinder further improvement of catalytic performance. Summary of the Invention

[0004] The purpose of this invention is to address the problems existing in the prior art by providing a hollow carbon sphere-perovskite nanoreactor catalyst for the deep treatment of organic pollutant wastewater through ozone catalytic oxidation. This catalyst, through the combination of hollow porous carbon spheres and perovskite, forms a hollow carbon sphere-perovskite nanoreactor catalyst with perovskite as the active center and hollow porous carbon spheres providing synergistic catalysis. This catalyst exhibits synergistic adsorption and catalytic effects, and the combination of the carbon layer and perovskite enhances electron transfer at the perovskite active centers. Furthermore, the hollow nanoreactor structure allows the catalyst to fully expose active sites, preventing the loss of active components, improving mass transfer performance, and thus enhancing catalyst performance.

[0005] Therefore, in a first aspect, the present invention provides a hollow carbon sphere-perovskite nanoreactor catalyst, which is composed of hollow porous carbon spheres and perovskite components supported on the hollow porous carbon spheres, wherein the molecular structure of the perovskite is Ca. 1.1 MnO 3-δ δ represents oxygen vacancies, with a value of 0-1.

[0006] In some embodiments of the present invention, the hollow carbon spheres are formed by high-temperature calcination and etching with sodium hydroxide aqueous solution from silica microspheres coated with dopamine hydrochloride.

[0007] In other embodiments of the present invention, the specific surface area of ​​the hollow carbon sphere-perovskite nanoreactor catalyst is 200-300 m². 2 / g, pore volume is 0.5-0.8cm³ 3 / g.

[0008] The second aspect of this invention provides a method for preparing the hollow carbon sphere-perovskite nanoreactor catalyst described in the first aspect of this invention, comprising:

[0009] Step A: Prepare perovskite Ca using the sol-gel method. 1.1 MnO 3-δ ;

[0010] Step B: Disperse TEOS in a water-ethanol-ammonia ternary solution and stir to obtain a SiO2 precursor solution;

[0011] Step C, perovskite Ca 1.1 MnO 3-δ The sample was ultrasonically treated in ultrapure water, then added to a SiO2 precursor solution, followed by dopamine hydrochloride. The mixture was stirred continuously at room temperature, and the precipitate was collected.

[0012] Step D: Wash the precipitate with ultrapure water and anhydrous ethanol until the pH is neutral, and dry to obtain the catalyst precursor;

[0013] Step E involves calcining the catalyst precursor to obtain a carbon sphere-perovskite catalyst.

[0014] Step F involves immersing the carbon sphere-perovskite catalyst in an aqueous NaOH solution, removing the SiO2 template using an oil bath, washing until the pH is neutral, and drying to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0015] In some embodiments of the present invention, in step B, the volume ratio of water, ethanol, and ammonia in the ternary solution is 10:70:3.

[0016] In some embodiments of the present invention, in step B, the ratio of TEOS to water-ethanol-ammonia in the SiO2 precursor solution is 5:10:70:3.

[0017] Preferably, in step B, the stirring time is 10-60 minutes.

[0018] In some embodiments of the present invention, in step C, the perovskite Ca... 1.1 MnO 3-δ The addition amount is 0.4-4 g / L.

[0019] In some embodiments of the present invention, in step C, the amount of dopamine hydrochloride used is 2.5-25 g / L, based on the volume of the SiO2 precursor solution.

[0020] Preferably, in step C, the continuous stirring time is 6-48 hours.

[0021] According to the present invention, in step D, drying is carried out under vacuum conditions, the drying temperature is 60-100°C, and the drying time is 6-12 hours.

[0022] According to the present invention, in step E, calcination is carried out in an inert gas atmosphere; preferably, the calcination temperature is 600-1000°C; and / or, the calcination time is 1-5 hours.

[0023] According to the present invention, in step F, the concentration of the NaOH aqueous solution is 0.5-4 mol / L.

[0024] In some embodiments of the present invention, in step F, the temperature of the oil bath is 40-100°C; and / or, the duration of the oil bath is 1-7 hours.

[0025] In some embodiments of the present invention, in step F, drying is performed under vacuum conditions, the drying temperature is 60-100°C, and the drying time is 6-12 hours.

[0026] The third aspect of the present invention provides the application of hollow carbon sphere-perovskite nanoreactor catalysts as described in the first aspect of the present invention or hollow carbon sphere-perovskite nanoreactor catalysts prepared by the preparation method described in the second aspect of the present invention in the advanced treatment of organic pollutant wastewater.

