K + Response-type hydrogel strain sensor and rapid and convenient quantitative detection method for trace blood potassium

By combining a K+ responsive hydrogel strain sensor with a resistance strain gauge, rapid and accurate detection of serum potassium concentration under trace serum sample conditions was achieved, solving the problem of blood sample detection in existing technologies and possessing the advantages of high efficiency, convenience and economy.

CN120063099BActive Publication Date: 2026-11-17SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510360237.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-25
Publication Date
2026-11-17
Estimated Expiration
2045-03-25

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve rapid and accurate quantitative detection of serum potassium concentration in blood samples, and existing hydrogel sensors suffer from insufficient response efficiency and mechanical properties, failing to meet the demands for high-efficiency detection.

Method used

A K+ responsive hydrogel strain sensor is employed, which consists of a K+ responsive hydrogel layer and a resistance strain gauge. The hydrogel layer is chemically bonded to the resistance strain gauge substrate, and a gel network is formed by physical cross-linking of Laponite XLG nanosheets. This network is then combined with a surface-silanized modified synthetic resin substrate to achieve rapid identification and signal transduction of serum potassium.

Benefits of technology

It enables rapid (within 2-4 minutes) quantitative detection of serum potassium concentration under trace serum sample conditions (16-20 μL), with high sensitivity and strong anti-interference ability. It is suitable for convenient testing in homes and primary healthcare units, reducing testing costs and complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120063099B_ABST
    Figure CN120063099B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of biomedical sensors and blood potassium detection, and provides K + A responsive hydrogel strain sensor and a rapid and convenient quantitative detection method for trace amounts of blood potassium. The K... + Response hydrogel strain sensor by K + It consists of a responsive hydrogel layer and a resistance strain gauge. The resistance strain gauge includes a substrate and a sensitive grid wire. The substrate is a surface-silanized modified synthetic resin substrate; K + The responsive hydrogel layer is chemically bonded to the substrate and completely covers the sensitive grid wire; the K + The responsive hydrogel layer's gel polymer network is formed by physical cross-linking of linear polymer poly(N-isopropylacrylamide-co-4-acrylamide benzo-15-crown-5) with physical cross-linking agent Laponite XLG nanosheets. Based on this strain sensor, this invention also provides a rapid and convenient quantitative detection method for trace amounts of serum potassium. This invention can achieve serum potassium detection with trace amounts of serum sample. + Rapid detection of concentration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomedical sensors and blood potassium detection, and relates to K. + A responsive hydrogel strain sensor and a rapid and convenient quantitative detection method for trace amounts of blood potassium. Background Technology

[0002] Potassium ions (K) + K+ is a major cation that maintains cellular physiological activities, playing a crucial role in maintaining electrolyte balance, nerve impulse transmission, and muscle contraction. Human serum K+ + The normal range for K concentration is 3.5–5.5 mmol / L. + When levels are abnormal, whether it is hyperkalemia (serum potassium) + >5.5 mmol / L) or hypokalemia (serum K) + A potassium level <3.5 mmol / L can lead to serious health problems. Hyperkalemia is commonly seen in cases of kidney failure and excessive intracellular potassium release, and may cause arrhythmias, decreased myocardial contractility, or even cardiac arrest; while hypokalemia can cause symptoms such as muscle weakness, increased heart rate, and paralytic ileus.

[0003] Currently, serum potassium is being tested. + Methods for determining concentration include spectroscopic, chemical, and electrochemical methods. Spectroscopic methods include flame atomic absorption spectrometry (FAAS), graphite furnace atomic absorption spectrometry (GFAAS), and Raman scattering spectroscopy (RSS). These methods detect concentrations by analyzing the spectral information of atoms' absorption or scattering characteristics at specific wavelengths of light, offering high sensitivity. However, spectroscopic methods require complex and expensive precision instruments and rely on highly trained professionals, making them inconvenient in practical applications. Furthermore, the detection process is complex and requires large sample volumes; for example, flame atomic absorption spectrometry requires complex sample pretreatment steps and more than 2 mL of serum sample. Chemical methods are based on the fundamental principles of specific chemical reactions. For example, serum potassium... + Concentration can be detected by the sodium tetraphenylborate method, which utilizes the reaction of sodium tetraphenylborate with K + A chemical reaction occurs, forming a precipitate, which causes a change in the turbidity of the solution. The serum potassium level can be calculated by measuring this change in turbidity. + The concentration of K. The electrochemical method utilizes an ion-selective electrode (ISE) to determine K by measuring the change in membrane potential between the blood sample and the electrode caused by a specific chemical reaction. + Although this method has high sensitivity, its detection accuracy is easily affected by other ions in the sample, and it requires high sample pretreatment.

[0004] Polymer materials, especially smart polymer hydrogels, have attracted researchers' attention due to their significant stimuli-responsiveness, excellent flexibility, and remarkable plasticity. Typically, by incorporating K-type polymers into the polymer matrix, specific K-type hydrogels can be identified. + Functional groups (such as crown ether 15-crown-5) can enable the detection of K using polymer materials. + The concentration is [missing information]. Currently, linear polymer poly(N-isopropylacrylamide-cobenzo-15-crown-5-acrylamide) is used to detect serum K [missing information]. + Reporting of concentrations. Identification of K under isothermal conditions. + Subsequently, the linear polymer changes from an expanded state to a contracted state, leading to a change in the solution's transmittance. This is necessary for the quantitative detection of potassium in serum. + Concentration requires precise measurement of the solution's transmittance; however, solution transmittance is always difficult to observe, and its measurement sensitivity is relatively low. Crosslinking polymers to form hydrogels allows for the measurement of the hydrogel's transmittance in identifying K+. + The subsequent volume shrinkage can be used to quantitatively detect serum K. + Concentration can overcome the limitations of linear polymers at K0 + There are shortcomings in detection. Currently, the measurement of hydrogel volume shrinkage is achieved through signal conversion by a hydrogel grating sensor. When the smart hydrogel interacts with K... + Upon contact, the height of the hydrogel grating changes at the nanometer scale, leading to a change in diffraction efficiency. However, since the hydrogel grating sensor uses diffracted light as the detection signal, maintaining the transparency of the hydrogel grating is necessary to ensure accurate detection. But for blood sample detection, the transparency of the hydrogel grating is inevitably affected by substances in the blood sample; therefore, using diffracted light as the detection signal is not suitable for detecting K+ in blood samples. + Concentration determination.

[0005] Furthermore, given the crucial role of hydrogel deformation in signal transduction, there is a significant demand in practical applications for hydrogels that can achieve both effective stimulus responses and robust mechanical properties. Existing stimulus-responsive hydrogels are typically prepared through chemical crosslinking (e.g., using N,N'-methylenebisacrylamide, 4-arm polyethylene glycol acrylamide, etc.). These chemical crosslinking agents usually form stable three-dimensional hydrogel networks through covalent bonds generated by free radical polymerization. Hydrogels prepared via chemical crosslinking often exhibit high crosslinking density, which increases Kc. + Spatial barriers to transport and restriction of molecular chain mobility result in lower response efficiency and mechanical properties of hydrogels, which is detrimental to K. + Highly efficient detection. In summary, the development of a rapid quantitative detection method for K in small-volume serum samples is crucial. + Concentration-based methods still face significant challenges. Summary of the Invention

[0006] Existing methods for signal conversion using hydrogel gratings are difficult to apply to K+ in blood samples. + The problems with quantitative detection, and the shortcomings of existing responsive hydrogels prepared based on chemical crosslinking agents in terms of response efficiency and mechanical properties, which are detrimental to K. + To address the problem of efficient detection, this invention provides K + A responsive hydrogel strain sensor and a rapid and convenient quantitative detection method for trace serum potassium levels were developed to achieve serum potassium detection with minimal serum sample volume. + Rapid detection of concentration.

[0007] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0008] A type of K + A responsive hydrogel strain sensor, which is composed of K + The system consists of a responsive hydrogel layer and a resistance strain gauge. The resistance strain gauge includes a substrate, a sensitive grid wire, a capping layer, and leads. The substrate is a surface-silanized modified synthetic resin substrate; K + The responsive hydrogel layer is chemically bonded to the substrate and completely covers the sensitive grid wire of the resistance strain gauge; the K + The responsive hydrogel layer is formed by physical crosslinking of linear polymer poly(N-isopropylacrylamide-co-4-acrylamidebenzo-15-crown-5) with physical crosslinking agent Laponite XLG nanosheets.

[0009] The above K + In the technical solution of responsive hydrogel strain sensors, K + The responsive hydrogel layer is made of K + Response hydrogel composition, K + The preferred content of Laponite XLG nanosheets in the responsive hydrogel is 0.01–0.05 mol / L.

[0010] Furthermore, the aforementioned K + In the technical solution of the responsive hydrogel strain sensor, the K +The responsive hydrogel layer is obtained by photoinitiated polymerization of a gel prepolymer solution. The gel prepolymer solution is obtained by fully dispersing the functional monomer 4-acrylamide benzo-15-crown-5, the gel monomer N-isopropylacrylamide, and a photoinitiator in a Laponite XLG nanosheet dispersion. In the gel prepolymer solution, the molar ratio of benzo-15-crown-5-acrylamide to N-isopropylacrylamide is (0.05–0.2):1, and the concentration of N-isopropylacrylamide monomer is 0.5–2 mol / L. Furthermore, the Laponite XLG nanosheet dispersion is obtained by fully dispersing Laponite XLG nanosheets in water, and the preferred concentration of Laponite XLG nanosheets in the dispersion is 0.01–0.05 mol / L.

[0011] Furthermore, the aforementioned K + In the technical solution of the responsive hydrogel strain sensor, the photoinitiator in the gel prepolymer solution plays a role in initiating the copolymerization reaction between the functional monomer 4-acrylamide benzo-15-crown-5 and the gel monomer N-isopropylacrylamide under appropriate wavelength light irradiation. The type and amount of photoinitiator are selected based on the principle of being able to initiate the copolymerization reaction of the two monomers mentioned above, and can be selected according to the actual application requirements. For example, 2,2-diethoxyacetophenone can be selected as the photoinitiator, and correspondingly, the volume content of the photoinitiator in the gel prepolymer solution is controlled to be 0.1% to 0.5%.

