Optical glass, optical components and optical instruments
By adjusting the component ratio of fluorophosphate optical glass, the problems of striations and poor thermal stability during the large-aperture molding process were solved, enabling high-quality optical imaging and the application of large-aperture optical equipment.
Patent Information
- Application Number
- CN202510159639.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-08
- Filing Date
- 2025-02-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-02-13
AI Technical Summary
Existing fluorophosphate optical glass is prone to streaks during large-aperture molding, resulting in poor image quality and poor thermal stability, making it difficult to achieve large-aperture precision molding and limiting its use in large-aperture precision optical equipment.
By optimizing the component ratios of optical glass, including the molar percentages of cations and anions, and controlling the ratios between components, the glass is ensured to have excellent large-diameter forming performance and thermal stability. The specific component contents are: P5+: 7-27%, Al3+: 10-45%, Ba2+: 5-25%, Sr2+: 5-25%, Ca2+: 5-30%, F-: 50-90%, O2-: 10-50%, and the contents of other cations and anions are adjusted to achieve optimal performance.
It achieves excellent forming performance and thermal stability of large-aperture optical glass, ensuring high-quality imaging results and making it suitable for large-aperture optical equipment.
Smart Images

Figure BDA0005270639770000121 
Figure BDA0005270639770000131 
Figure BDA0005270639770000141
Abstract
Description
Technical Field
[0001] This invention relates to an optical glass, and more particularly to an optical glass with a refractive index of 1.46 to 1.52 and an Abbe number of 81 to 89. Background Technology
[0002] Fluorophosphate optical glass, as a widely used new type of glass material, possesses characteristics of low dispersion and low refractive index. In optical systems, it can eliminate special dispersion in the second-order spectrum, improve resolution, and significantly enhance the imaging quality of optical systems. In existing technologies, fluorophosphate optical glasses with refractive indices in the range of 1.46–1.52 and Abbe numbers in the range of 81–89 are mainly used in small-aperture optical systems. Therefore, researchers focus primarily on the forming and precision molding performance of small-aperture fluorophosphate glasses.
[0003] In recent years, with the rapid development of large-aperture precision optical equipment, the demand for large-aperture fluorophosphate glass with high optical homogeneity has also increased. In existing technologies, fluorophosphate glasses with a refractive index of 1.46–1.52 and an Abbe number of 81–89 are prone to developing internal striations during the molding process of large-aperture (thickness > 20 mm) optical components, resulting in poor imaging quality. Furthermore, this type of glass has poor thermal stability, making it difficult to achieve large-aperture precision molding. These issues limit its use in large-aperture precision optical equipment. Summary of the Invention
[0004] Based on the above reasons, the technical problem to be solved by the present invention is to provide an optical glass with a refractive index of 1.46 to 1.52, an Abbe number of 81 to 89, and excellent large-diameter forming performance and excellent thermal stability suitable for large-diameter molding.
[0005] The technical solution adopted by this invention to solve the technical problem is:
[0006] (1) Optical glass, the composition of which is expressed as a mole percentage, the cationic component contains: P 5+ 7-27%; Al 3+ : 10-45%; Ba 2+ 5-25%; Sr 2+ 5-25%; Ca 2+ 5-30%,
[0007] The anionic component contains: F - 50-90%; O 2- : 10-50%.
[0008] (2) According to the optical glass described in (1), its components are expressed as mole percentages, and the cationic component also contains: Mg 2+ : 0–15%; and / or Y3+ : 0–10%; and / or La 3+ 0–10%; and / or Gd 3+ : 0–10%; and / or R + : 0-10%; and / or Sb 3+ :0~1%, the R + For Li + Na + K + One or more of them.
[0009] (3) According to the optical glass described in (1), its components are expressed as mole percentages, and the anionic component also contains: Cl - : 0-1%.
[0010] (4) Optical glass, the composition of which is expressed as a mole percentage, the cationic component is composed of P 5+ 7-27%; Al 3+ : 10-45%; Ba 2+ 5-25%; Sr 2+ 5-25%; Ca 2+ 5-30%; Mg 2+ : 0-15%; Y 3+ : 0-10%; La 3+ 0-10%; Gd 3+ : 0-10%; R + : 0-10%; Sb 3+ Composition: 0-1%, wherein R + For Li + Na + K + One or more of them, the anionic component is F - 50-90%; O 2- : 10-50%; Cl - Composition: 0-1%.
[0011] (5) The optical glass according to any one of (1) to (4) has a composition expressed as a mole percentage that satisfies one or more of the following five conditions:
[0012] 1)(Ba 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ The value is 2.0 to 4.6, preferably 2.5 to 4.1, and more preferably 3.0 to 3.9;
[0013] 2)(45%-Al 3+ ) / (15%-Mg 2+ The concentration is 0.3–5.0, preferably (45%-Al).3+ ) / (15%-Mg 2+ The content is 0.4 to 4.0, more preferably (45%-Al). 3+ ) / (15%-Mg 2+ The concentration is 0.5–3.0, with (45%-Al) being a further preferred value. 3+ ) / (15%-Mg 2+ The value ranges from 0.6 to 2.0.