[0027] Preferably, the application includes filling a wastewater treatment device with a hollow carbon sphere-perovskite nanoreactor catalyst, introducing organic pollutant wastewater, and introducing ozone to treat the organic pollutant wastewater with ozone oxidation.

[0028] The beneficial effects of this invention are as follows:

[0029] A hollow carbon sphere-perovskite nanoreactor catalyst is provided for the deep treatment of organic pollutant wastewater by ozone catalytic oxidation. The hollow carbon spheres exhibit excellent adsorption capacity for organic pollutants, effectively promoting their oxidative degradation. Compared to traditional metal oxide catalysts, this catalyst, through the combination of hollow porous carbon spheres and perovskite, forms a hollow carbon sphere-perovskite nanoreactor catalyst with perovskite as the active center and hollow porous carbon spheres providing synergistic catalysis. This catalyst possesses advantages such as synergistic adsorption and catalysis, and the combination of the carbon layer and perovskite enhances electron transfer at the perovskite active centers. Furthermore, the hollow nanoreactor structure allows for full exposure of active sites, preventing the loss of active components, improving mass transfer performance, and thus enhancing catalyst performance. Attached Figure Description

[0030] The invention will be further described below with reference to the accompanying drawings.

[0031] Figure 1 Electron micrographs of the catalyst in the hollow carbon sphere-perovskite nanoreactor at different magnifications (ac). Detailed Implementation

[0032] To facilitate understanding of the present invention, it will be described in detail below with reference to embodiments. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terminology used herein is for describing specific embodiments only and is not intended to be restrictive.

[0033] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. While any methods and materials similar to or equivalent to those described herein may also be used in the practice or testing of this invention, preferred methods and materials are now described.

[0034] I. Terminology

[0035] The term "deep wastewater treatment" as used in this invention generally refers to further treating the residual organic matter in secondary effluent that has undergone biochemical treatment, using advanced oxidation and other technologies.

[0036] The term "reactor catalyst" used in this invention refers to an ideal model catalyst used to study spatial confinement effects, mass transfer and diffusion, and reaction mechanisms in catalytic reactions. By altering the composition, structure, and surface properties of core-shell nanomaterials, they can be endowed with specific catalytic activities.

[0037] The “Ca” described in this invention 1.1 MnO 3-δ “ is the molecular structural formula of perovskite, where δ is an oxygen vacancy with a value of 0-1.

[0038] The term "Ca" as used in this invention 1.1 MnO 3-δ In "@HCS", "HCS" (Hollow carbon spheres) refers to hollow carbon spheres, and "@" refers to Ca. 1.1 MnO 3-δ Loaded in hollow carbon spheres.

[0039] Unless otherwise specified, the term "water" in this invention refers to deionized water, distilled water, or ultrapure water.

[0040] II. Implementation Plan

[0041] As mentioned above, there is room for further investigation of existing metal oxide catalysts, such as low O3 utilization, limited mass transfer of reactive oxygen species (ROSs), low mineralization rate, and reduced catalyst stability and activity. In view of this, the inventors have conducted extensive research on ozone oxidation technology for the deep treatment of organic pollutant wastewater.

[0042] The inventors have noted that a larger surface area enhances the exposure of active components, which is crucial for improving catalytic activity. The hollow shell provides a larger surface area, allowing reactants such as organic pollutants and ROS to enter the nano-confined environment of the porous core-shell structure, promoting contact between high-concentration reactants and fully exposed active sites, which is of great significance for promoting mass transfer in the catalytic ozone oxidation process.

[0043] The inventors have discovered that hollow carbon spheres possess excellent adsorption capacity for organic pollutants, effectively promoting their oxidative degradation. Further research revealed that by loading perovskite onto a hollow carbon shell, and combining the hollow porous carbon spheres with the perovskite, a catalyst is formed with perovskite as the active center and the hollow porous carbon spheres providing synergistic catalysis, exhibiting both adsorption and catalytic synergy. Simultaneously, the hollow nanoreactor structure of this catalyst allows for full exposure of active sites, enhancing mass transfer, increasing the exposure of active sites, maximizing the contact between ROSs and organic pollutants, and providing excellent stability while preventing the loss of active components. This, in turn, improves catalyst performance and increases degradation efficiency in wastewater treatment.