[0012] The above K + In the technical solution of responsive hydrogel strain sensors, K + The fabrication method of the responsive hydrogel strain sensor is as follows: The aforementioned resistance strain gauge is placed in a mold; a gel prepolymer is added to the mold, ensuring the prepolymer is located on the substrate side of the strain gauge and in contact with the substrate; photo-initiated polymerization of the prepolymer transforms the prepolymer into a hydrogel state, thus obtaining the sensor. The aforementioned K... + In the technical solution of the responsive hydrogel strain sensor, the K + The thickness of the responsive hydrogel layer is preferably 0.2–1 mm. K + The reasons why the thickness of the responsive hydrogel layer is preferably in the range of 0.2 to 1 mm are as follows:

[0013] First, K + The thickness of the responsive hydrogel layer affects the detection sensitivity and K. + The response value and response range of a responsive hydrogel strain sensor are significantly affected. Thinner K... + The responsive hydrogel layer conforms to curved surfaces, can withstand repeated mechanical deformation, and improves the resistance to K-type deformation. + The strain transfer efficiency from the responsive hydrogel layer to the resistance strain gauge is improved, thereby enhancing K.+ The sensitivity of responsive hydrogel strain sensors to mechanical deformation and K + The overall flexibility of the responsive hydrogel strain sensor. Secondly, to improve K... + K of responsive hydrogel layers + Response performance, thinner K + responsive hydrogel layers due to their K + The shorter diffusion path length results in a faster response time, which is crucial for real-time strain detection requiring rapid signal transduction. Third, a thinner K... + The responsive hydrogel layer minimizes background noise and interference, resulting in a higher signal-to-noise ratio in strain detection. This, in turn, improves the accuracy and reliability of the sensor; however, an excessively thin K... + Responsive hydrogel layers may not provide sufficient mechanical strength and toughness, leading to unstable signal output and increased susceptibility to external interference. Therefore, this invention, through systematic experiments and considering multiple factors, ultimately determined the aforementioned K. + Preferred thickness of the responsive hydrogel layer.

[0014] The above K + In the technical solution of the responsive hydrogel strain sensor, the resistance strain gauge is preferably a thin-film resistance strain gauge.

[0015] The above K + In the technical solution of the responsive hydrogel strain sensor, the resistance strain gauge used is obtained by surface silanization modification of the substrate of an existing commercially available resistance strain gauge based on synthetic resin. The method for surface silanization modification of the substrate of the resistance strain gauge can refer to existing technologies. More specifically, the surface silanized synthetic resin substrate is obtained by grafting a synthetic resin substrate with a silane coupling agent containing carbon-carbon double bonds after plasma treatment. The specific grafting reaction conditions can be determined according to the selected silane coupling agent containing carbon-carbon double bonds, referring to existing technologies.

[0016] Furthermore, the aforementioned K + In the technical solution of the responsive hydrogel strain sensor, the silane coupling agent containing carbon-carbon double bonds includes 3-(methacryloyloxy)propyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane or γ-methacryloyloxypropyltrimethoxysilane, but feasible silane coupling agents containing carbon-carbon double bonds are not limited to the specific types listed above.

[0017] Furthermore, the aforementioned K +In the technical solution of the responsive hydrogel strain sensor, the synthetic resin substrate includes a polyimide substrate, a phenolic resin substrate, a phenolic-acetal resin substrate, an epoxy resin substrate, or a polyester resin substrate, but the feasible resin substrates are not limited to the specific types listed above.

[0018] This invention also provides a rapid and convenient quantitative detection method for trace amounts of blood potassium, comprising the following steps:

[0019] ①The above K + A responsive hydrogel strain sensor is connected to a Wheatstone bridge module integrated data acquisition device to form a detection device.

[0020] ②Prepare a series of K + Standard samples of different concentrations will be used in the K detector. + The responsive hydrogel strain sensor is placed on a hot stage, according to K + The concentration is arranged from low to high, towards K. + K of responsive hydrogel strain sensor + Standard samples were sequentially and uniformly dropped onto the responsive hydrogel layer. After the microstrain measured by the Wheatstone bridge module integrated data acquisition device reached stability, the microstrain corresponding to each standard sample was recorded; thus, a series of microstrains corresponding to the standard samples were obtained.

[0021] Using the micro-strain corresponding to each standard specimen as the ordinate, and the K of each standard specimen as the coordinate... + Plot the working curve with concentration on the x-axis and determine K. + The conversion formula between concentration and microstrain;

[0022] ③ Use the same K as in step ① + The responsive hydrogel strain sensor replaces the K sensor used in step ②. + Response-type hydrogel strain sensor, or K after step ② + K of responsive hydrogel strain sensor + The responsive hydrogel layer was restored to its state before the test in step ②;

[0023] Replace the standard sample in step ② with the sample to be tested, and measure the micro-strain of the sample to be tested according to the operation in step ②. Based on K determined in step ②, + The conversion formula between concentration and microstrain is used to calculate K of the test sample. + concentration;

[0024] In steps ② and ③, the temperature of the standard sample and the test sample is controlled to be the same as the temperature of the hot stage. The temperature of the hot stage is controlled to be a constant value between 25 and 40°C. The amount of standard sample and test sample added is controlled to be the same. The test sample is a serum sample.

[0025] In steps ② and ③ of the above-mentioned rapid and convenient quantitative detection method for trace serum potassium, the amount of standard sample and test sample added should be at least K + The responsive hydrogel layer provides complete coverage.

[0026] This invention experimentally confirms that, for a 3AA model standard resistance strain gauge with dimensions of 6.4mm × 3.5mm, bonding a 0.3mm thick K-type strain gauge to this strain gauge is effective. + Response hydrogel layer formation K + Following the responsive hydrogel strain sensor, quantitative detection of serum potassium can be achieved when the amount of standard sample or test sample added is 16–20 μL. The rapid and convenient quantitative detection method for trace serum potassium described in this invention features the advantage of requiring a small sample volume.

[0027] This invention experimentally confirms that, for a 3AA model standard resistance strain gauge with dimensions of 6.4mm × 3.5mm, bonding a 0.3mm thick K-type strain gauge to this strain gauge is effective. + Response hydrogel layer formation K + Following the responsive hydrogel strain sensor, when containing K + The sample was evenly added dropwise to K + K of responsive hydrogel strain sensor + After the responsive hydrogel layer is applied, the micro-strain measured by the Wheatstone bridge module integrated data acquisition device stabilizes within 2–4 minutes. The rapid and convenient quantitative detection method for trace amounts of serum potassium described in this invention has the advantage of high detection speed.

[0028] In the above-mentioned technical solution for rapid and convenient quantitative detection of trace blood potassium, the K of the detection device is used. + After the responsive hydrogel strain sensor is placed on the hot stage, K should be ensured. + K is not set on the responsive hydrogel strain sensor + One side of the responsive hydrogel layer is attached to the heating plane of the hot plate, typically K... + The responsive hydrogel strain sensor is placed horizontally on the heating plane of the hot stage, so that K + The responsive hydrogel layer faces upwards.

[0029] This invention is based on K + The principle behind the rapid and convenient quantitative detection of trace amounts of blood potassium using a responsive hydrogel strain sensor is as follows:

[0030] The K described in this invention + The K-type responsive hydrogel strain sensor + The responsive hydrogel layer is obtained by chemically bonding it to the substrate of the resistance strain gauge and completely covering the sensitive grid wire of the strain gauge. The substrate is a surface-silanized modified synthetic resin substrate, and the K...+ The responsive hydrogel layer is formed by physical crosslinking of linear polymer poly(N-isopropylacrylamide-co-4-acrylamidebenzo-15-crown-5) with physical crosslinking agent Laponite XLG nanosheets.

[0031] K + The responsive hydrogel layer is obtained by photoinitiated polymerization of a gel prepolymer containing the functional monomer 4-acrylamide benzo-15-crown-5, the gel monomer N-isopropylacrylamide, a photoinitiator, and the physical crosslinking agent Laponite XLG nanosheets. The 4-acrylamide benzo-15-crown-5 monomer and the N-isopropylacrylamide monomer provide K+ for the hydrogel layer, respectively. + The hydrogel layer possesses unique sensing properties due to its recognition performance and temperature responsiveness. Laponite XLG nanosheets are synthetic nanoclays composed of disc-shaped silicate particles, approximately 25 nm in diameter and 1 nm thick. Using Laponite XLG nanosheets as a physical crosslinking agent effectively increases the spacing between molecular chains in the gel network and reduces Kc. + Spatial barriers during transmission effectively accelerate sensor response time, enabling rapid detection. Laponite XLG utilizes reversible electrostatic interactions and / or hydrogen bonds, rather than permanent covalent bonds, between surface charges and the molecular chains of the gel network. This dynamic cross-linking allows the gel network to locally dissociate and rebuild under external forces, thereby enhancing K... + The strength and ductility of responsive hydrogels enable them to exhibit excellent adaptability and fatigue resistance in complex environments. This invention modifies the surface of the substrate for the resistance strain gauge through silanization, and the gel prepolymer solution polymerizes to form K... + During the process of creating the responsive hydrogel layer, covalent bonds are formed between it and the silanized modified substrate, enhancing the K... + The bonding stability between the responsive hydrogel layer and the resistance strain gauge can prevent K from being lost due to bending deformation during the detection process. + The problem of failure due to the detachment of the responsive hydrogel layer from the resistance strain gauge.