[0014] 3)(Al 3+ +Mg 2+ ) / Ba 2+ The value is 1.5 to 3.5, preferably (Al). 3+ +Mg 2+ ) / Ba 2+ The value is 2.0 to 3.0, more preferably (Al). 3+ +Mg 2+ ) / Ba 2+ It ranges from 2.3 to 2.7;
[0015] 4)(45%-Al 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value ranges from 2.0 to 80.0, with 45% Al being preferred. 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The content is 6.0 to 50.0, more preferably (45%-Al). 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value ranges from 8.0 to 35.0.
[0016] (6) The optical glass according to any one of (1) to (4), wherein the composition is expressed as a mole percentage, wherein: Mg 2+ / Al 3 + The value is 0 to 0.5, with Mg being preferred. 2+ / Al 3+ The value is 0 to 0.3, more preferably Mg. 2+ / Al 3+ 0 to 0.1; and / or (Al) 3+ -Mg 2+ -Li + ) / P 5+ The value is 0.5–2.5, preferably (Al). 3+ -Mg 2+ -Li+ ) / P 5+ The value is 1.0 to 2.3, more preferably (Al). 3+ -Mg 2+ -Li + ) / P 5+ It ranges from 1.3 to 2.1.
[0017] (7) The optical glass according to any one of (1) to (4), wherein its composition is expressed in mole percentage, wherein: P 5+ 11-24%, P is preferred 5+ 15-20%; and / or Al 3+ 18-40%, with Al preferred 3+ 24-35%; and / or Ba 2+ 9-21%, Ba is preferred 2+ : 12-19%; and / or Sr 2+ : 8-21%, with Sr preferred 2+ : 11-17%; and / or Ca 2+ 10-25%, preferably Ca 2+ 15-20%; and / or Mg 2+ 0-10%, preferably Mg 2+ : 0-5%; and / or Y 3+ 0-5%, preferably Y 3+ : 0–3%; and / or La 3+ 0-5%, preferably La 3+ 0–2%; and / or Gd 3+ 0-5%, preferably Gd 3+ : 0–3%; and / or R + 0-6%, preferred R + 0-3%, preferably free of R + ; and / or Sb 3+ 0-0.5%, preferably Sb 3+ : 0~0.3%, the R + For Li + Na + K + One or more of them.
[0018] (8) The optical glass according to any one of (1) to (4), wherein its composition is expressed in mole percentage, wherein: F - 60-80%, with F being the preferred option. - 67-75%; and / or O 2- 20-40%, preferred O 2- 25-33%; and / or Cl - 0-0.5%, preferably Cl -: 0~0.3%.
[0019] (9) The optical glass according to any one of (1) to (4), wherein the refractive index n of the optical glass is d The preferred refractive index is 1.46–1.52. d The refractive index n is 1.47 to 1.51, and more preferably 1.47 to 1.51. d The Abbe number is 1.48–1.50. d The optimal Abbe number is ν, which is between 81 and 89. d The value is 83-88, with the Abbe number ν being more preferred. d It ranges from 84 to 87.
[0020] (10) The optical glass according to any one of (1) to (4), wherein the λ of the optical glass 80 340 nm or less, preferably λ 80 Less than or equal to 335nm, preferably λ 80 λ is less than or equal to 330 nm, and is further preferred. 80 λ is preferred to be less than or equal to 325nm. 80 The wavelength is less than or equal to 320 nm; and / or λ5 is less than or equal to 265 nm, preferably λ5 is less than or equal to 260 nm, more preferably λ5 is less than or equal to 255 nm, even more preferably λ5 is less than or equal to 250 nm, and still more preferably λ5 is less than or equal to 245 nm; and / or the density ρ is 3.90 g / cm³. 3 The preferred density ρ is 3.82 g / cm³. 3 Below, a density ρ of 3.78 g / cm³ is preferred. 3 Hereinafter, a density ρ of 3.74 g / cm³ is further preferred. 3 The following; and / or transition temperature T g The preferred temperature is below 500℃, with a transition temperature T. g The temperature should be below 490°C, and the preferred transition temperature is T. g The temperature is below 480℃; and / or the acid resistance stability RA is Class 3 or above, preferably Class 2 or above; and / or the moisture resistance stability RC is Class 2 or above, preferably Class 1; and / or the streaking is Grade C or above, preferably Grade B or above, more preferably Grade A; and / or the anti-crystallization performance is Grade D or above, preferably Grade C or above, more preferably Grade B, and even more preferably Grade A.
[0021] (11) Glass preform, made of any of the optical glass described in (1) to (10).
[0022] (12) An optical element made of any of the optical glass described in (1) to (10), or made of the glass preform described in (11).
[0023] (13) An optical instrument containing any of the optical glass described in (1) to (10) and / or containing the optical element described in (12).
[0024] The beneficial effects of the present invention are: by rationally designing the content of each component, the optical glass of the present invention not only ensures excellent optical performance, but also has excellent large-diameter forming performance and excellent thermal stability suitable for large-diameter molding. Detailed Implementation
[0025] The embodiments of the optical glass of the present invention will now be described in detail. However, the present invention is not limited to the embodiments described below, and appropriate modifications can be made to implement it within the scope of the purpose of the present invention. Furthermore, regarding repeated descriptions, although there are appropriate omissions, this will not limit the spirit of the invention. In the following text, the optical glass of the present invention will sometimes be simply referred to as glass.
