Light stone-like coating

By adopting the lightweight real stone paint formula and improved mixing process, the problems of traditional real stone paint have been solved, such as large color difference, rough surface, and large construction usage, and the lightweight decoration system has been realized, and the construction efficiency and anti-fouling performance have been improved, which meets the requirements of energy conservation and environmental protection.

CN119708941APending Publication Date: 2025-03-28SHANXI LASLON PAINT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411881951.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-19
Publication Date
2025-03-28

AI Technical Summary

Technical Problem

Because traditional real stone paint relies on natural color sand, it leads to large color difference, rough surface, easy to get ash and hang soil, and large construction usage, waste resources, and natural color sand resources are exhausted, which has environmental pollution problems.

Method used

The lightweight real stone paint formula includes hydroxyethyl cellulose, modified bentonite, dispersant, defoaming agent, PH regulator, propylene glycol, alcohol esters twelve, pure acrylic emulsion, fungicide, thickener, flexible ultra-thin fine rock flakes, hollow glass microbeads and natural colored sand, and was prepared by an improved stirring process.

Benefits of technology

It has realized a lightweight decoration system, reduced building load, improved construction efficiency and anti-fouling performance, reduced material usage and production costs, and has rich colors and realistic texture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119708941A_ABST
    Figure CN119708941A_ABST
Patent Text Reader

Abstract

The invention discloses a light stone-like coating, and belongs to the technical field of coatings. The stone-like paint is prepared from the following raw materials in parts by weight: 0.1 to 0.2 part of hydroxyethyl cellulose, 0.1 to 0.2 part of modified bentonite, 0.1 to 0.2 part of a dispersing agent, 0.1 to 0.2 part of a defoaming agent, 0.1 to 0.2 part of a PH (Potential of Hydrogen) regulator, 1 to 1.5 parts of propylene glycol, 0.5 to 0.8 part of texanol, 12 to 16 parts of pure acrylic emulsion, 0.2 to 0.3 part of a sterilizing agent, 0.1 to 0.2 part of a thickening agent, 2 to 3 parts of flexible ultrathin fine rock slices, 5 to 10 parts of hollow glass beads and 60 to 65 parts of natural colored sand. The weight of the prepared light stone-like paint is only 1 / 3 of that of traditional stone-like paint, an extremely light decoration system is formed, the load of a building main body is not increased, the load of a building outer wall is effectively reduced, and therefore the risk of falling off is eliminated. Compared with the traditional stone-like paint, the stone-like paint provided by the invention has stronger texture under the support of the small color points, and has richer and more natural stone-like effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a light-weight real stone paint. Background Art

[0002] Real stone paint is a thick paint. Buildings decorated with real stone paint have the effect of natural sand and stone. The decorative feeling is vivid, lifelike, solemn and elegant, which can give people the effect of returning to nature. Therefore, it is widely loved by people and is increasingly used in the exterior wall decoration of various buildings.

[0003] However, the main source of real stone paint is the large amount of natural colored sand. The large differences between batches lead to large color differences in real stone paint, and low-quality and low-content emulsions are used to reduce costs. The decorative effect is single color, rough surface, easy to get dust and dirt. It is easy to produce flowery, color difference, rain marks, and poor stain resistance. During construction, the square meter usage is large, sand falling is serious, and materials are wasted. During production, the batches of colored sand vary greatly, and production and color matching are difficult.

[0004] The colorful imitation stone paint has poor initial water whiteness, difficult to control the color point state, low production efficiency, many color point sizes and types, long color adjustment cycle, high control requirements for spraying equipment during construction, and difficulty in high-rise residential construction.

[0005] Specifically, the main raw material of traditional real stone paint relies on natural colored sand, and in recent years, natural colored sand resources have become increasingly depleted, and blind mining has led to a series of problems such as serious air pollution and climate deterioration. In addition, natural colored sand itself has a large specific gravity, which makes the real stone paint heavy and increases the difficulty of construction, resulting in a large amount of real stone paint in construction, which not only wastes resources but also poses certain safety hazards, and can no longer meet China's national conditions for energy conservation and environmental protection. For this reason, a lightweight real stone paint is proposed.

[0006] The above information disclosed in this background technology is only used to increase the understanding of the background technology of the present invention and therefore, it may include information that does not constitute the prior art known to ordinary technicians in this field. Summary of the invention

[0007] The present invention aims to solve at least one of the technical problems in the prior art. To this end, an object of the present invention is to provide a light real stone paint.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A lightweight real stone paint is prepared from the following raw materials in parts by weight: 0.1-0.2 parts of hydroxyethyl cellulose, 0.1-0.2 parts of modified bentonite, 0.1-0.2 parts of dispersant, 0.1-0.2 parts of defoamer, 0.1-0.2 parts of pH regulator, 1-1.5 parts of propylene glycol, 0.5-0.8 parts of alcohol ester dodecahydrate, 12-16 parts of pure acrylic emulsion, 0.2-0.3 parts of bactericide, 0.1-0.2 parts of thickener, 2-3 parts of flexible ultra-thin fine rock slices, 5-10 parts of hollow glass microspheres, and 60-65 parts of natural colored sand.