[0032] Based on the above, when K + The 15-crown-5 group in the responsive hydrogel layer reacts with potassium in serum. + Upon contact, a specific recognition reaction occurs. 15-crown-5 and K + It will form a stable "2:1" sandwich-like complex, making K + Precisely captured and fixed in K + Inside the responsive hydrogel layer. As the complex forms, the hydrogen bonds between the crown ether and water molecules are broken, leading to K... +The collapse of the three-dimensional network structure of the responsive hydrogel triggered K + The responsive hydrogel layer undergoes overall shrinkage and deformation. Due to K... + The responsive hydrogel layer is tightly bonded to the resistance strain gauge, therefore K + The shrinkage deformation of the responsive hydrogel layer is transmitted to the resistance strain gauge, causing it to bend and eventually leading to complete deformation of the strain gauge, resulting in bending and shrinkage deformation of the sensitive grid wire. Resistance strain gauges operate based on the piezoresistive effect; the resistance of the strain gauge changes with mechanical deformation (strain), and this change in resistance is linearly related to the applied strain. Therefore, K... + The shrinkage and deformation of the responsive hydrogel layer leads to a significant change in the resistance of the strain gauge. Using a high-precision resistance detection device, this resistance change can be monitored in real time, thus obtaining its micro-strain. By measuring the micro-strain value of the strain gauge, the concentration of potassium (K) in serum can be monitored. + Quantitative detection, such as Figure 14 As shown.

[0033] Compared with the prior art, the technical solution provided by the present invention has the following beneficial technical effects:

[0034] 1. This invention provides a K + A responsive hydrogel strain sensor, which is composed of K + The system consists of a responsive hydrogel layer and a resistance strain gauge. The resistance strain gauge includes a substrate, a sensitive grid wire, a capping layer, and leads. The substrate is a surface-silanized modified synthetic resin substrate; K + The responsive hydrogel layer is chemically bonded to the substrate and completely covers the sensitive grid wire of the resistance strain gauge; the K + The responsive hydrogel layer's gel polymer network is formed by physical crosslinking of linear polymer poly(N-isopropylacrylamide-co-4-acrylamide benzo-15-crown-5) with physical crosslinking agent Laponite XLG nanosheets. On one hand, this invention uses Laponite XLG nanosheets as a physical crosslinking agent, which can increase the spacing between the molecular chains of the gel network and reduce Kc. + Spatial barriers during transmission effectively accelerate sensor response time, enabling rapid detection. On the other hand, Laponite XLG utilizes reversible electrostatic interactions and / or hydrogen bonds, rather than permanent covalent bonds, between surface charges and the molecular chains of the gel network. This dynamic cross-linking allows the gel network to locally dissociate and rebuild under external forces, thereby enhancing K... + The strength and ductility of responsive hydrogels enable them to exhibit good adaptability and fatigue resistance in complex environments. Furthermore, this invention modifies the surface of the substrate for the resistance strain gauge by silanization to improve K... +The responsive hydrogel layer is covalently bonded to the substrate, effectively enhancing the bonding stability between the two, thereby increasing the stability of detection and signal transmission. Based on the above aspects, K... + Response hydrogel layers can achieve the targeting of K in serum + Quickly identify and K + The responsive hydrogel accurately and efficiently transmits signals to the resistance strain gauge, allowing for the monitoring of potassium levels in serum by identifying changes in the microstrain of the strain gauge. + Rapid quantitative detection.

[0035] 2. The K described in this invention + The responsive hydrogel strain sensor is used in conjunction with a Wheatstone bridge module integrated data acquisition device, K + The resistance strain gauge of the responsive hydrogel strain sensor can measure K + The minute deformation of the responsive hydrogel layer during detection is converted into an electrical signal output. This signal is amplified and collected by a Wheatstone bridge module, which not only improves detection sensitivity but also ensures signal stability and reliability. The accompanying Wheatstone bridge module integrates a small, lightweight data acquisition device with no complex internal components, resulting in low cost and simple operation. Therefore, the K described in this invention... + Based on a responsive hydrogel strain sensor, blood potassium testing can be performed without the need for large equipment and professional operators, making it particularly suitable for applications in homes, primary healthcare units, or on-site rapid testing scenarios.

[0036] 3. The K described in this invention + Based on a responsive hydrogel strain sensor, this invention also provides a rapid and convenient quantitative detection method for trace amounts of serum potassium. This method can achieve serum potassium detection with a small serum sample volume (16–20 μL). +Rapid concentration detection (2 min). The method described in this invention has significant advantages over existing serum potassium detection methods, especially in terms of detection speed and sample volume. Existing serum potassium detection methods, such as flame atomic absorption spectrometry, graphite furnace atomic absorption spectrometry, and detection using ion-selective electrodes (ISE), while technically mature, have many limitations in practical applications. For example, flame atomic absorption spectrometry requires complex sample pretreatment steps and more than 2 mL of serum sample; the detection time of graphite furnace atomic absorption spectrometry is usually several minutes to tens of minutes; the detection accuracy of detection using ion-selective electrodes is easily affected by interference from other ions in the sample, and the requirements for sample pretreatment are high. Furthermore, currently available serum potassium test kits are mainly used for laboratory analysis, are complex to operate, and have long detection times. In contrast, the method described in this invention requires only a small amount of serum sample, greatly reducing sample volume and significantly improving detection efficiency. It also eliminates the need for complex sample pretreatment, achieving rapid, efficient, and convenient detection of serum potassium.

[0037] 4. The rapid and convenient quantitative detection method for trace blood potassium described in this invention has a wide detection range and excellent anti-interference ability. Regarding the detection range, the method of this invention can detect up to 10... -6 Accurate detection of K within a concentration range of ~10 mmol / L + It covers everything from extremely low K + Concentration to high K + This invention offers various applications across different concentrations. Regarding anti-interference performance, the method of this invention exhibits excellent anti-interference capabilities against multiple metal ions. Even in the presence of high concentrations of common metal ions such as sodium, calcium, and magnesium, the method maintains good detection accuracy. This characteristic enables the method of this invention to effectively avoid interference from other ions in complex biological samples, ensuring the accuracy of the detection results. Furthermore, the K relied upon by the method of this invention... + The responsive hydrogel strain sensor exhibited virtually no performance degradation during 12 consecutive cycle tests, demonstrating excellent cyclic performance and stability. This characteristic not only improves detection efficiency but also reduces detection costs, making it more economical for large-scale applications. This invention provides an efficient, convenient, and economical solution for blood potassium detection through its wide detection range, strong anti-interference capability, and excellent cyclic performance. Attached Figure Description

[0038] Figure 1 Figure (a) is a SEM image of PNB-1 after freeze-drying. Figure 1 Figure (b) shows the infrared spectra of PNB-1, B15C5Am, L-XLG, and PNIPAm hydrogels.

[0039] Figure 2 These are the tensile stress-strain curves for PNB-1, PNB-3, and PNB-5.

[0040] Figure 3 Figures (a) and (b) show PNB-1 in deionized water at different temperatures and at different K, respectively. + A photograph in an aqueous solution.

[0041] Figure 4 Figure (a) shows the S of PNB-1. T / S0 as a function of temperature curve Figure 4 Figure (b) shows the R of PNB-1. S Curve showing the change with temperature.

[0042] Figure 5 It is K + Photographs showing the changes in the volume of PNB-1, PNB-3, and PNB-5 in aqueous solution over soaking time.

[0043] Figure 6 It is the S of PNB-1, PNB-3 and PNB-5 t / S0 variation curve with soaking time.

[0044] Figure 7 This is a schematic diagram illustrating the principle and process of surface silanization modification of a polyimide substrate.

[0045] Figure 8 Figure (a) shows the XPS spectra of the unmodified PI substrate (Before modification) and the modified PI substrate (After modification). Figure 8 Figure (b) is a peak breakdown diagram of the Si 2p XPS spectrum of the modified PI substrate.

[0046] Figure 9 Figure (a) is K + Peel strength test results between the responsive hydrogel and the modified PI substrate. Figure 9 Figure (b) is K + Shear strength test results between the responsive hydrogel and the modified PI substrate.

[0047] Figure 10 Figure (a) shows photographs of the deformation of the PNB-1 patch at different temperatures. Figure 10 Figure (b) is a photograph of the deformation of the unmodified hydrogel patch at different temperatures.

[0048] Figure 11 It is K + A schematic diagram of the structure of a responsive hydrogel strain sensor. In the diagram, 1—K +2—Responsive hydrogel layer, 3—Resistant strain gauge, 4—Sensitive grid wire.

[0049] Figure 12 This is a schematic diagram of a detection device for rapid and convenient quantitative detection of trace amounts of blood potassium. In the diagram, 4—wire, 5—Wheatstone bridge module integrated data acquisition device.

[0050] Figure 13 This is a circuit diagram of a detection device for rapid and convenient quantitative detection of trace amounts of blood potassium.

[0051] Figure 14 This invention is based on K + A schematic diagram illustrating the principle of using a responsive hydrogel strain sensor to detect blood potassium levels.

[0052] Figure 15 Figure (a) is K + Microstrain of responsive hydrogel strain sensor with K + Concentration (10) -6 ~10 1 Changes in mmol / L Figure 15 Figure (b) is K + Microstrain of responsive hydrogel strain sensor with K + Changes in concentration (1–9 mmol / L), Figure 15 The (c) diagram is K + The change of microstrain in a responsive hydrogel strain sensor over time.

[0053] Figure 16 It is K + Response hydrogel strain sensor at different concentrations of K + The change of micro-strain in aqueous solution with detection time.

[0054] Figure 17 It is K + When the concentration of K increases from 0 to 9 mmol / L + Continuous detection performance of responsive hydrogel strain sensors.

[0055] Figure 18 K is used under different dropping conditions. + Response-type hydrogel strain sensor identifies different K + Microstrain of human serum samples at concentrations.

[0056] Figure 19 Figure (a) is K + Response hydrogel strain sensor for K + Anti-interference detection performance of aqueous solutions and interfering ion aqueous solutions. Figure 19 Figure (b) is K +Response-type hydrogel strain sensor for different concentrations of Na + Mg 2+ Ca 2+ and K + The anti-interference detection performance of the mixed solution.