[0026] Optical Glass
[0027] The composition range of each component (ingredient) constituting the optical glass of the present invention is described below. In this specification, unless otherwise specified, the content of a cationic component is expressed as the molar percentage (mol%) of the cation to all cationic components, and the content of anionic components is expressed as the molar percentage (mol%) of the anion to all anionic components; the ratio between the contents of cationic components is the ratio of the molar percentage contents of each cationic component.
[0028] Unless otherwise specified in the specific context, the numerical ranges listed herein include upper and lower limits. "Above" and "below" include endpoint values and all integers and fractions included within the range, but are not limited to the specific values listed when the range is defined. The term "and / or" as used herein is inclusive; for example, "A and / or B" means either only A, or only B, or both A and B.
[0029] It should be noted that the ionic valences of the components described below are representative values used for convenience and are not distinguishable from the ionic valences of other components. The ionic valences of the components in optical glass may exist beyond these representative values. For example, phosphorus (P) typically exists in glass with a +5 valence, therefore it is referred to as "P" in this disclosure. 5+ "As a representative value, but there is a possibility that it exists in other ionic valence states, which is also within the scope of protection of this disclosure."
[0030] <Catonic Components>
[0031] P 5+This component is a constituent of the optical glass of the present invention, and it has the function of suppressing devitrification and density increase. When its content is below 7%, the devitrification resistance of the glass decreases and the density increases; when its content exceeds 27%, the Abbe number of the glass decreases and the cost increases. Therefore, P in the present invention... 5+ The content is 7-27%, preferably 11-24%, and more preferably 15-20%.
[0032] Al 3+ It can improve the stability of glass, effectively enhance its processability and chemical stability, and increase viscosity during glass forming. When Al 3+ When the content of Al is less than 10%, a stable glass framework cannot be formed and the above-mentioned effects cannot be obtained; when Al 3+ When the Al content exceeds 45%, the glass transition temperature and liquidus temperature increase, making melting more difficult and increasing the forming temperature, leading to accelerated glass volatilization, worsening the glass striations, and hindering large-diameter forming. Furthermore, excessively high transition temperatures make molding difficult. Therefore, in this invention, Al... 3+ The content is 10-45%, preferably 18-40%, and more preferably 24-35%.
[0033] Ba 2+ Ba can improve the refractive index, thermal stability, and weather resistance of glass, but excessive Ba can lead to problems. 2+ This leads to increased glass density and decreased abrasion resistance, and reduces viscosity, resulting in poorer striations during molding, making it difficult to obtain large-diameter, high-quality optical glass. Therefore, in this invention, Ba... 2+ The content is 5-25%, preferably 9-21%, and more preferably 12-19%.
[0034] Sr 2+ It can reduce the coefficient of thermal expansion of glass and effectively adjust its refractive index and density, increase its viscosity, and improve forming streaks. However, if its content is too high, the glass's devitrification resistance and chemical stability will decrease. Therefore, in this invention, Sr... 2+ The content is 5-25%, preferably 8-21%, and more preferably 11-17%.
[0035] Ca 2+ It increases the viscosity of glass, improves forming striations, and enhances the chemical stability and grinding performance of glass. However, if its content is too high, the glass refractive index may not meet design requirements, and it may lead to a deterioration in devitrification resistance. Therefore, in this invention, Ca... 2+ The content is 5-30%, preferably 10-25%, and more preferably 15-20%.
[0036] Through extensive research, the inventors discovered that in some implementation methods, by controlling (Ba 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ A ratio above 2.0 can effectively control the viscosity of molten glass during the forming stage, increase the stability of the glass, and obtain large-diameter optical glass with good striation patterns; however, when (Ba... 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ When the viscosity is greater than 4.6, the devitrification resistance of the glass decreases sharply, making it difficult to form. Therefore, (Ba) is preferred. 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ The value is 2.0 to 4.6, more preferably 2.5 to 4.1, and even more preferably 3.0 to 3.9.
[0037] Mg 2+ It can improve the abrasion resistance of glass, increase its viscosity, and improve forming striations; however, when its content exceeds 15%, the thermal stability of the glass decreases significantly. Therefore, in this invention, Mg... 2+ The content is 0-15%, preferably 0-10%, and more preferably 0-5%.
[0038] In some implementations, by controlling Mg 2+ The content of Al 3+ The ratio between the contents of Mg 2+ / Al 3+ At concentrations below 0.5, Mg can improve the glass's resistance to crystallization, resulting in superior glass production performance. Therefore, Mg is preferred. 2+ / Al 3+ The value is 0 to 0.5, more preferably Mg. 2+ / Al 3+ The value is 0-0.3, with Mg being the preferred option. 2+ / Al 3+ The range is 0 to 0.1.