[0010] As a further optimization scheme of the present invention, the chemical formula of the modified bentonite is Al2H2Na2O13Si4.

[0011] As a further optimization scheme of the present invention, the defoamer is selected from one or two of mineral oil defoamers, polymer defoamers or silicone defoamers.

[0012] As a further optimized solution of the present invention, the pH regulator is one of 10% sodium hydroxide aqueous solution, 2-amino-2-methyl-1-propanol, ammonia water or 10% potassium hydroxide aqueous solution.

[0013] The bactericide is one or more of isothiazolinones, formaldehyde-releasing agents and benzimidazoles.

[0014] As a further optimization scheme of the present invention, the pure acrylic emulsion is an acrylic polymer.

[0015] As a further optimized solution of the present invention, the thickener is polyurethane with a solid content of 50-60%.

[0016] As a further optimization scheme of the present invention, the flexible ultra-thin fine rock slices are water-based ultra-fine colored rock slices, and the particle size of the water-based ultra-fine colored rock slices is 0.5-0.9 mm and the thickness is 0.05-0.10 mm.

[0017] As a further optimization scheme of the present invention, the mesh number of the hollow glass micro powder is 80-120 meshes, and the mesh number of the natural colored sand is 40-120 meshes.

[0018] As a further optimization scheme of the present invention, a method for preparing a lightweight real stone paint comprises the following steps:

[0019] Step 1: At a stirring speed of 400-600r / min, add water, hydroxyethyl cellulose and modified bentonite in sequence, stir and disperse for 10 minutes, then slowly add dispersant, defoamer and pH adjuster in sequence, increase the speed to 600-800r / min, and stir and disperse for 5 minutes;

[0020] Step 2: Reduce the speed to 400-600r / min, slowly add pure acrylic emulsion, stir and disperse for 6-8 minutes, then slowly add alcohol ester 12, propylene glycol and fungicide at the same speed, stir and disperse for 5 minutes;

[0021] Step 3: Slowly add the polyurethane thickener at a speed of 800-1000r / min, stir and disperse for 5-10 minutes, increase the speed to 1500r / min, add flexible ultra-thin fine rock flakes, hollow glass beads, and natural colored sand, stir and disperse for 15 minutes, and you can get the lightweight real stone paint.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The lightweight real stone paint prepared by the present invention weighs only 1 / 3 of the traditional real stone paint, forming an extremely lightweight decoration system, which does not increase the load of the building body, effectively reduces the load of the building exterior wall, and thus eliminates the risk of falling off. Compared with traditional real stone paint, through the support of small color dots, its texture is more intense, with a richer and more natural imitation stone effect.

[0024] The lightweight real stone paint of the present invention can be constructed using a real stone paint spray gun, which greatly improves the construction efficiency, makes the construction process more convenient and quick, and adapts to various climate environments, has stable quality, and can effectively extend the service life of building finishes. The paint film is more dense, the surface is smooth, and the self-cleaning property is good. Compared with traditional real stone paint, it has better anti-fouling performance. For the repair and rework of the building body, the present invention can effectively improve the color difference problem of the decorative surface and maintain the overall beauty. At the same time, the unit area consumption is small, but the coating area is 2-3 times that of traditional real stone paint, which reduces secondary handling and saves costs. At the same construction site, the lightweight real stone paint material of the present invention can save 50-60% of the freight, which has significant economic advantages.

[0025] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present invention will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a step diagram of the preparation method of the lightweight real stone paint of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides a technical solution:

[0029] Embodiment 1

[0030] A lightweight real stone paint is prepared from the following raw materials in parts by weight: 0.1 part of hydroxyethyl cellulose, 0.1 part of modified bentonite, 0.1 part of dispersant, 0.1 part of defoamer, 0.1 part of pH regulator, 1 part of propylene glycol, 0.5 part of alcohol ester twelve, 12 parts of pure acrylic emulsion, 0.2 part of bactericide, 0.1 part of thickener, 2 parts of flexible ultra-thin fine rock flakes, 5 parts of hollow glass microspheres, and 60 parts of natural colored sand.

[0031] Specifically, the chemical formula of the modified bentonite is Al2H2Na2O13Si4.

[0032] Specifically, the defoaming agent is selected from one or two of mineral oil defoaming agents, polymer defoaming agents or silicone defoaming agents.

[0033] Specifically, the pH adjuster is one of 10% sodium hydroxide aqueous solution, 2-amino-2-methyl-1-propanol, ammonia water or 10% potassium hydroxide aqueous solution.