[0057] Figure 20 Figure (a) is K + Response-type hydrogel strain sensors in deionized water and K + Performance graph of cyclic detection in aqueous solution. Figure 20 Figure (a) is K + Response-type hydrogel strain sensors in deionized water and K + Micro-strain test results obtained by cyclic testing in aqueous solution.

[0058] Figure 21 (a) The figure shows the microstrain of each standard sample obtained at different testing temperatures. Figure 21 Graph (b) shows the effect of temperature and blood potassium concentration on K. + A diagram illustrating the combined effects of a responsive hydrogel strain sensor on serum potassium levels. Figure 21 Figure (c) shows K at different detection temperatures. + Response-type hydrogel strain sensor for detecting K in serum + Micro-strain reference standard spectrum of concentration. Detailed Implementation

[0059] The following examples illustrate the K of the present invention. + The responsive hydrogel strain sensor and the rapid and convenient quantitative detection method for trace amounts of serum potassium are further explained. It should be noted that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made to the present invention by those skilled in the art based on the above description are still within the scope of protection of the present invention.

[0060] Example 1

[0061] In this embodiment, K with different contents of physical crosslinking agent is prepared. + Responsive hydrogel (PNB hydrogel).

[0062] (1) Preparation of gel prepolymer solution

[0063] Laponite XLG nanosheets (L-XLG) were added to deionized water under ice bath conditions and stirred for 6 h to obtain an L-XLG dispersion. L-XLG dispersions with concentrations of 0.01 mol / L, 0.03 mol / L, and 0.05 mol / L were prepared respectively.

[0064] The functional monomer benzo-15-crown-5-acrylamide (B15C5Am), the gelling monomer N-isopropylacrylamide (NIPAm), and the photoinitiator 2,2-diethoxyacetophenone were added to an L-XLG dispersion and thoroughly mixed to obtain a gel prepolymer. Three gel prepolymers were prepared using L-XLG dispersions with concentrations of 0.01 mol / L, 0.03 mol / L, and 0.05 mol / L. In each gel prepolymer, the concentration of B15C5Am was 0.1 mol / L, the concentration of NIPAm was 1 mol / L, the volume concentration of the photoinitiator was 0.2%, and the concentrations of L-XLG were 0.01 mol / L, 0.03 mol / L, and 0.05 mol / L, respectively.

[0065] (2) Preparation of K + Response hydrogel (PNB hydrogel)

[0066] The gel prepolymer was added to the mold, and UV light was applied above the mold for 10 minutes to induce K... + The responsive hydrogel prepolymer undergoes a polymerization reaction, bringing K... + The responsive hydrogel prepolymer is transformed into K + A responsive hydrogel (1 mm thick) was then removed from the mold and washed with deionized water. + Response hydrogel. Based on the K... + Different concentrations of L-XLG in the responsive hydrogel prepolymer will affect K + The responsive hydrogels are designated PNB-1, PNB-3, and PNB-5, respectively, corresponding to L-XLG concentrations of 0.01 mol / L, 0.03 mol / L, and 0.05 mol / L.

[0067] Comparative Example 1

[0068] In this comparative example, N-isopropylacrylamide hydrogel (PNIPAm hydrogel) was prepared.

[0069] (1) Under ice bath conditions, the crosslinking agent L-XLG was added to deionized water and stirred for 6 h to obtain an L-XLG dispersion with a concentration of 0.01 mol / L. NIPAm and the photoinitiator 2,2-diethoxyacetophenone were added to the L-XLG dispersion and stirred thoroughly until dissolved to obtain a gel prepolymer solution, wherein the concentration of NIPAm monomer was 1 mol / L, the volume concentration of the photoinitiator was 0.2%, and the concentration of L-XLG was 0.01 mol / L.

[0070] (2) Preparation of poly(N-isopropylacrylamide) hydrogel (PNIPAm hydrogel)

[0071] The prepolymer was added to the mold, and ultraviolet light was applied to the mold for 10 minutes to induce the polymerization reaction of the gel prepolymer, which transformed the gel prepolymer into poly(N-isopropylacrylamide) hydrogel (1 mm thick). The mold was then removed and the poly(N-isopropylacrylamide) hydrogel was washed with deionized water.

[0072] The PNB-1 prepared in Example 1 was freeze-dried and its cross-section was tested by scanning electron microscopy (SEM). The results are as follows: Figure 1 As shown in Figure (a), the porous structure inside PNB-1 can be clearly observed from the SEM image. The presence of these porous structures is due to K + It provides a favorable channel for diffusion and transport, and can increase the specific surface area of ​​PNB-1 and reduce the resistance to ion transport, thereby improving the ion conduction performance of PNB-1.

[0073] Infrared spectroscopy was performed on PNB-1 (PNB hydrogel in the figure), B15C5Am (B15C5Ammonomer in the figure), L-XLG prepared in Example 1 and PNIPAm hydrogel prepared in Comparative Example 1. The results are as follows: Figure 1 As shown in Figure (b), the characteristic absorption peak of the stretching vibration of the C=C skeleton on the B15C5Am benzene ring appears at 1515 cm⁻¹. -1 The characteristic absorption peak of the CO asymmetric stretching vibration on Ar-OR is located at 1223 cm⁻¹. -1 The characteristic absorption peak of L-XLG is at 960 cm⁻¹. -1 An absorption peak representing the silanol group appears at 640 cm⁻¹. -1 The peak value at 1367 cm⁻¹ corresponds to the stretching vibration of Mg-O. The characteristic absorption peak of poly(N-isopropylacrylamide) hydrogels is at 1367 cm⁻¹. -1 and 1387cm -1 The peaks appearing at 640 cm⁻¹ are characteristic absorption peaks of isopropyl groups. The presence of these peaks indicates successful polymerization of the NIPAM monomer, forming a temperature-responsive hydrogel network. Furthermore, the peaks at 640 cm⁻¹... -1 The peak at this location is also correlated with the tensile vibration of Mg-O, further confirming the presence of L-XLG in poly(N-isopropylacrylamide) hydrogel. Poly(N-isopropylacrylamide) hydrogel and K + The Si-O bonds in the responsive hydrogel exhibited a significant red shift, with the absorption peak moving from a higher wavenumber to 1000 cm⁻¹. -1This is mainly because the chemical interaction between L-XLG and monomers or polymer chains alters the local chemical environment, affecting the vibrational frequency of Si-O bonds. This chemical interaction not only enhances the mechanical properties of the hydrogel but also provides a more stable network structure. The characteristic absorption peaks of B15C5Am, L-XLG, and PNIPAM are all located at K... + The responsive hydrogel is clearly visible in the infrared spectrum.

[0074] To evaluate the K prepared in Example 1 + The mechanical properties of the responsive hydrogels were tested using a mechanical testing machine (model EZ-LX, Shimadzu) for PNB-1, PNB-3, and PNB-5. During the test, a 100N sensor was used to perform tensile tests on PNB-1, PNB-3, and PNB-5 at a tensile rate of 20 mm / min to obtain their tensile stress-strain curves.

[0075] The tensile stress-strain curves of PNB-1, PNB-3, and PNB-5 are shown below. Figure 2 As shown, Figure 2 In this context, 1% L-XLG, 3% L-XLG, and 5% L-XLG represent PNB-1, PNB-3, and PNB-5, respectively. + The mechanical properties of the responsive hydrogels significantly improved with increasing concentration of the crosslinking agent L-XLG. The tensile strengths of PNB-1, PNB-3, and PNB-5 increased from 30 kPa to 55 kPa and 95 kPa, respectively, and their strain capacity also increased from 400% to 550% and 603%. This indicates that the addition of L-XLG not only enhanced the K... + The responsive hydrogel's strength is enhanced by improved ductility. This is primarily attributed to the synergistic effect of L-XLG's dynamic cross-linking properties and nano-reinforcement. Specifically, L-XLG forms reversible electrostatic interactions and / or hydrogen bonds with the hydrogel's polymer chains through its surface charge (positively charged edges, negatively charged surfaces), rather than permanent covalent bonds. This dynamic cross-linking mechanism allows the hydrogel network to locally dissociate and rebuild under external forces, thereby enhancing the hydrogel's strength and ductility. Furthermore, the interface between L-XLG and the hydrogel's polymer chains effectively transfers stress, optimizes network uniformity, and delays crack propagation, contributing to higher toughness and fatigue resistance under complex stresses. The sliding friction and fracture of dynamic bonds also absorb a significant amount of energy, further improving the hydrogel's toughness.

[0076] Example 2

[0077] In this embodiment, the test temperature and K + Effect of concentration on volume change of PNB-1 prepared in Example 1.

[0078] PNB-1 was immersed in deionized water and K, respectively. + K at a concentration of 0.2 mol / L + In aqueous solution, observe the volume change under different temperature conditions (24-40℃), specifically using the change in bottom area to reflect the volume change. Figure 3 Figures (a) and (b) show PNB-1 in deionized water at different temperatures and at different K, respectively. + A photograph of an aqueous solution. (By...) Figure 3 It can be seen that in deionized water and K + In aqueous solution, the volume of PNB-1 gradually decreases with increasing temperature, indicating that the K provided by this invention... + Responsive hydrogels exhibit temperature responsiveness. Furthermore, K... + The presence of K also had a significant impact on the volume change of PNB-1, indicating that K + In conjunction with temperature, K + Volume changes of responsive hydrogels.

[0079] To more accurately describe the volume change of PNB-1 at different temperatures, the rate of change of the bottom area of ​​PNB-1 (Si) was tested. T / S0), where S T S0 represents the base area of ​​PNB-1 at a specific temperature, and S0 represents the base area of ​​PNB-1 at 24°C. The results are as follows: Figure 4 As shown in Figure (a), "pure water" represents the test conducted in deionized water, 0.2MK + Represents 0.2 mol / L K + The test was conducted in an aqueous solution. This is to more clearly reflect the K content. + The enhanced effect of concentration on the volume change of PNB-1 introduces a change in relative bottom area (R0). S To estimate the temperature response K of PNB-1 + The impact of R S The value is defined as the K at 0.2 mol / L at each temperature. + S in aqueous solution T / S0 value and S in deionized water T The ratio of / S0 values, through R S K can be detected + The optimal operating temperature for the concentration, and the results are as follows: Figure 4 As shown in Figure (b). Figure 4 It can be seen that at 32℃, R S The minimum value indicates that at 32℃, K + The responsive hydrogel exhibits the greatest volume change, therefore 32℃ was chosen as the temperature for Kt. +Response hydrogel detection K + The optimal operating temperature for the concentration.