[0039] Through extensive experimental research, the inventors discovered that in some implementation methods, by controlling AI... 3 The maximum content is 45% with Al 3+ The difference in actual content is 45% - Al 3+ With Mg 2+ The maximum content is 15% with Mg 2+ The difference of 15% between the actual content and Mg content 2+ The ratio between (45% - Al) 3+ ) / (15%-Mg 2+This can effectively control the thermal stability (anti-crystallization performance) of glass during reheating. When (45% Al) 3+ ) / (15%-Mg 2+ When the temperature is below 5.0, the thermal stability of the glass can be significantly optimized, enabling stable large-diameter molding; however, when (45%-Al) 3+ ) / (15%-Mg 2+ When the concentration of Al is less than 0.3, the glass's resistance to crystallization deteriorates, the liquidus temperature increases, and the glass production becomes more difficult. Therefore, (45% Al) is preferred. 3+ ) / (15%-Mg 2+ The concentration is 0.3 to 5.0, more preferably (45%-Al). 3 + ) / (15%-Mg 2+ The content of (45%-Al) is 0.4-4.0, with (45%-Al) being a further preferred value. 3+ ) / (15%-Mg 2+ The concentration is 0.5–3.0, with a further preferred concentration of (45%-Al). 3+ ) / (15%-Mg 2+ The value ranges from 0.6 to 2.0.
[0040] Al 3+ Mg 2+ In fluorophosphate glass, it plays a role in forming a network and increasing the viscosity of the molten glass, but it also leads to an increase in the temperature of the glass melt. 2+ It is possible to improve the devitrification resistance of molten glass while adjusting its viscosity. Therefore, in some embodiments, when Al 3+ +Mg 2+ with Ba 2+ The ratio (Al) 3+ +Mg 2+ ) / Ba 2+ At viscosities below 3.5, fluorophosphate glasses with suitable viscosity and good devitrification resistance can be obtained; when (Al) 3+ +Mg 2+ ) / Ba 2+ When the viscosity is less than 1.5, the glass melt viscosity is too low, resulting in a narrower forming range and poorer striations, which is detrimental to large-diameter forming. Therefore, (Al) is preferred. 3+ +Mg 2+ ) / Ba 2+ The value is 1.5 to 3.5, more preferably (Al). 3+ +Mg 2+ ) / Ba 2+ The value is 2.0 to 3.0, and further optimization is needed (Al). 3+ +Mg 2+ ) / Ba 2+ It ranges from 2.3 to 2.7.
[0041] Y 3+ It can increase the refractive index of glass and reduce the coefficient of thermal expansion. However, if its content exceeds 10%, the liquidus temperature of the glass rises, its devitrification resistance decreases, and its material properties become shorter, making it more difficult to control large-diameter forming. Therefore, Y 3+ The content is 0-10%, preferably 0-5%, and more preferably 0-3%.
[0042] La 3+ It has the effect of increasing the refractive index of glass and improving its acid resistance. 3+ When the content of La is too high, the thermal stability and devitrification resistance of the glass decrease, and the glass is prone to devitrification during the manufacturing process. Therefore, in this invention, La... 3+ The content is 0-10%, preferably 0-5%, and more preferably 0-2%.
[0043] Gd 3+ It can improve the stability of glass, maintain low dispersion while appropriately increasing the refractive index, and also appropriately increase mechanical strength and reduce the coefficient of thermal expansion. However, if its content exceeds 10%, the glass's devitrification resistance decreases. Therefore, Gd... 3+ The content is 0-10%, preferably 0-5%, and more preferably 0-3%.
[0044] R + (R + For Li + Na + K + One or more of these can effectively reduce the glass transition temperature, but R + A content greater than 10% will cause the glass liquid phase temperature to rise, while the viscosity will decrease, making forming difficult. Therefore, R + The content of [R] is 0-10%, preferably 0-6%, and more preferably 0-3%. In some embodiments, it is further preferred that it does not contain [R]. + .
[0045] Extensive experimental research has revealed that in some implementation methods, when Al 3+ The maximum content is 45% with Al 3+ The difference in actual content is 45% - Al 3+ With the easily crystallizable component Gd 3+ Y 3+ La 3+ Li + Total content of Gd 3+ +Y 3+ +La 3+ +Li + The ratio between (45% - Al) 3+ ) / (Gd 3+ +Y 3+ +La3+ +Li + When the (45%-Al) value is greater than 2.0, it is easier to obtain glass with low crystallization tendency and good stripe pattern; however, when (45%-Al) 3+ ) /
[0046] (Gd 3+ +Y 3+ +La 3+ +Li + When the chromaticity of the glass exceeds 80.0, the coloring intensity increases, but the stripe pattern deteriorates, making it even difficult to form. Therefore, (45% Al) is preferred. 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value is 2.0 to 80.0, more preferably (45%-Al). 3+ ) / (Gd 3 + +Y 3+ +La 3+ +Li + The value is 6.0–50.0, with (45%-Al) being further preferred. 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value ranges from 8.0 to 35.0.
[0047] In some implementations, by controlling Al 3+ The content of Mg 2+ Li + Difference in content Al 3+ -Mg 2+ -Li + With P 5+ The ratio between the contents of Al 3+ -Mg 2+ -Li + ) / P 5+ Within the range of 0.5 to 2.5, the desired optical properties can be obtained more easily while improving the glass's resistance to crystallization. Therefore, (Al) is preferred. 3+ -Mg 2+ -Li + ) / P 5+ The value is 0.5 to 2.5, more preferably (Al). 3+ -Mg 2 + -Li + ) / P 5+ The value is 1.0 to 2.3, and further optimization is preferred (Al). 3+ -Mg 2+ -Li+ ) / P 5+ It ranges from 1.3 to 2.1.