[0044] Therefore, the hollow carbon sphere-perovskite nanoreactor catalyst for ozone catalytic oxidation deep treatment of organic pollutant wastewater according to the first aspect of the present invention is composed of hollow porous carbon spheres and perovskite components supported on the hollow porous carbon spheres, wherein the molecular structural formula of the perovskite is Ca. 1.1 MnO 3-δ Due to the excessive regulation of Ca sites, even a small amount of excess will not affect the structure of the perovskite, resulting in the formation of oxygen vacancies. We use δ to represent oxygen vacancies, and the value of δ obtained according to the specific preparation process is between 0 and 1.

[0045] The hollow carbon sphere-perovskite nanoreactor catalyst presented in this paper combines hollow porous carbon spheres with perovskite to form a catalyst with perovskite as the active center and hollow porous carbon spheres as the synergistic catalytic agents. The hollow carbon spheres have a good adsorption capacity for organic pollutants and can effectively promote the oxidative degradation of organic pollutants.

[0046] According to the present invention, the hollow carbon spheres are prepared by a one-pot method using silica microspheres and an outer layer coated with dopamine hydrochloride, followed by high-temperature calcination and etching with sodium hydroxide aqueous solution.

[0047] Based on the above easy understanding, the hollow carbon sphere-perovskite nanoreactor catalyst described in this invention is formed by combining perovskite with dopamine hydrochloride and then etching it after high-temperature calcination; preferably, the process of combining perovskite with dopamine hydrochloride also prepares a silica microsphere template.

[0048] The catalyst mentioned above can be represented as Ca 1.1 MnO 3-δ @HCS.

[0049] In some embodiments of the present invention, the specific surface area of ​​the hollow carbon sphere-perovskite nanoreactor catalyst is 200-300 m². 2 / g, preferably 210-300m 2 / g; pore volume is 0.5-0.8cm³ 3 / g, preferably 0.55-0.8cm 3 / g.

[0050] The preparation method of the hollow carbon sphere-perovskite nanoreactor catalyst as described in the first aspect of the present invention, as involved in the second aspect of the present invention, includes:

[0051] Step A: Prepare Ca using the citrate sol-gel method. 1.1 MnO 3-δ ;

[0052] Step B: Disperse TEOS (tetraethyl orthosilicate) in a ternary solution of water-ethanol-ammonia (10mL / 70mL / 3mL) and stir to obtain a SiO2 precursor solution;

[0053] Step C, weigh out the perovskite Ca 1.1 MnO 3-δ The sample was placed in ultrapure water and sonicated for half an hour. The SiO2 precursor solution was then added, followed by dopamine hydrochloride. The mixture was stirred continuously at room temperature, and the precipitate was collected.

[0054] Step D: Wash the precipitate with ultrapure water and anhydrous ethanol until the pH is neutral, and dry it in an oven to obtain the catalyst precursor;

[0055] Step E involves calcining the catalyst precursor to obtain a carbon sphere-perovskite catalyst.

[0056] Step F involves removing the SiO2 template using NaOH aqueous solution in an oil bath, washing until the pH is neutral, and then drying in an oven to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0057] Since this invention is based on the combination of hollow porous carbon spheres and perovskite to form a hollow carbon sphere-perovskite nanoreactor catalyst with perovskite as the active center and hollow porous carbon spheres as the synergistic catalytic center, it is important to investigate and determine the amount of dopamine hydrochloride and perovskite used.

[0058] For example, in some specific embodiments of the present invention, in step B, the volume ratio of water-ethanol-ammonia in the ternary solution is 10:70:3, and the ratio of TEOS to water-ethanol-ammonia in the SiO2 precursor solution is 5:10:70:3. Simultaneously, the stirring time for obtaining the SiO2 precursor solution is set, and the results show that a stirring time of 10-60 min results in a hollow carbon sphere-perovskite nanoreactor catalyst with high activity and stability.

[0059] In some embodiments of the present invention, in step C, the perovskite Ca... 1.1 MnO 3-δThe amount added is 0.4-4 g / L, and the amount of dopamine hydrochloride is 2.5-25 g / L; the continuous stirring time is 6-48 h.

[0060] In some embodiments of the present invention, in step D, drying is performed under vacuum conditions at a temperature of 60-100°C for a duration of 6-12 hours.

[0061] In some embodiments of the present invention, in step E, calcination is carried out in an inert gas atmosphere; the calcination temperature is 600-1000°C, and the calcination time is 1-5 hours.