[0080] Example 3

[0081] K was tested at the optimal operating temperature determined in Example 2. + The effect on the volume change of PNB-1, PNB-3 and PNB-5 prepared in Example 1.

[0082] PNB-1, PNB-3 and PNB-5 were immersed in K respectively. + K at a concentration of 0.2 mol / L and a temperature of 32℃ + In an aqueous solution, observe the change in its volume over time. The results are as follows: Figure 5 As shown, Figure 5 Figures (a) to (c) represent PNB-5, PNB-3, and PNB-1, respectively. With increasing soaking time, the K... + The volume of the responsive hydrogels gradually decreased, and under the same immersion time, with K... + The increase of crosslinking agent L-XLG content in responsive hydrogels, K + The volume shrinkage of the responsive hydrogel gradually decreases, which indicates that K + The more robust cross-linked network in responsive hydrogels hinders K... + The rapid and widespread response.

[0083] PNB-1, PNB-3 and PNB-5 were immersed in K respectively. + K at a concentration of 0.2 mol / L and a temperature of 32℃ + In solution, measure K + The bottom area (S) of responsive hydrogels at a specific time point t Given the base area (S0) at the starting time point, calculate S. t / S0, draw S t The curve of / S0 changing with soaking time is shown below. Figure 6 As shown, Figure 6 In the figures, 1% L-XLG, 3% L-XLG, and 5% L-XLG represent PNB-1, PNB-3, and PNB-5, respectively. PNB-5 reduced its bottom area by 54% within 12 minutes, PNB-3 reacted slightly faster, reducing its bottom area by 61% within 10 minutes, while PNB-1 showed better reaction performance, reducing its bottom area by 81% within 7 minutes. Therefore, K... + The lower the L-XLG content in a responsive hydrogel, the lower the K content. + responsive hydrogels and K + The faster the reaction speed.

[0084] Example 4

[0085] Polyimide (PI) lacks active groups on its surface, exhibits strong chemical inertness, and is difficult to react with K. + The responsive hydrogel adheres tightly to enhance the bonding between the PI substrate and K. + The binding between responsive hydrogels is described in this embodiment, where a modified PI substrate is prepared by surface silanization modification. The modification principle and process are illustrated in the diagram below. Figure 7 As shown, the steps are as follows:

[0086] (1) Preparation of 3-(methacryloyloxy)propyltrimethoxysilane hydrolysate

[0087] The silane coupling agent 3-(methacryloyloxy)propyltrimethoxysilane was added to a sodium acetate buffer solution with pH=5.2 to prepare a 1wt% solution. The solution was stirred for 30 min to hydrolyze the methoxy group of the silane coupling agent to a hydroxyl group, thus obtaining a 3-(methacryloyloxy)propyltrimethoxysilane hydrolysate.

[0088] (2) Plasma treatment

[0089] The sheet-like PI substrate was ultrasonically cleaned in anhydrous ethanol for 30 min, then removed and dried, and treated with plasma for 5 min to further clean the PI substrate surface and introduce active functional groups, including hydroxyl and carboxyl groups, onto the PI substrate surface.

[0090] (3) Grafting reaction

[0091] The plasma-treated PI substrate was completely immersed in a 3-(methacryloyloxy)propyltrimethoxysilane hydrolysis solution at 60°C for 30 min. During this process, the silanol groups of 3-(methacryloyloxy)propyltrihydroxysilane underwent a condensation reaction with the active functional groups on the surface of the PI substrate to form covalent bonds. The substrate was then removed, dried at 60°C, rinsed with anhydrous ethanol, and dried again at 60°C to obtain a PI substrate with surface silanization modification (modified PI substrate).

[0092] X-ray photoelectron spectroscopy (XPS) was performed on the unmodified PI substrate (before modification) and the modified PI substrate (after modification). The results are as follows: Figure 8 As shown in Figure (a), compared to the unmodified PI substrate, the modified PI substrate exhibits a distinct Si 2p peak in its XPS spectrum, confirming the successful grafting of the silane coupling agent onto the PI substrate. The peak distribution diagram of the Si 2p XPS spectrum of the modified PI substrate is shown below. Figure 8As shown in Figure (b), the figure clearly displays three main components, each corresponding to a different chemical bond: Si-O bond (100.9 eV), Si-C bond (100 eV), and Si-Si bond (99.2 eV). The presence of Si-O bonds is related to the grafting of the silane coupling agent, i.e., the silicon-oxygen bond in the 3-(methacryloyloxy)propyltrimethoxysilane molecule undergoes a condensation reaction with the hydroxyl groups on the PI substrate surface to form a chemical bond; the Si-C bond indicates the presence of a chemical bond between silicon and carbon on the PI substrate surface, which may originate from the silicon-carbon double bond in the 3-(methacryloyloxy)propyltrimethoxysilane molecule. These double bonds will participate in the reaction during the subsequent hydrogel polymerization process, enhancing the bonding between the PI substrate and the hydrogel; the S-Si bond indicates the presence of a direct connection between silicon atoms on the PI substrate surface, which is related to the self-polymerization and crosslinking of the 3-(methacryloyloxy)propyltrimethoxysilane molecule.

[0093] Example 5

[0094] In this embodiment, K is prepared + Responsive hydrogel patch.

[0095] (1) Preparation of gel prepolymer solution

[0096] The operation is the same as step (1) in Example 1.

[0097] (2) Assembly mold

[0098] In this step, a glass plate is used as the supporting base, and a polytetrafluoroethylene (PTFE) plate with rectangular through-holes is used as the template. The shape and size of the rectangular through-holes on the template are consistent with the shape and size of the substrate. A circular through-hole protruding beyond one corner of the rectangular through-hole is also provided. The template thickness is 1 mm. A transparent glass plate is used as the cover plate, and the cover plate has one through-hole. The dimensions of the supporting base, the template, and the cover plate are all larger than the dimensions of the modified PI substrate.

[0099] The modified PI substrate prepared in Example 4 is placed on a horizontally placed support plate. The template is placed above the modified PI substrate, so that the modified PI substrate is completely located in the rectangular through hole of the template. A cover plate is placed horizontally above the template to completely cover the rectangular through hole of the template and match the position of the through hole on the cover plate with the position of the circular through hole on the template, so that the through hole on the cover plate is connected to the circular through hole on the template. Then the positions of the support plate, the modified PI substrate, the mold and the cover plate are fixed, thus completing the assembly of the mold. The mold has a cuboid cavity.

[0100] (3) Polymerization reaction and post-processing

[0101] The gel prepolymer solution was injected into and filled the rectangular cavity of the mold through the through-holes in the cover plate and the circular through-holes in the template. Ultraviolet light was applied above the mold for 10 minutes to initiate a polymerization reaction in the gel prepolymer solution, converting it into K. + A responsive hydrogel was formed and chemically bonded to a modified PI substrate. The cover plate, template, and support base were then carefully removed, and K was washed with deionized water. + Response hydrogels, yielding K + Responsive hydrogel patch.

[0102] Depending on the concentration of L-XLG in the gel prepolymer solution used, the prepared K + The responsive hydrogel patches are designated as PNB-1 patch, PNB-3 patch, and PNB-5 patch, respectively, corresponding to L-XLG concentrations of 0.01 mol / L, 0.03 mol / L, and 0.05 mol / L.

[0103] Comparative Example 2

[0104] The operation of this comparative example is basically the same as that of Example 5, except that the modified PI substrate is replaced with an unmodified PI substrate, and the concentration of L-XLG in the gel prepolymer solution is 0.01 mol / L, so as to prepare an unmodified hydrogel patch.

[0105] Example 6

[0106] The K prepared in Example 5 was tested by peeling and lap shear tests. + K on responsive hydrogel patches + The adhesion strength between the responsive hydrogel and the modified PI substrate.

[0107] The peel test is a test that measures K + The force required for a responsive hydrogel to peel off from a modified PI substrate reflects the degree of adhesion between the two. The test results are as follows: Figure 9 As shown in Figure (a), the adhesion strength between the two gradually increases with the increase of the concentration of crosslinking agent L-XLG in the gel prepolymer solution. When the concentration of L-XLG increases from 0.01 mol / L to 0.03 mol / L and 0.05 mol / L, the adhesion strength between the two increases from 10 Nm. -1 Increased to 24 N m -1 and 50N m -1 .

[0108] The lap shear test is performed by measuring K. + When responsive hydrogels and modified PI substrates are subjected to shear forces parallel to the interface direction, K + The performance of the responsive hydrogel patch is shown in the test results. Figure 9As shown in Figure (b), with the increase of the concentration of crosslinking agent L-XLG in the gel prepolymer solution, K + The shear force between the responsive hydrogel and the modified PI substrate gradually increased. When the concentration of L-XLG increased from 0.01 mol / L to 0.03 mol / L and 0.05 mol / L, the shear force between them rapidly increased from 8.2 kPa to 16.5 kPa and 23.8 kPa, respectively.

[0109] This embodiment confirms K's effectiveness through peel and lap shear tests. + The responsive hydrogel exhibits stable binding with the modified PI substrate, primarily due to K... + A chemical bond was formed between the responsive hydrogel and the modified PI substrate.

[0110] Example 7

[0111] Test Example 5 prepared K + Deformation of responsive hydrogel patches at different temperatures.