[0048] In the optical glass of this invention, Sb containing less than 1% can be used. 3+ Sb is preferred as a clarifying agent to improve the clarification effect of glass. 3+ The content is 0-0.5%, more preferably 0-0.3%.
[0049] Without compromising the excellent properties of the glass of the present invention, the optical glass of the present invention may contain, as needed, elements such as Ta. 5+ W 6+ 、Ge 4+ Bi 3+ Te 4+ Other components.
[0050] <Anionic components>
[0051] F - It plays a significant role in reducing the refractive index, temperature coefficient of refractive index, and transition temperature of glass, and is an important component for improving the Abbe number and anomalous dispersion. If F - Excessive F content weakens the stability of glass, increases the coefficient of thermal expansion and abrasion, especially during the melting process. - The volatilization of these substances not only pollutes the environment but also causes the optical constants of the glass to exceed their design limits. If F... - If the content is less than 50%, it is difficult to obtain the designed Abbe number and abnormal dispersion; if F - If the content of [amount] exceeds 90%, the Abbe number of the glass will become excessively high, and volatilization will increase dramatically during melting and precision molding. Therefore, F [content] - The content is 50-90%, preferably 60-80%, and more preferably 67-75%.
[0052] The optical glass of this invention contains O 2- Especially through the presence of more than 10% O 2- It can achieve excellent optical performance and low wear, if O 2- When the content of O is greater than 50%, the liquidus temperature of the glass rises rapidly. Therefore, O 2- The content is 10-50%, preferably 20-40%, and more preferably 25-33%.
[0053] In the optical glass of this invention, less than 1% Cl can be used. - Cl is preferred as a clarifying agent to improve the clarification effect of glass. - The content is 0-0.5%, more preferably 0-0.3%.
[0054] <Ingredients that should not be present>
[0055] Other components not mentioned above can be added as needed without compromising the excellent properties of the glass of the present invention. However, transition metal components such as Ce, V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo, even when contained in small amounts individually or in combination, can color the glass and cause absorption at specific wavelengths in the visible light region, thereby weakening the visible light transmittance improvement effect of the present invention. Therefore, it is preferable that the above-mentioned components are not actually present, especially for optical glass where transmittance in the visible light region is required.
[0056] The cations Pb, Th, Cd, Tl, Os, Be, and Se have been increasingly subject to controlled use in recent years due to their status as hazardous chemicals. Environmental protection measures are essential not only in glass manufacturing but also in processing and post-product disposal. Therefore, given the importance of environmental impact, it is preferable to ideally contain virtually none of these substances, except where their contamination is unavoidable. Consequently, the optical glass becomes virtually free of pollutants. Therefore, the optical glass of this invention can be manufactured, processed, and disposed of even without specific environmental countermeasures.
[0057] The terms "not containing" and "0%" as used herein mean that the component or the like was not intentionally added as a raw material to the optical glass of this invention; however, as raw materials and / or equipment used in the production of optical glass, there may be certain impurities or components that are not intentionally added, which may be present in small or trace amounts in the final optical glass, and such cases are also within the scope of protection of this patent.
[0058] The performance of the optical glass of the present invention will now be described.
[0059] <Refractive Index and Abbe Number>
[0060] The refractive index (n) of optical glass d ) and Abbe number (ν d Test according to the method specified in GB / T 7962.1—2010.
[0061] In some embodiments, the refractive index (n) of the optical glass of the present invention d The preferred refractive index (n) is 1.46–1.52. d The refractive index (n) is 1.47–1.51, more preferably 1.47–1.51. d The value is 1.48 to 1.50.
[0062] In some embodiments, the Abbe number (ν) of the optical glass of the present invention d The optimal Abbe number is 81-89. d The Abbe number is 83-88, and more preferably ν. dThe value is 84-87.
[0063] <Colorization>
[0064] The short-wavelength transmission spectral characteristics of the optical glass of this invention are expressed using chromaticity (λ). 80 / λ5) represents. λ 80 λ5 refers to the wavelength corresponding to a glass transmittance of 80%, while λ6 refers to the wavelength corresponding to a glass transmittance of 5%. Where λ... 80 The measurement was performed using a glass with a thickness of 10 ± 0.1 mm and two optically polished, parallel planes. The spectral transmittance was measured in the wavelength range from 280 nm to 700 nm, and wavelengths exhibiting 80% transmittance were recorded. Spectroscopic transmittance, or transmittance, refers to the transmittance of light incident perpendicularly to the aforementioned surface of the glass at wavelengths of intensity I. in Light, passing through the glass and emitted from another plane, has an intensity of I. out In the case of light, through I out / I in The quantity represented also includes the transmittance of the glass due to surface reflection loss on the aforementioned surface. In the glass of the present invention, λ 80 A small value means that the glass itself has very little coloration. The same applies to λ5.
[0065] In some embodiments, the λ of the optical glass of the present invention 80 340 nm or less, preferably λ 80 Less than or equal to 335nm, preferably λ 80 λ is less than or equal to 330 nm, and is further preferred. 80 λ is preferred to be less than or equal to 325nm. 80 Less than or equal to 320nm.