[0062] In some other embodiments of the present invention, in step F, the concentration of the NaOH aqueous solution is 0.5-4 mol / L; the temperature of the oil bath is 40-100°C; the time of the oil bath is 1-7 h; and drying is carried out under vacuum conditions at a temperature of 60-100°C for 6-12 h.

[0063] In some specific preferred embodiments of the present invention, Ca is prepared using the citrate sol-gel method. 1.1 MnO 3-δ The methods include:

[0064] Step A: Dissolve Ca(NO3)2·4H2O and Mn(NO3)2 in a mixture of ultrapure water and ethanol (volume ratio of ethanol to water is 3:2) according to a Ca / Mn ratio of 1.1 to obtain a metal ion mixture.

[0065] Step B: Slowly add citric acid (the molar ratio of total metal ions to citric acid is 1:1) to the above metal ion mixture, stir at room temperature for 3 hours to mix evenly, and obtain the catalyst precursor mixture;

[0066] Step C: The resulting mixture is heat-treated in an oil bath at 80°C for 6 hours to form a pale yellow gel, which is then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0067] Step D: The catalyst precursor is calcined at 800℃ for 4 hours to obtain an oxygen-rich vacancy perovskite catalyst.

[0068] In the above preparation method, Mn(NO3)2 is added as a purchased solution of 50 wt% concentration; the amount of Mn(NO3)2 used (working concentration) is 0.004 mol / L, and the amount of Ca(NO3)2·4H2O used is 1.1 times the amount of Mn(NO3)2 used.

[0069] The third aspect of the present invention provides the application of the hollow carbon sphere-perovskite nanoreactor catalyst as described in the first aspect of the present invention or the hollow carbon sphere-perovskite nanoreactor catalyst prepared by the preparation method described in the second aspect of the present invention in the advanced treatment of organic pollutant wastewater; it can be understood as a method for advanced treatment of organic pollutant wastewater using the hollow carbon sphere-perovskite nanoreactor catalyst as described in the first aspect of the present invention or the hollow carbon sphere-perovskite nanoreactor catalyst prepared by the preparation method described in the second aspect of the present invention.

[0070] Specifically, the application includes loading an ozone oxidation catalyst into a wastewater treatment device, introducing organic pollutant wastewater, and introducing ozone to treat the organic pollutant wastewater by ozone oxidation.

[0071] The organic pollutant wastewater described in this invention includes, but is not limited to, bisphenol A pollutant wastewater.

[0072] In some embodiments of the present invention, the reaction conditions for ozone oxidation treatment are: 20 mg / L of bisphenol A pollutant wastewater, 0.2 g / L of catalyst, 0.03 L / min of ozone flow rate, 30 min of reaction time, and 3-21 mg / L of ozone concentration.

[0073] The hollow carbon sphere-perovskite nanoreactor catalyst for the deep ozone catalytic oxidation treatment of organic pollutant wastewater in this invention consists of hollow porous carbon spheres and a perovskite component supported on the hollow porous carbon spheres, wherein the perovskite component is Ca. 1.1 MnO 3-δ The hollow carbon spheres are prepared by a one-pot method using silica microspheres coated with dopamine hydrochloride, followed by high-temperature calcination and etching with sodium hydroxide solution. The hollow carbon spheres in the hollow carbon sphere-perovskite nanoreactor catalyst exhibit excellent adsorption capacity for organic pollutants, effectively promoting their oxidative degradation. This catalyst, through the combination of hollow porous carbon spheres and perovskite, forms a catalyst with perovskite as the active center and hollow porous carbon spheres providing synergistic catalysis. This catalyst exhibits synergistic adsorption and catalysis effects, and the hollow carbon spheres in the hollow carbon sphere-perovskite nanoreactor catalyst demonstrate excellent adsorption capacity for organic pollutants, effectively promoting their oxidative degradation. Compared to traditional metal oxide catalysts, this catalyst has advantages such as improved electron transfer at the perovskite active centers due to the combination of the carbon layer and perovskite. Furthermore, the hollow nanoreactor structure allows the catalyst to fully expose active sites, avoiding the loss of active components, improving mass transfer performance, and thus enhancing catalyst performance.

[0074] Example

[0075] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. Unless otherwise specified, the experimental methods described below are standard laboratory methods. Unless otherwise specified, the experimental materials described below are commercially available.