[0112] The PNB-1 patch prepared in Example 5 and the unmodified hydrogel patch prepared in Comparative Example 2 were placed in a high-precision temperature control device. The initial temperature was set to 28°C. After stabilizing for 10 minutes, the patch status was recorded using an image acquisition system. Then, the temperature was gradually increased to 32, 36, 40, and 60°C, and the patch status was recorded at each temperature. The results are as follows: Figure 10 As shown. When the temperature rises from 28℃ to 60℃, the PNB-1 patch, due to K... + The responsive hydrogel undergoes thermally induced shrinkage and significantly bends towards the hydrogel side. Throughout the deformation process, K + The responsive hydrogel remains firmly bonded to the modified PI substrate, such as... Figure 10 As shown in Figure (a). However, for the unmodified hydrogel patch prepared in Comparative Example 2, during the temperature increase from 28°C to 60°C, the bonding strength between the hydrogel and the PI substrate was insufficient to withstand the force generated by the hydrogel shrinkage, causing the hydrogel to detach from the PI substrate, as shown in Figure (a). Figure 10 As shown in Figure (b), this embodiment demonstrates that by modifying the PI substrate and then covalently bonding the hydrogel to the PI substrate, the bonding strength between the hydrogel and the PI substrate can be effectively enhanced, paving the way for the utilization of K... + K-type responsive hydrogels and resistance strain gauges + Response-type hydrogel strain sensor achieves K + Quantitative concentration detection provides an important foundation.

[0113] Example 8

[0114] In this embodiment, K is provided. +A responsive hydrogel strain sensor and its fabrication method.

[0115] K + A schematic diagram of the structure of the responsive hydrogel strain sensor is shown below. Figure 11 As shown, by K + The system comprises a responsive hydrogel layer 1 and a resistance strain gauge 2. The resistance strain gauge 2 includes a substrate, a sensitive grid wire 3, a capping layer, and leads. The sensitive grid wire is made of constantan alloy. The leads are located at both ends of the sensitive grid wire and are used to connect the sensitive grid wire to the measurement circuit. The substrate serves to fix and support the sensitive grid wire 3, and the capping layer serves to protect the sensitive grid wire 3. The substrate is a surface-silanized modified polyimide (PI) substrate; K + The responsive hydrogel layer 1 is chemically bonded to the substrate and completely covers the sensitive grid wire 3 of the resistance strain gauge 2. The K... + The responsive hydrogel layer 1's gel polymer network is formed by physical crosslinking of linear polymer poly(N-isopropylacrylamide-co-4-acrylamidebenzo-15-crown-5) with physical crosslinking agent Laponite XLG nanosheets, K + The thickness of the responsive hydrogel layer 1 is 0.3 mm.

[0116] K + The fabrication method of the responsive hydrogel strain sensor is as follows:

[0117] (1) Surface silanization modification of the substrate of the resistance strain gauge.

[0118] ① Preparation of 3-(methacryloyloxy)propyltrimethoxysilane hydrolysate

[0119] The operation is the same as step (1) in Example 4.

[0120] ②Plasma treatment

[0121] The resistance strain gauge (specifically a standard resistance strain gauge of model 3AA, with dimensions of 6.4mm × 3.5mm) was ultrasonically cleaned in anhydrous ethanol for 30 minutes, removed and dried, and then treated with plasma for 5 minutes to further clean the PI substrate surface of the resistance strain gauge and introduce active functional groups, including hydroxyl and carboxyl groups, onto the PI substrate surface of the resistance strain gauge.

[0122] ③Grafting reaction

[0123] The plasma-treated resistance strain gauge was completely immersed in a 3-(methacryloyloxy)propyltrimethoxysilane hydrolysis solution at 60°C for 30 min, then removed and dried at 60°C. Subsequently, it was rinsed with anhydrous ethanol and dried again at 60°C to complete the surface silanization modification of the resistance strain gauge substrate.

[0124] (2) Preparation of gel prepolymer solution

[0125] L-XLG was added to deionized water under ice bath conditions and stirred for 6 hours to obtain an L-XLG dispersion with a concentration of 0.01 mol / L. B15C5Am, NIPAm, and the photoinitiator 2,2-diethoxyacetophenone were added to the L-XLG nanosheet dispersion and stirred thoroughly to obtain a gel prepolymer.

[0126] In the gel prepolymer solution, the concentration of B15C5Am was 0.1 mol / L, the concentration of NIPAm was 1 mol / L, the volume concentration of the photoinitiator was 0.2%, and the concentration of L-XLG was 0.01 mol / L.

[0127] (3) Assembly mold

[0128] In this step, a glass plate is used as the supporting base, and a polytetrafluoroethylene plate with rectangular through holes is used as the template. The shape and size of the rectangular through holes on the template are consistent with the shape and size of the silanized substrate. A circular through hole protruding beyond the rectangular through hole is also provided at one corner. The template thickness is 0.3 mm. A transparent glass plate is used as the cover plate, and the cover plate has one through hole. The dimensions of the supporting base, the template, and the cover plate are all larger than the dimensions of the resistance strain gauge substrate.

[0129] The surface-silanized strain gauge obtained in step (1) is placed horizontally on the support base plate with the surface-silanized substrate facing upwards. The template is placed above the strain gauge so that the surface-silanized substrate is completely located in the rectangular through hole of the template. A cover plate is placed horizontally above the template to completely cover the rectangular through hole of the template and make the through hole on the cover plate match the position of the circular through hole on the template, so that the through hole on the cover plate is connected to the circular through hole on the template. Then the positions of the support base plate, the strain gauge, the mold and the cover plate are fixed to complete the assembly of the mold. The mold has a cuboid cavity.

[0130] (3) Polymerization reaction and post-processing

[0131] The gel prepolymer solution was injected into and filled the rectangular cavity of the mold through the through-holes in the cover plate and the circular through-holes in the template. Ultraviolet light was applied above the mold for 10 minutes to initiate a polymerization reaction in the gel prepolymer solution, converting it into K. + The responsive hydrogel was chemically bonded to a surface-silanized modified substrate. The cover plate, template, and support base were then carefully removed, and K was washed with deionized water. + Response hydrogels, yielding K + Response-type hydrogel strain sensor.

[0132] Example 9

[0133] In this embodiment, K is provided. + The responsive hydrogel strain sensor and its preparation method are basically the same as those in Example 8, except that the concentration of L-XLG in the gel prepolymer solution is 0.03 mol / L.

[0134] Example 10

[0135] This embodiment provides K + The responsive hydrogel strain sensor and its preparation method are basically the same as those in Example 8, except that the concentration of L-XLG in the gel prepolymer solution is 0.05 mol / L.

[0136] Example 11

[0137] This embodiment provides a detection device for rapid and convenient quantitative detection of trace amounts of blood potassium, and its structural schematic diagram is shown below. Figure 12 .

[0138] The detection device for rapid and convenient quantitative detection of trace blood potassium, based on K in Example 8. + The data acquisition device consists of a responsive hydrogel strain sensor and a Wheatstone bridge module integrated into a 5-unit system. + The leads of the responsive hydrogel strain sensor are connected to the Wheatstone bridge module integrated data acquisition device 5 via a welded connection structure and wire 4. A circuit diagram of the detection device is shown below. Figure 13 K is about to be K + The circuit diagram of the responsive hydrogel strain sensor connected to the Wheatstone bridge circuit is shown below. Figure 13 As shown.

[0139] Example 12

[0140] This embodiment provides a detection device for rapid and convenient quantitative detection of trace amounts of blood potassium, and its structural schematic diagram is shown below. Figure 12 .

[0141] The detection device for rapid and convenient quantitative detection of trace blood potassium, comprising K from Example 9. + The data acquisition device consists of a responsive hydrogel strain sensor and a Wheatstone bridge module integrated into a 5-unit system. + The leads of the responsive hydrogel strain sensor are connected to the Wheatstone bridge module integrated data acquisition device 5 via a welded connection structure and wire 4.

[0142] Example 13

[0143] This embodiment provides a detection device for rapid and convenient quantitative detection of trace amounts of blood potassium, and its structural schematic diagram is shown below. Figure 12 .

[0144] The detection device for rapid and convenient quantitative detection of trace blood potassium, based on the K in Example 10. + The data acquisition device consists of a responsive hydrogel strain sensor and a Wheatstone bridge module integrated into a 5-unit system. + The leads of the responsive hydrogel strain sensor are connected to the Wheatstone bridge module integrated data acquisition device 5 via a welded connection structure and wire 4.

[0145] Example 14

[0146] Examine the K provided in Examples 8-10 + Response hydrogel strain sensor for K + Detection performance.

[0147] (1) Prepare a concentration of 10 -6 10 -5 10 -4 10 -3 10 -2 10 -1 10 0 and 10 1 K mmol / L (mM) + Aqueous solution.

[0148] The K of the detection device in Examples 11 to 13 are respectively + The responsive hydrogel strain sensor was completely immersed in the above-mentioned different concentrations of K. + In the aqueous solution samples, the amount of each sample was the same, and the temperature was 32℃. After the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reached stability, the corresponding micro-strain for each sample was recorded. The results are as follows: Figure 15 As shown in Figure (a).

[0149] (2) Usually, blood potassium + The concentration is at the mmol / L level, with a normal range of 3.5–5.5 mmol / L. Therefore, K can be prepared at concentrations of 1, 3, 5, 7, and 9 mmol / L (mM). + Aqueous solution.

[0150] The K of the detection device in Examples 11 to 13 are respectively + The responsive hydrogel strain sensor was completely immersed in the above-mentioned different concentrations of K. + In the aqueous solution samples, the amount of each sample was the same, and the temperature was 32℃. After the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reached stability, the corresponding micro-strain for each sample was recorded. The results are as follows: Figure 15 As shown in Figure (b).

[0151] (3) The K of the detection device in Examples 11 to 13 are respectively +The responsive hydrogel strain sensor was completely immersed in a solution of 5 mmol / L K. + For each detection device, K is an aqueous solution. + The aqueous solution was used in the same amount and at a temperature of 32℃. The change of micro-strain (με) over time was recorded using a Wheatstone bridge module integrated data acquisition device. The results are as follows: Figure 15 As shown in Figure (c).