[0034] The bactericide is one or more of isothiazolinones, formaldehyde-releasing agents and benzimidazoles.

[0035] Specifically, the pure acrylic emulsion is an acrylic polymer.

[0036] Specifically, the thickener is polyurethane and has a solid content of 50%.

[0037] Specifically, the flexible ultra-thin rock flakes are water-based ultra-fine colored rock flakes, and the particle size of the water-based ultra-fine colored rock flakes is 0.5 mm and the thickness is 0.05 mm.

[0038] Specifically, the mesh number of the hollow glass powder is 80 meshes, and the mesh number of the natural colored sand is 40 meshes.

[0039] Embodiment 2

[0040] Lightweight real stone paint, the real stone paint is prepared from the following raw materials in parts by weight: 0.15 parts of hydroxyethyl cellulose, 0.15 parts of modified bentonite, 0.15 parts of dispersant, 0.15 parts of defoamer, 0.15 parts of pH regulator, 1.3 parts of propylene glycol, 0.6 parts of alcohol ester twelve, 15 parts of pure acrylic emulsion, 0.25 parts of bactericide, 0.15 parts of thickener, 2.5 parts of flexible ultra-thin fine rock flakes, 8 parts of hollow glass microspheres, and 63 parts of natural colored sand.

[0041] Specifically, the chemical formula of the modified bentonite is Al2H2Na2O13Si4.

[0042] Specifically, the defoaming agent is selected from one or two of mineral oil defoaming agents, polymer defoaming agents or silicone defoaming agents.

[0043] Specifically, the pH adjuster is one of 10% sodium hydroxide aqueous solution, 2-amino-2-methyl-1-propanol, ammonia water or 10% potassium hydroxide aqueous solution.

[0044] The bactericide is one or more of isothiazolinones, formaldehyde-releasing agents and benzimidazoles.

[0045] Specifically, the pure acrylic emulsion is an acrylic polymer.

[0046] Specifically, the thickener is polyurethane and has a solid content of 55%.

[0047] Specifically, the flexible ultra-thin rock flakes are water-based ultra-fine colored rock flakes, and the particle size of the water-based ultra-fine colored rock flakes is 0.7 mm and the thickness is 0.8 mm.

[0048] Specifically, the mesh size of the hollow glass powder is 100 meshes, and the mesh size of the natural colored sand is 80 meshes.

[0049] Embodiment 3

[0050] Lightweight real stone paint, which is prepared from the following raw materials in parts by weight: 0.2 parts of hydroxyethyl cellulose, 0.2 parts of modified bentonite, 0.2 parts of dispersant, 0.2 parts of defoamer, 0.2 parts of pH regulator, 1.5 parts of propylene glycol, 0.8 parts of alcohol ester twelve, 16 parts of pure acrylic emulsion, 0.3 parts of bactericide, 0.2 parts of thickener, 3 parts of flexible ultra-thin fine rock flakes, 10 parts of hollow glass microbeads, and 65 parts of natural colored sand.

[0051] Specifically, the chemical formula of the modified bentonite is Al2H2Na2O13Si4.

[0052] Specifically, the defoaming agent is selected from one or two of mineral oil defoaming agents, polymer defoaming agents or silicone defoaming agents.

[0053] Specifically, the pH adjuster is one of 10% sodium hydroxide aqueous solution, 2-amino-2-methyl-1-propanol, ammonia water or 10% potassium hydroxide aqueous solution.

[0054] The bactericide is one or more of isothiazolinones, formaldehyde-releasing agents and benzimidazoles.

[0055] Specifically, the pure acrylic emulsion is an acrylic polymer.

[0056] Specifically, the thickener is polyurethane and has a solid content of 60%.

[0057] Specifically, the flexible ultra-thin rock flakes are water-based ultra-fine colored rock flakes, and the particle size of the water-based ultra-fine colored rock flakes is 0.9 mm and the thickness is 0.10 mm.

[0058] Specifically, the mesh number of the hollow glass powder is 120 meshes, and the mesh number of the natural colored sand is 120 meshes.

[0059] Embodiment 4

[0060] A method for preparing a lightweight real stone paint comprises the following steps:

[0061] Step 1: At a stirring speed of 400r / min, add water, hydroxyethyl cellulose and modified bentonite in sequence, stir and disperse for 10 minutes, then slowly add dispersant, defoamer and pH adjuster in sequence, increase the speed to 600r / min, and stir and disperse for 5 minutes;

[0062] Step 2: Reduce the speed to 400r / min, slowly add pure acrylic emulsion, stir and disperse for 6 minutes, then slowly add alcohol ester 12, propylene glycol and fungicide at the same speed, stir and disperse for 5 minutes;

[0063] Step 3: Slowly add the polyurethane thickener at a speed of 800r / min, stir and disperse for 5 minutes, then increase the speed to 1500r / min, add flexible ultra-thin rock flakes, hollow glass beads, and natural colored sand, stir and disperse for 15 minutes to obtain lightweight real stone paint.