[0066] In some embodiments, the λ5 of the optical glass of the present invention is less than or equal to 265 nm, preferably less than or equal to 260 nm, more preferably less than or equal to 255 nm, even more preferably less than or equal to 250 nm, and even more preferably less than or equal to 245 nm.
[0067] <Density>
[0068] The density (ρ) of optical glass is tested according to the method specified in GB / T 7962.20-2010, and is the mass per unit volume at a temperature of 20℃, expressed in g / cm³. 3 express.
[0069] In some embodiments, the density (ρ) of the optical glass of the present invention is 3.90 g / cm³. 3 The preferred value is 3.82 g / cm³. 3 The preferred value is 3.78 g / cm³.3 The following is a further preferred value: 3.74 g / cm³ 3 the following.
[0070] <Transition Temperature>
[0071] Transition temperature of optical glass (T) g Test according to the method specified in GB / T 7962.16-2010.
[0072] In some embodiments, the transition temperature (T) of the optical glass of the present invention is... g The temperature is below 500°C, preferably below 490°C, and more preferably below 480°C.
[0073] <Acid resistance>
[0074] The acid resistance stability (RA) (surface method) of optical glass was tested according to the method specified in GB / T 7962.14-2010.
[0075] In some embodiments, the acid resistance (RA) of the optical glass of the present invention is Class 3 or above, preferably Class 2 or above.
[0076] Moisture resistance stability
[0077] The moisture resistance stability (RC) (surface method) of optical glass was tested according to the method specified in GB / T 7962.15-2010.
[0078] In some embodiments, the moisture resistance stability (RC) of the optical glass of the present invention is Class 2 or above, preferably Class 1.
[0079] <Stripe>
[0080] Glass is formed to a size of 200mm wide and 30mm thick, and then cut into pieces every 360mm in length to obtain glass blanks. The blanks are then sized as follows: width × thickness × length 200mm × 30mm × 360mm. These glass blanks are processed into samples with a width × thickness × length of 200mm × 30mm × 80mm, and both ends of the sample are polished along its length to obtain a stripe test sample.
[0081] The striae of the glass are checked by comparing it with a standard sample from the direction in which the striae are most easily visible using a striameter consisting of a point light source and a lens. The striae are divided into 4 levels, as detailed in Table 1 below.
[0082] Table 1. Stripe Grading Table
[0083] grade stripe intensity A Under the specified testing conditions, there are no visible streaks inside, and the edge streaks are <2mm. B Under the specified testing conditions, there are no visible streaks inside, and the edge streaks are 2-4mm. C Slight parallel streaks are present under the specified testing conditions. D Under the specified testing conditions, there are coarse parallel stripes.
[0084] In some embodiments, when the glass forming thickness is greater than 20 mm, the striation of the optical glass of the present invention is grade C or above, preferably grade B or above, and more preferably grade A, exhibiting excellent large-diameter forming performance.
[0085] Anti-crystallization properties
[0086] The method for testing the anti-crystallization performance of the optical glass of this invention is as follows: A 10mm×20mm×20mm glass sample is placed inside a semi-circular ceramic box with a radius of 15mm and a depth of 15mm. The glass sample and the ceramic box are then placed in a T... g The initial heating was performed in a test furnace at +(140~160℃) for 15 minutes, followed by removal and cooling to 200℃ in a tunnel annealing furnace; subsequently, the temperature was stabilized at a set holding temperature of T. g The glass sample was heated a second time in a test furnace at 140–160°C for 15 minutes, then removed and cooled again to 200°C in a tunnel annealing furnace. After the second heating, the glass sample and ceramic box were placed in the tunnel annealing furnace and cooled to 200°C. The glass sample was then removed and allowed to cool naturally to room temperature in an atmospheric environment. After grinding and polishing, the overall softening and devitrification of the glass were observed visually, and the presence of crystallized particles was confirmed by microscopic observation of the interior of the glass. The anti-crystallization performance of the glass was judged according to Table 2 below, with Grade A being the best and Grade E being the worst.
[0087] Table 2. Grading and Judgment Criteria for Anti-crystallization Performance
[0088]
[0089] In some embodiments, the optical glass of the present invention has an anti-crystallization performance of grade D or above, preferably grade C or above, more preferably grade B, and even more preferably grade A, and has excellent thermal stability suitable for large-diameter molding.
[0090] [Manufacturing methods for optical glass]
[0091] The manufacturing method of the optical glass of this invention is as follows: The optical glass of this invention is produced using conventional raw materials and conventional processes. Carbonates, nitrates, sulfates, phosphates, oxides, fluorides, metaphosphates, etc., are used as raw materials. After being batched according to conventional methods, the batched material is melted in a melting furnace at 900–1000°C. After clarification and thorough homogenization, it is cast or punched at a temperature below 800°C to obtain the optical glass of this invention. Those skilled in the art can appropriately select raw materials, process methods, and process parameters according to actual needs.
[0092] [Glass preforms and optical components]
[0093] Glass preforms can be manufactured from the optical glass using methods such as grinding, hot pressing, or precision stamping. Specifically, glass preforms can be manufactured by machining the optical glass, such as grinding and polishing; or by hot pressing a preform made from the optical glass for molding and then grinding it; or by precision stamping a preform made from the ground glass.