[0152] Depend on Figure 15 It can be seen that the K prepared in Examples 8-10 + Response-type hydrogel strain sensors exhibit different K + Detection range, but all have a very wide K-band. + Detection range. Specifically, K prepared in Example 8... + The responsive hydrogel strain sensor has the widest detection range, at 10. -6 ~10 mmol / L, K prepared in Example 9 + The detection range of the responsive hydrogel strain sensor is 10. -5 ~10 mmol / L, K prepared in Example 10 + The detection range of the responsive hydrogel strain sensor is 10. -4 ~10mmol / L. K + When the concentration is in the range of 1–9 mmol / L, K + Microstrain and K-S of Response Hydrogel Strain Sensors + The concentration showed a linear relationship. K prepared in Examples 8-10 + The degree of microstrain change in the responsive hydrogel strain sensor gradually decreases. K0 prepared in Examples 8-10 + Microstrain of responsive hydrogel strain sensor at 5 mmol / L K + The times to reach equilibrium in the aqueous solution were 2.0 min, 2.8 min, and 3.4 min, respectively, all of which enabled rapid detection.

[0153] Example 15

[0154] Examining K prepared in Example 8 + Response-type hydrogel strain sensors for rapid detection of K + Performance in this aspect.

[0155] Prepare K at concentrations of 1, 3, 5, 7, and 9 mmol / L (mM). + Aqueous solution. The K of the detection device from Example 11 was respectively... + The responsive hydrogel strain sensor was completely immersed in the above-mentioned different concentrations of K. +In the aqueous solution samples, the amount of each sample was the same, and the temperature was 32℃. The change of micro-strain (με) over time was recorded using a Wheatstone bridge module integrated data acquisition device. The results are as follows: Figure 16 As shown.

[0156] Depend on Figure 16 It can be seen that K + When the concentration is in the range of 1–9 mmol / L, K + All responsive hydrogel strain sensors exhibited a fast response of 2.0 min, with micro-strain and K... + Concentration linear correlation (see) Figure 15 (Figure (b)). This illustrates the K prepared in Example 8. + Response-type hydrogel strain sensors can quickly and effectively detect K + concentration.

[0157] Example 16

[0158] Examining K prepared in Example 8 + Performance of responsive hydrogel strain sensors in continuous detection.

[0159] Prepare K at concentrations of 1, 3, 5, 7, and 9 mmol / L (mM). + Aqueous solution. The K of the detection device from Example 11... + The responsive hydrogel strain sensor is fully immersed in 1 mmol / L K. + In aqueous solution, K + The aqueous solution was kept at 32°C for 5.0 min, and the change in micro-strain (με) over time was recorded using a Wheatstone bridge module integrated data acquisition device. The above operation was then repeated, sequentially adjusting K... + The concentrations of the aqueous solution were increased to 3, 5, 7, and 9 mmol / L. The results are as follows: Figure 17 As shown.

[0160] Depend on Figure 17 It can be seen that during the entire testing process in this embodiment, K + The microstrain of the responsive hydrogel strain sensor exhibits characteristics similar to K + The gradual change trend closely correlated with the concentration increment demonstrates excellent rapid response characteristics. This indicates that K + Response-type hydrogel strain sensors can achieve K + Rapid and efficient detection of concentration.

[0161] Example 17

[0162] Examining K prepared in Example 8 + Performance of responsive hydrogel strain sensors in the detection of trace serum samples.

[0163] The K of the detection device in Example 11 + The responsive hydrogel strain sensor was placed on a hot stage at 32°C, and a temperature reading of 32°C K was taken using a pipette. + 10 μL of a 3.8 mmol / L human serum sample was added dropwise to K. + K-type responsive hydrogel strain sensing + On the responsive hydrogel layer, after the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reaches stability, the corresponding micro-strain of each sample is recorded. Then, K is adjusted respectively. + The above procedure was repeated for the addition of human serum samples with a concentration of 3.8 mmol / L at volumes of 12, 14, 16, 18, and 20 μL. Then, K... + The concentration of human serum sample at 3.8 mmol / L was replaced with K. + Repeat the above procedure for human serum samples with concentrations of 4.6, 5.4, and 0 mmol / L.

[0164] Figure 18 K is used under different dropping conditions. + Response-type hydrogel strain sensor identifies different K + Microstrain at concentrations of human serum samples. When the volume of human serum sample is 10 μL, K + Response-type hydrogel strain sensors can now detect K+ in serum. + To produce an effective response; when the volume of human serum sample reaches 16–20 μL, it has an effect on K. + Human serum samples with concentrations of 3.8–5.4 mmol / L, K + The microstrain values ​​of the responsive hydrogel strain sensor remain essentially stable. This indicates that the K described in this invention... + A responsive hydrogel strain sensor requires only a single drop of serum sample (16–20 μL) to detect K+ in the serum sample. + Quantitative detection of concentration has extremely high application value in fields such as clinical testing.

[0165] Example 18

[0166] Examining K prepared in Example 8 + Interference resistance detection performance of responsive hydrogel strain sensors.

[0167] Normally, in human serum, except for K + Outside, Na + Ca 2+ and Mg 2+ Li is the most common and highly concentrated metal ion. + Cu 2+ Zn 2+ and Fe 3+Ba is an essential trace element for the human body. 2+ and Pd 2+ These are typical heavy metal ions harmful to human health. Therefore, these metal ions were selected as interfering ions for this study. In a real serum environment, Na... + The serum concentration ranged from 135 to 145 mmol / L, and the Ca concentration was... 2+ The concentration range is 2.25–2.75 mmol / L, Mg 2+ The concentration range is 0.8–1.0 mmol / L. The operation in this example is as follows:

[0168] (1) Prepare Li concentrations of 1, 3, 5, 7, and 9 mmol / L (mM) respectively. + Na + Mg 2+ Ca 2+ Cu 2+ Zn 2+ Ba 2+ Pd 2+ and Fe 3+ Aqueous solutions of metal ions were used as interfering ion solutions. K+ solutions with concentrations of 1, 3, 5, 7, and 9 mmol / L (mM) were prepared. + Aqueous solution.

[0169] The K of the detection device in Example 11 + The responsive hydrogel strain sensor was completely immersed in the above-mentioned K concentrations. + In both aqueous solution samples and samples containing interfering ions, the amount of each sample was the same, and the temperature was 32℃. After the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reached stability, the corresponding micro-strain for each sample was recorded. During testing, the tests were conducted in order of increasing ion concentration, and the same K0 was used for the same metal ion solution. + Response-type hydrogel strain sensing. Test results are as follows: Figure 19 As shown in Figure (a).

[0170] (2) At a concentration of 5 mmol / L K + Different concentrations of Na were added to the aqueous solution. + Mg 2+ and Ca 2+ Prepare a mixed ionic solution.

[0171] The K of the detection device in Example 11 +The responsive hydrogel strain sensor was completely immersed in mixed ionic solution samples of various concentrations, with identical sample volumes and a temperature of 32°C. After the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device stabilized, the corresponding micro-strain for each sample was recorded. Mixed solutions containing the same metal ions were treated with the same K0... + Response-type hydrogel strain sensing. Test results are as follows: Figure 19 As shown in Figure (b).

[0172] Depend on Figure 19 It can be seen that interfering metal ions with concentrations in the range of 1–9 mmol / L have an effect on K + Response-type hydrogel strain sensing detection K + The performance impact is negligible, K + The detection performance of responsive hydrogel strain sensors is almost unaffected by high concentrations of interfering ions. + Response-type hydrogel strain sensor in detecting K + It exhibits excellent anti-interference performance at certain concentrations.

[0173] Example 19

[0174] Examining K prepared in Example 8 + Repeat detection performance of responsive hydrogel strain sensor.

[0175] Prepare two sets of samples: one set of deionized water and the other set of K+ with a concentration of 5 mmol / L. + Aqueous solution.

[0176] First, the K of the detection device in Example 11... + The responsive hydrogel strain sensor was completely immersed in deionized water at 32°C. After the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reached stability, the micro-strain was recorded. K... + Switching to K-type responsive hydrogel strain sensor + In aqueous solution, after the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reaches stability, the micro-strain is recorded, and K is... + The responsive hydrogel strain sensor was switched to deionized water. Once the micro-strain (με) measured by the Wheatstone bridge module integrated data acquisition device reached a stable value, the micro-strain was recorded. This process was repeated until 12 measurements were completed. The test results are as follows: Figure 20 As shown.

[0177] Depend on Figure 20 It can be seen that when K + Response hydrogel strain sensor immersed in K +After being immersed in aqueous solution, its micro-strain signal changes rapidly, rising quickly and reaching a stable level within 2.0 minutes. When one test of K is completed... + After the detection of the aqueous solution, K + After the responsive hydrogel strain sensor was removed and quickly immersed in deionized water, K could be observed. + The microstrain signal of the responsive hydrogel strain sensor gradually decreased and recovered to its initial state in deionized water within approximately 8 minutes. Switching back to K... + After being placed in aqueous solution, the microstrain curve rose rapidly and then stabilized. After switching to deionized water, the microstrain curve gradually returned to the initial baseline. Over 12 cycles, K... + The detection performance of the responsive hydrogel strain sensor remained consistently stable, demonstrating the effectiveness of the K-type sensor. + The responsive hydrogel strain sensor exhibits excellent repeatability under alternating concentrations, a characteristic that makes it suitable for applications such as clinical testing of K... + It has great application potential and value in fields where the accuracy and reliability of concentration detection are extremely high.

[0178] Example 20

[0179] Examining K prepared in Example 8 + Performance of a responsive hydrogel strain sensor in detecting trace serum samples under different temperature conditions.

[0180] (1) Preparation of standard samples

[0181] Prepare a series of K + Serum standard samples of different concentrations, specifically: K + Human serum standard samples with concentrations of 3.8, 4.6, and 5.4 mmol / L (mM).