[0076] In the following examples, COD was determined using Hach COD reagent digested on a Hach DRB200 digester (Hach Instruments, Inc., USA), and then measured using a DR5000 UV spectrophotometer (Hach Instruments, Inc., USA). TDS was determined using a DDSJ-319L conductivity meter (Shanghai Leici Instruments Co., Ltd.). The COD removal rate was calculated using the following formula:

[0077] COD removal rate = (COD removal rate) 原始 -COD 氧化后 COD 原始 ×100%

[0078] Example 1:

[0079] (1) Disperse 5 mL of TEOS in a ternary solution of water-ethanol-ammonia (10 mL / 70 mL / 3 mL) and stir for 15 min to obtain SiO2 precursor;

[0080] (2) Weigh 0.2g Ca 1.1 MnO 3-δ The sample was placed in 10 ml of ultrapure water and sonicated for half an hour, then added to the above solution. Subsequently, 0.25, 0.5, 0.75, 1, and 1.25 g of dopamine hydrochloride were weighed out and added to the above solution. The mixture was stirred continuously at room temperature for 12 hours, and the precipitate was collected.

[0081] (3) The precipitate was washed with ultrapure water and anhydrous ethanol until the pH was neutral, and then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0082] (4) The catalyst precursor was placed in an inert gas atmosphere in a tube furnace and calcined at 800°C for 2 hours to obtain carbon sphere-perovskite catalyst.

[0083] (5) The SiO2 template was removed by using 2 mol / L NaOH solution in an oil bath at 80°C for 5 h, and the solution was washed until the pH was neutral. The solution was then dried in an oven at 80°C for 12 h to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0084] Reaction conditions: 20 mg / L bisphenol A pollutant wastewater, 0.02 g / L catalyst, 0.03 L / min ozone flow rate, 30 min reaction time, and 8 mg / L ozone concentration.

[0085] Experimental results show that Ca 1.1 MnO 3-δ@HCS catalyst COD removal rate is between 55-70%.

[0086] Example 2:

[0087] (1) Disperse 5 mL of TEOS in a ternary solution of water-ethanol-ammonia (10 mL / 70 mL / 3 mL) and stir for 15 min to obtain SiO2 precursor;

[0088] (2) Weigh out 0.1, 0.15, 0.2, 0.25, and 0.3 g of Ca respectively. 1.1 MnO 3-δ The sample was placed in 10 ml of ultrapure water and sonicated for half an hour, then added to the above solution. Subsequently, 1.25 g of dopamine hydrochloride was weighed and added to the above solution. The mixture was stirred continuously at room temperature for 12 hours, and the precipitate was collected.

[0089] (3) The precipitate was washed with ultrapure water and anhydrous ethanol until the pH was neutral, and then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0090] (4) The catalyst precursor was placed in an inert gas atmosphere in a tube furnace and calcined at 800°C for 2 hours to obtain carbon sphere-perovskite catalyst.

[0091] (5) The SiO2 template was removed by using 2 mol / L NaOH solution in an oil bath at 80°C for 5 h, and the solution was washed until the pH was neutral. The solution was then dried in an oven at 80°C for 12 h to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0092] Reaction conditions: 20 mg / L bisphenol A pollutant wastewater, 0.02 g / L catalyst, 0.03 L / min ozone flow rate, 30 min reaction time, and 8 mg / L ozone concentration.

[0093] Experimental results show that Ca 1.1 MnO 3-δ @HCS catalyst has a COD removal rate between 60-70%.

[0094] Example 3:

[0095] (1) Disperse 5 mL of TEOS in a ternary solution of water-ethanol-ammonia (10 mL / 70 mL / 3 mL) and stir for 15 min to obtain SiO2 precursor;

[0096] (2) Weigh 0.2g Ca 1.1 MnO 3-δ The sample was placed in 10 ml of ultrapure water and sonicated for half an hour, then added to the above solution. Subsequently, 1.25 g of dopamine hydrochloride was weighed and added to the above solution. The mixture was stirred continuously at room temperature for 12 hours, and the precipitate was collected.

[0097] (3) The precipitate was washed with ultrapure water and anhydrous ethanol until the pH was neutral, and then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0098] (4) The catalyst precursor was placed in an inert gas atmosphere in a tube furnace and calcined at 600-1000℃ for 2 hours to obtain carbon sphere-perovskite catalyst.