[0094] It should be noted that the means of preparing the glass preform are not limited to those described above. As mentioned above, the optical glass of the present invention is useful for various optical components and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention, using the preform for re-hot pressing, precision stamping, etc., to manufacture optical components such as lenses and prisms.
[0095] Both the glass preform and the optical element of the present invention are formed from the optical glass described above. The glass preform of the present invention possesses the excellent properties of optical glass, and the optical element of the present invention possesses the excellent properties of optical glass. Examples of lenses include various lenses such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses, whose lens surfaces are spherical or aspherical.
[0096] [Optical Instruments]
[0097] The optical elements formed by the optical glass of this invention can be used to manufacture optical instruments such as photographic equipment, video equipment, display equipment, and monitoring equipment.
[0098] Example
[0099] <Example of Optical Glass>
[0100] To further illustrate and explain the technical solution of the present invention, the following non-limiting embodiments are provided.
[0101] In this embodiment, optical glass with the composition shown in Tables 3 to 5 was obtained using the optical glass manufacturing method described above. Furthermore, the properties of each glass were measured using the testing method described in this invention, and the measurement results are shown in Tables 3 to 5.
[0102] Table 3.
[0103]
[0104]
[0105] Table 4.
[0106]
[0107]
[0108] Table 5.
[0109]
[0110]
[0111] <Example of Glass Prefabricated Components>
[0112] The glass obtained from Examples 1 to 22# of optical glass is used for molding processes such as grinding, hot pressing, and precision stamping to produce preforms of various lenses and prisms, including concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. Under the original molding process, the molded products do not contain crystal particles, greatly improving molding efficiency and product yield.
[0113] <Optical Component Examples>
[0114] Annealing these preforms obtained from the above glass preform examples reduces internal stress in the glass while fine-tuning the refractive index, so that optical properties such as the refractive index reach the desired values.
[0115] Next, the prefabricated parts are ground and polished to produce various lenses and prisms, such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. Anti-reflective coatings can also be applied to the surface of the resulting optical elements.
[0116] The optical glass obtained in Examples 1 to 22# is cut into predetermined sizes, and large-diameter, high-quality optical components are obtained by performing optical cold processing processes such as grinding and polishing on the blanks. An anti-reflective film can also be coated on the surface of the obtained optical components.
[0117] <Examples of Optical Instruments>
[0118] The optical elements obtained from the above-described optical element embodiments can be used, through optical design, to form optical components or optical assemblies by using one or more optical elements. These components can be used in, for example, imaging devices, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices that include such circuits and chips.
Claims
1. Optical glass, characterized in that, Its components are expressed as mole percentages, and the cationic component contains: P 5+ 7-27%; Al 3 + : 10~45%; Ba 2+ 5-25%; Sr 2+ 5-25%; Ca 2+ 5-30%, (45%-Al) 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value ranges from 7.46 to 80.
0. (Al) 3+ -Mg 2+ -Li + ) / P 5+ The value ranges from 1.34 to 2.1 (45%-Al). 3+ ) / (15%-Mg 2+ The value ranges from 0.3 to 1.
23. The anionic component contains: F - 67-75%; O 2- The refractive index n of the optical glass is 25-33%. d The Abbe number ν ranges from 1.47953 to 1.
52. d The value is 81-89, the striation is grade B or above, the resistance to crystallization is grade A, and the transformation temperature T g It is below 481℃.
2. The optical glass according to claim 1, characterized in that, Its components are expressed as mole percentages, and the cationic component also contains: Mg 2+ : 0–15%; and / or Y 3+ : 0–10%; and / or La 3+ : 0–10%; and / or Gd 3+ : 0–10%; and / or R + : 0–10%; and / or Sb 3+ :0~1%, the R + For Li + Na + K + One or more of them.
3. The optical glass according to claim 1, characterized in that, Its components are expressed as mole percentages, and the anionic components also contain: Cl - : 0~1%.
4. Optical glass, characterized in that, Its components are expressed as mole percentages, with the cationic component consisting of P 5+ 7-27%; Al 3+ : 10~45%; Ba 2+ 5-25%; Sr 2+ 5-25%; Ca 2+ 5-30%; Mg 2+ : 0~15%; Y 3+ : 0~10%; La 3+ : 0~10%; Gd 3+ : 0~10%; R + : 0~10%; Sb 3+ Composition: 0-1%, (45%-Al) 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + The value ranges from 7.46 to 80.
0. (Al) 3+ -Mg 2+ -Li + ) / P 5+ The value ranges from 1.34 to 2.1 (45%-Al). 3+ ) / (15%-Mg 2+ The value of R is 0.3 to 1.
23. + For Li + Na + K + One or more of them, the anionic component is F - 67-75%; O 2- : 25~33%; Cl - Composition: 0-1% of the optical glass, wherein the refractive index n d The Abbe number ν ranges from 1.47953 to 1.
52. d The value is 81-89, the striation is grade B or above, the resistance to crystallization is grade A, and the transformation temperature T g It is below 481℃.
5. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages and satisfy one or more of the following four conditions: 1) (Ba 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ is 2.0 to 4.6; 2)(45%-Al 3+ ) / (15%-Mg 2+ The value ranges from 0.4 to 1.
23. 3)(Al) 3+ +Mg 2+ ) / Ba 2+ The value is 1.5 to 3.
5. 4) (45%-Al 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + ) is 8.0 to 50.
0.
6. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages and satisfy one or more of the following four conditions: 1) (Ba 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ is 2.5 to 4.1; 2)(45%-Al 3+ ) / (15%-Mg 2+ The value ranges from 0.5 to 1.
23. 3)(Al) 3+ +Mg 2+ ) / Ba 2+ The value is 2.0 to 3.
0. 4) (45%-Al 3+ ) / (Gd 3+ +Y 3+ +La 3+ +Li + ) is 8.0 to 35.
0.
7. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages and satisfy one or more of the following four conditions: 1) (Ba 2+ +Sr 2+ +Ca 2+ ) / Ba 2+ is 3.0 to 3.9; 2)(45%-Al 3+ ) / (15%-Mg 2+ The values range from 0.6 to 1.
23. 3)(Al) 3+ +Mg 2+ ) / Ba 2+ It ranges from 2.3 to 2.
7.
8. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, of which: Mg 2+ / Al 3+ The range is 0 to 0.
5.
9. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, of which: Mg 2+ / Al 3+ The range is 0 to 0.
3.
10. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, of which: Mg 2+ / Al 3+ The range is 0 to 0.
1.
11. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, where: P 5+ : 11–24%; and / or Al 3+ : 18–40%; and / or Ba 2+ : 9–21%; and / or Sr 2+ : 8–21%; and / or Ca 2+ 10–25%; and / or Mg 2+ : 0–10%; and / or Y 3+ : 0–5%; and / or La 3+ : 0–5%; and / or Gd 3+ : 0–5%; and / or R + : 0–6%; and / or Sb 3+ : 0~0.5%, the R + For Li + Na + K + One or more of them.
12. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, where: P 5+ 15-20%; and / or Al 3+ 24–35%; and / or Ba 2+ : 12-19%; and / or Sr 2+ : 11-17%; and / or Ca 2 + 15-20%; and / or Mg 2+ : 0–5%; and / or Y 3+ : 0–3%; and / or La 3+ : 0–2%; and / or Gd 3+ : 0–3%; and / or R + : 0–3%; and / or Sb 3+ : 0~0.3%, the R + For Li + Na + K + One or more of them.
13. The optical glass according to any one of claims 1 to 4, characterized in that, Does not contain R + The R + For Li + Na + K + One or more of them.
14. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, of which: Cl - : 0~0.5%.
15. The optical glass according to any one of claims 1 to 4, characterized in that, Its components are expressed as mole percentages, of which: Cl - : 0~0.3%.
16. The optical glass according to any one of claims 1 to 4, characterized in that, The refractive index n of the optical glass d The values range from 1.47953 to 1.51; the Abbe number ν d It ranges from 83 to 88.
17. The optical glass according to any one of claims 1 to 4, characterized in that, The refractive index n of the optical glass d The Abbe number is 1.48–1.
50. d It ranges from 84 to 87.
18. The optical glass according to any one of claims 1 to 4, characterized in that, The λ of the optical glass 80 Less than or equal to 340 nm; and / or λ5 less than or equal to 265 nm; and / or density ρ is 3.90 g / cm³. 3 The following; and / or transition temperature T g Temperature below 480℃; and / or acid resistance (RA) of class 3 or above; and / or moisture resistance (RC) of class 2 or above; and / or streaking grade A.
19. The optical glass according to any one of claims 1 to 4, characterized in that, The λ of the optical glass 80 Less than or equal to 335 nm; and / or λ5 less than or equal to 260 nm; and / or density ρ is 3.82 g / cm³. 3 The following are acceptable: acid resistance (RA) is Class 2 or above; and / or moisture resistance (RC) is Class 1.
20. The optical glass according to any one of claims 1 to 4, characterized in that, The λ of the optical glass 80 Less than or equal to 330 nm; and / or λ5 less than or equal to 255 nm; and / or density ρ is 3.78 g / cm³. 3 the following.
21. The optical glass according to any one of claims 1 to 4, characterized in that, The λ of the optical glass 80 Less than or equal to 325nm; and / or λ5 less than or equal to 250nm.
22. The optical glass according to any one of claims 1 to 4, characterized in that, The λ of the optical glass 80 Less than or equal to 320nm; and / or λ5 less than or equal to 245nm.
23. A glass preform, characterized in that, It is made of the optical glass described in any one of claims 1 to 22.
24. An optical element, characterized in that, It is made of optical glass as described in any one of claims 1 to 22, or of glass preform as described in claim 23.
25. An optical instrument, characterized in that, It contains the optical glass according to any one of claims 1 to 22, and / or contains the optical element according to claim 24.
Citation Information
Patent Citations
Fluorophosphate glass, glass material for press molding, optical element blank, optical element and methods of manufacuring the same
CN103183471A
Optical glass, optical prefabricated member and optical element
CN106145668A
Optical glass, optical preform and optical element
CN107540214A
Glass, glass material for press molding, optical element blank, and optical element
JP2016113307A