[0064] Embodiment 5

[0065] A method for preparing a lightweight real stone paint comprises the following steps:

[0066] Step 1: At a stirring speed of 600r / min, add water, hydroxyethyl cellulose and modified bentonite in sequence, stir and disperse for 10 minutes, then slowly add dispersant, defoamer and pH adjuster in sequence, increase the speed to 800r / min, and stir and disperse for 5 minutes;

[0067] Step 2: Reduce the speed to 600r / min, slowly add pure acrylic emulsion, stir and disperse for 8 minutes, then slowly add alcohol ester 12, propylene glycol and fungicide at the same speed, stir and disperse for 5 minutes;

[0068] Step 3: Slowly add the polyurethane thickener at a speed of 1000r / min, stir and disperse for 10 minutes, increase the speed to 1500r / min, add flexible ultra-thin fine rock flakes, hollow glass beads, and natural colored sand, stir and disperse for 15 minutes, and you can get the lightweight real stone paint.

[0069] In summary, the present invention is refined from highly weather-resistant acrylic emulsion, fine quartz sand, small-grained rock flakes and green environmentally friendly raw materials. The formula uses a higher proportion of emulsion and lighter fillers to restore the colorful and realistic hemp sandstone effect in the form of "de-coloring sand". Compared with existing real stone paint products, it can greatly improve the stain resistance, weather resistance and delivery performance, and inject a perfect fusion texture into the exterior wall finish.

[0070] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0071] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.

[0072] Parts not involved in the present invention are the same as the prior art or can be implemented by the prior art. Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A lightweight real stone paint, characterized in that: The real stone paint is prepared from the following raw materials in parts by weight: 0.1-0.2 parts of hydroxyethyl cellulose, 0.1-0.2 parts of modified bentonite, 0.1-0.2 parts of dispersant, 0.1-0.2 parts of defoamer, 0.1-0.2 parts of pH regulator, 1-1.5 parts of propylene glycol, 0.5-0.8 parts of alcohol ester twelve, 12-16 parts of pure acrylic emulsion, 0.2-0.3 parts of bactericide, 0.1-0.2 parts of thickener, 2-3 parts of flexible ultra-thin fine rock flakes, 5-10 parts of hollow glass microspheres, and 60-65 parts of natural colored sand.

2. The lightweight real stone paint according to claim 1, characterized in that: The chemical formula of the modified bentonite is Al2H2Na2O13Si4.

3. The lightweight real stone paint according to claim 1, characterized in that: The defoamer is selected from one or two of a mineral oil defoamer, a polymer defoamer or a silicone defoamer.

4. The lightweight real stone paint according to claim 1, characterized in that: The pH regulator is one of 10% sodium hydroxide aqueous solution, 2-amino-2-methyl-1-propanol, ammonia water or 10% potassium hydroxide aqueous solution; The bactericide is one or more of isothiazolinones, formaldehyde-releasing agents and benzimidazoles.

5. The lightweight real stone paint according to claim 1, characterized in that: The pure acrylic emulsion is an acrylic polymer.

6. The lightweight real stone paint according to claim 1, characterized in that: The thickener is polyurethane and has a solid content of 50-60%.

7. The lightweight real stone paint according to claim 1, characterized in that: The flexible ultra-thin fine rock slice is a water-based ultra-fine colored rock slice, and the particle size of the water-based ultra-fine colored rock slice is 0.5-0.9 mm and the thickness is 0.05-0.10 mm.

8. The lightweight real stone paint according to claim 1, characterized in that: The mesh number of the hollow glass micro powder is 80-120 meshes, and the mesh number of the natural colored sand is 40-120 meshes.

9. The lightweight real stone paint according to claim 1, characterized in that: The preparation method of light real stone paint comprises the following steps: Step 1: At a stirring speed of 400-600r / min, add water, hydroxyethyl cellulose and modified bentonite in sequence, stir and disperse for 10 minutes, then slowly add dispersant, defoamer and pH adjuster in sequence, increase the speed to 600-800r / min, and stir and disperse for 5 minutes; Step 2: Reduce the speed to 400-600r / min, slowly add pure acrylic emulsion, stir and disperse for 6-8 minutes, then slowly add alcohol ester 12, propylene glycol and fungicide at the same speed, stir and disperse for 5 minutes; Step 3: Slowly add the polyurethane thickener at a speed of 800-1000r / min, stir and disperse for 5-10 minutes, increase the speed to 1500r / min, add flexible ultra-thin fine rock flakes, hollow glass beads, and natural colored sand, stir and disperse for 15 minutes, and you can get the lightweight real stone paint.