[0099] (5) The SiO2 template was removed by using 2 mol / L NaOH solution in an oil bath at 80°C for 5 h, and the solution was washed until the pH was neutral. The solution was then dried in an oven at 80°C for 12 h to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0100] Reaction conditions: 20 mg / L bisphenol A pollutant wastewater, 0.02 g / L catalyst, 0.03 L / min ozone flow rate, 30 min reaction time, and 8 mg / L ozone concentration.

[0101] Experimental results show that Ca 1.1 MnO 3-δ @HCS catalyst COD removal rate is between 55-70%.

[0102] Example 4:

[0103] (1) Disperse 5 mL of TEOS in a ternary solution of water-ethanol-ammonia (10 mL / 70 mL / 3 mL) and stir for 15 min to obtain SiO2 precursor;

[0104] (2) Weigh 0.2g Ca 1.1 MnO 3-δ The sample was placed in 10 ml of ultrapure water and sonicated for half an hour, then added to the above solution. Subsequently, 1.25 g of dopamine hydrochloride was weighed and added to the above solution. The mixture was stirred continuously at room temperature for 12 hours, and the precipitate was collected.

[0105] (3) The precipitate was washed with ultrapure water and anhydrous ethanol until the pH was neutral, and then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0106] (4) The catalyst precursor is placed in an inert gas atmosphere in a tube furnace and calcined at 800°C for 1-5 hours to obtain carbon sphere-perovskite catalyst.

[0107] (5) The SiO2 template was removed by using 2 mol / L NaOH solution in an oil bath at 80°C for 5 h, and the solution was washed until the pH was neutral. The solution was then dried in an oven at 80°C for 12 h to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0108] Reaction conditions: 20 mg / L bisphenol A pollutant wastewater, 0.02 g / L catalyst, 0.03 L / min ozone flow rate, 30 min reaction time, and 8 mg / L ozone concentration.

[0109] Experimental results show that Ca 1.1 MnO 3-δ @HCS catalyst has a COD removal rate between 60-70%.

[0110] Example 5:

[0111] (1) Disperse 5 mL of TEOS in a ternary solution of water-ethanol-ammonia (10 mL / 70 mL / 3 mL) and stir for 15 min to obtain SiO2 precursor;

[0112] (2) Weigh 0.2g Ca 1.1 MnO 3-δ The sample was placed in 10 ml of ultrapure water and sonicated for half an hour, then added to the above solution. Subsequently, 1.25 g of dopamine hydrochloride was weighed and added to the above solution. The mixture was stirred continuously at room temperature for 12 hours, and the precipitate was collected.

[0113] (3) The precipitate was washed with ultrapure water and anhydrous ethanol until the pH was neutral, and then dried in an oven at 110°C for 12 hours to obtain the catalyst precursor.

[0114] (4) The catalyst precursor was placed in an inert gas atmosphere in a tube furnace and calcined at 800°C for 2 hours to obtain carbon sphere-perovskite catalyst.

[0115] (5) The SiO2 template was removed by using 2 mol / L NaOH solution in an oil bath at 80°C for 5 h, and the solution was washed until the pH was neutral. The solution was then dried in an oven at 80°C for 12 h to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

[0116] Ca in this embodiment was observed at different magnifications using a transmission electron microscope (JEOL JEM-F200, Japan). 1.1 MnO 3-δ The microstructure of the HCS catalyst was determined, and the results are as follows: Figure 1 As shown.

[0117] Through electron micrographs ( Figure 1 The hollow structure of the hollow carbon sphere-perovskite nanoreactor catalyst can be observed. The hollow nanoreactor structure allows the catalyst to fully expose active sites, avoids the loss of active components, improves mass transfer performance, and thus improves catalyst performance.

[0118] Reaction conditions: 20 mg / L bisphenol A pollutant wastewater, 0.02 g / L catalyst, 0.03 L / min ozone flow rate, 30 min reaction time, and 8 mg / L ozone concentration.

[0119] Experimental results show that Ca 1.1 MnO 3-δ @HCS catalyst achieves a COD removal rate of 70%.

[0120] It should be noted that the embodiments described above are merely preferred embodiments of the present invention, used to explain the present invention, and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the terms used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications having the same function.

Claims

1. A hollow carbon sphere-perovskite nanoreactor catalyst, comprising hollow porous carbon spheres and perovskite components supported on the hollow porous carbon spheres, wherein, The molecular structure of the perovskite is Ca. 1.1 MnO 3-δ δ represents oxygen vacancies, with a value of 0-1; The hollow carbon spheres are formed by high-temperature calcination and etching with sodium hydroxide aqueous solution from silica microspheres coated with dopamine hydrochloride prepared by a one-pot method. The specific surface area of ​​the hollow carbon sphere-perovskite nanoreactor catalyst is 200-300 m². 2 / g, pore volume is 0.5-0.8cm³ 3 / g; The preparation method of the hollow carbon sphere-perovskite nanoreactor catalyst includes: Step A: Prepare perovskite Ca using the sol-gel method. 1.1 MnO 3-δ ; Step B: Disperse TEOS in a water-ethanol-ammonia ternary solution and stir for 10-60 min to obtain a SiO2 precursor solution; Step C, perovskite Ca 1.1 MnO 3-δ The sample was ultrasonically treated in ultrapure water, then added to a SiO2 precursor solution, followed by dopamine hydrochloride. The mixture was stirred continuously at room temperature, and the precipitate was collected. Step D: Wash the precipitate with ultrapure water and anhydrous ethanol until the pH is neutral, and dry to obtain the catalyst precursor; Step E: Calcining the catalyst precursor to obtain a carbon sphere-perovskite catalyst; Step F involves immersing the carbon sphere-perovskite catalyst in an aqueous NaOH solution, removing the SiO2 template using an oil bath, washing until the pH is neutral, and drying to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

2. The method for preparing the hollow carbon sphere-perovskite nanoreactor catalyst according to claim 1, comprising: Step A: Prepare perovskite Ca using the sol-gel method. 1.1 MnO 3-δ ; Step B: Disperse TEOS in a water-ethanol-ammonia ternary solution and stir for 10-60 min to obtain a SiO2 precursor solution; Step C, perovskite Ca 1.1 MnO 3-δ The sample was ultrasonically treated in ultrapure water, then added to a SiO2 precursor solution, followed by dopamine hydrochloride. The mixture was stirred continuously at room temperature, and the precipitate was collected. Step D: Wash the precipitate with ultrapure water and anhydrous ethanol until the pH is neutral, and dry to obtain the catalyst precursor; Step E: Calcining the catalyst precursor to obtain a carbon sphere-perovskite catalyst; Step F involves immersing the carbon sphere-perovskite catalyst in an aqueous NaOH solution, removing the SiO2 template using an oil bath, washing until the pH is neutral, and drying to obtain the hollow carbon sphere-perovskite nanoreactor catalyst.

3. The preparation method according to claim 2, characterized in that, In step B, the volume ratio of water-ethanol-ammonia in the ternary solution is 10:70:3; and / or, the volume ratio of TEOS to water-ethanol-ammonia in the SiO2 precursor solution is 5:10:70:

3.

4. The preparation method according to claim 3, characterized in that, In step C, the perovskite Ca, based on the volume of the SiO2 precursor solution, 1.1 MnO 3-δ The amount added is 0.4-4 g / L; and / or, based on the volume of the SiO2 precursor solution, the amount of dopamine hydrochloride is 2.5-25 g / L; and / or, the continuous stirring time is 6-48 h.

5. The preparation method according to claim 2, characterized in that, In step D, drying is carried out under vacuum conditions at a temperature of 60-100°C for 6-12 hours.

6. The preparation method according to claim 2, characterized in that, In step E, calcination is carried out in an inert gas atmosphere; the calcination temperature is 600-1000℃; and / or the calcination time is 1-5h.

7. The preparation method according to claim 2, characterized in that, In step F, the concentration of the NaOH aqueous solution is 0.5-4 mol / L; and / or, the temperature of the oil bath is 40-100℃; and / or, the time of the oil bath is 1-7 h; and / or, drying is carried out under vacuum conditions, the drying temperature is 60-100℃, and the drying time is 6-12 h.

8. The application of the hollow carbon sphere-perovskite nanoreactor catalyst as described in claim 1 or the hollow carbon sphere-perovskite nanoreactor catalyst prepared by any one of the preparation methods described in claims 2-7 in the advanced treatment of organic pollutant wastewater.

9. The application according to claim 8, characterized in that, The application involves filling a wastewater treatment device with a hollow carbon sphere-perovskite nanoreactor catalyst, introducing organic pollutant wastewater, and introducing ozone to treat the organic pollutant wastewater with ozone oxidation.

Citation Information

Patent Citations