[0182] (2) Determine K + Conversion formula between concentration and microstrain

[0183] The K of the detection device in Example 11 + The responsive hydrogel strain sensor was placed on a hot stage at 25°C, according to K... + In ascending order of concentration, 20 μL of the standard sample at 25 °C was taken sequentially using a pipette and added evenly to the Kc. + K of responsive hydrogel strain sensor + On the responsive hydrogel layer, after the microstrain (με) measured by the Wheatstone bridge module integrated data acquisition device reaches stability, the microstrain corresponding to each standard sample is recorded. The microstrain corresponding to each standard sample is plotted as the ordinate, and the K-value of each standard sample is plotted as the ordinate. +Plot a working curve with concentration on the x-axis to determine K at a detection temperature of 25℃. + Concentration ([K) + The conversion relationship between με and microstrain is as follows: με = -115.39 × [K] + -0.136.

[0184] Replace with a new K + The responsive hydrogel strain sensor, following the above procedure, yields K at a detection temperature of 30℃. + The conversion formula between concentration and microstrain is as follows: με=-143.37×[K + -0.3052.

[0185] Replace with a new K + The responsive hydrogel strain sensor, following the above procedure, yields K at a detection temperature of 32℃. + The conversion formula between concentration and microstrain is as follows: με=-163.23×[K + -0.1209.

[0186] Replace with a new K + The responsive hydrogel strain sensor, following the above procedure, yields K at a detection temperature of 35℃. + The conversion formula between concentration and microstrain is as follows: με=-173.56×[K + +0.0799.

[0187] Replace with a new K + The responsive hydrogel strain sensor, following the above procedure, yields K at a detection temperature of 40℃. + The conversion formula between concentration and microstrain is as follows: με=-197.3×[K + -5.0331.

[0188] (3) Detection of serum potassium concentration in the test sample

[0189] Replace with a new K + A responsive hydrogel strain sensor is used, replacing the standard sample in step (2) with the test sample (serum sample). The micro-strain corresponding to the test sample is measured according to the operation in step (2), and the K is determined in step (2). + The conversion formula between concentration and microstrain is used to calculate K of the test sample. + concentration.

[0190] The detection temperature used in step (3) is the same as the detection temperature used when plotting the working curve in step (2). The temperature is determined by K based on the micro-strain corresponding to the test sample. + The conversion formula between concentration and microstrain is used to calculate K of the test sample. +When determining the concentration, K at the appropriate detection temperature should be used. + The conversion relationship between concentration and microstrain is used for calculation.

[0191] (4) K at different detection temperatures + Response-type hydrogel strain sensor for detecting K in serum + Plotting the micro-strain reference standard spectrum of concentration

[0192] Considering human serum K + The normal concentration range is 3.5–5.5 mmol / L. This step uses K... + Human serum samples at concentrations of 3.8, 4.6, and 5.4 mmol / L (mM) were tested at different detection temperatures.

[0193] Replace with a new K + A responsive hydrogel strain sensor is used, replacing the standard sample in step (2) with the sample prepared in this step, and the micro-strain corresponding to the sample is measured according to the operation in step (2). Based on K... + Microstrain of samples with concentrations of 3.8, 4.6, and 5.4 mmol / L at different detection temperatures is plotted with detection temperature on the x-axis and microstrain on the y-axis, and Kelvin on the y-axis. + The microstrain corresponding to a sample with a concentration of 5.5 mmol / L is taken as the upper limit of the normal range of microstrain, expressed in K. + The microstrain value corresponding to the sample with a concentration of 3.8 mmol / L is used as the lower limit of the normal range of microstrain. K is plotted at different detection temperatures. + Response-type hydrogel strain sensor for detecting K in serum + Micro-strain reference standard spectrum of concentration.

[0194] Figure 21 (a) The figure shows the microstrain of serum samples obtained at different detection temperatures. Figure 21 Graph (b) shows the effect of temperature and blood potassium concentration on K. + A diagram illustrating the combined effects of a responsive hydrogel strain sensor on serum potassium levels. Figure 21 Figure (c) shows K at different detection temperatures. + Response-type hydrogel strain sensor for detecting K in serum + Micro-strain reference standard spectrum of concentration. Figure 21 Figure (c) shows the microstrain ranges corresponding to hyperkalemia, hypokalemia, and normal serum potassium at different detection temperatures. This figure can provide a basis for subsequent clinical applications to quickly determine whether the serum potassium level of a sample is normal.

[0195] Example 21

[0196] In this embodiment, K is provided. +A responsive hydrogel strain sensor and its fabrication method.

[0197] K + The structure of the responsive hydrogel strain sensor is the same as that of K in Example 8. + The responsive hydrogel strain sensors are basically the same, except that the substrate is a surface-silanized modified epoxy resin substrate; K + The thickness of the responsive hydrogel layer 1 is 0.2 mm. K + The preparation method of the responsive hydrogel strain sensor differs from that of Example 8 only in that: the silane coupling agent used is vinyltriethoxysilane; in the gel prepolymer solution, the concentration of B15C5Am is 0.1 mol / L, the concentration of NIPAm is 0.5 mol / L, the volume concentration of the photoinitiator is 0.2%, the concentration of L-XLG is 0.01 mol / L; and the thickness of the template is 0.2 mm.

[0198] Example 22

[0199] In this embodiment, K is provided. + A responsive hydrogel strain sensor and its fabrication method.

[0200] K + The structure of the responsive hydrogel strain sensor is the same as that of K in Example 8. + The responsive hydrogel strain sensors are basically the same, except that the substrate is a phenolic resin substrate with surface silanization modification; K + The thickness of the responsive hydrogel layer 1 is 1 mm. K + The preparation method of the responsive hydrogel strain sensor differs from that of Example 8 only in that: the silane coupling agent used is vinyltris(2-methoxyethoxy)silane; in the gel prepolymer solution, the concentration of B15C5Am is 0.1 mol / L, the concentration of NIPAm is 2 mol / L, the volume concentration of the photoinitiator is 0.2%, and the concentration of L-XLG is 0.01 mol / L; the thickness of the template is 1 mm.

Claims

1. A type of K + A responsive hydrogel strain sensor, characterized in that, The strain sensor is made of K + The structure consists of a responsive hydrogel layer (1) and a resistance strain gauge (2). The resistance strain gauge (2) includes a substrate, a sensitive grid wire (3), a capping layer, and leads. The substrate is a surface-silanized modified synthetic resin substrate. + The responsive hydrogel layer (1) is chemically bonded to the substrate and completely covers the sensitive grid wire (3) of the resistance strain gauge (2); the K + The responsive hydrogel layer (1) has a gel polymer network composed of linear polymer poly(N-isopropylacrylamide- co -4-Acrylamide benzo-15-crown-5) is physically cross-linked with Laponite XLG nanosheets.

2. K according to claim 1 + A responsive hydrogel strain sensor, characterized in that, K + The responsive hydrogel layer (1) is made of K + Response hydrogel composition, K + The content of Laponite XLG nanosheets in the responsive hydrogel is 0.01~0.05 mol / L.

3. K according to claim 2 + A responsive hydrogel strain sensor, characterized in that, The K + The responsive hydrogel layer (1) is obtained by photoinitiated polymerization of a gel prepolymer. The gel prepolymer is obtained by fully dispersing the functional monomer 4-acrylamide benzo-15-crown-5, the gel monomer N-isopropylacrylamide and the photoinitiator in a Laponite XLG nanosheet dispersion. In the gel prepolymer, the molar ratio of 4-acrylamide benzo-15-crown-5 to N-isopropylacrylamide is (0.05~0.2):1, and the concentration of N-isopropylacrylamide monomer is 0.5~2 mol / L.

4. K according to any one of claims 1 to 3 + A responsive hydrogel strain sensor, characterized in that, K + The thickness of the responsive hydrogel layer (1) is 0.2~1 mm.

5. K according to any one of claims 1 to 3 + The responsive hydrogel strain sensor, wherein the resistance strain gauge (2) is a thin-film resistance strain gauge.

6. K according to any one of claims 1 to 3 + A responsive hydrogel strain sensor, characterized in that, The surface-silanized modified synthetic resin substrate is obtained by grafting a synthetic resin substrate with a silane coupling agent containing carbon-carbon double bonds after plasma treatment.

7. K according to claim 6 + A responsive hydrogel strain sensor, characterized in that, The silane coupling agents containing carbon-carbon double bonds include 3-(methacryloyloxy)propyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, or γ-methacryloyloxypropyltrimethoxysilane.

8. K according to any one of claims 1 to 3 + A responsive hydrogel strain sensor, characterized in that, The synthetic resin substrate includes a polyimide substrate, a phenolic resin substrate, a phenolic-acetal resin substrate, an epoxy resin substrate, or a polyester resin substrate.

9. A rapid and convenient quantitative detection method for trace amounts of blood potassium, characterized in that, Includes the following steps: ①K as described in any one of claims 1 to 8 + The responsive hydrogel strain sensor is connected to the Wheatstone bridge module integrated data acquisition device (5) to form a detection device; ②Prepare a series of K + Standard samples of different concentrations will be used in the K detector. + The responsive hydrogel strain sensor is placed on a hot stage, according to K + The concentration is arranged from low to high, towards K. + K of responsive hydrogel strain sensors + Standard samples were sequentially and uniformly dropped onto the responsive hydrogel layer. After the microstrain measured by the Wheatstone bridge module integrated data acquisition device reached stability, the microstrain corresponding to each standard sample was recorded; thus, a series of microstrains corresponding to the standard samples were obtained. Using the micro-strain corresponding to each standard specimen as the ordinate, and the K of each standard specimen as the coordinate... + Plot the working curve with concentration on the x-axis and determine K. + The conversion formula between concentration and microstrain; ③ Use the same K as in step ① + The responsive hydrogel strain sensor replaces the K sensor used in step ②. + Response-type hydrogel strain sensor, or K after step ② + K of responsive hydrogel strain sensors + The responsive hydrogel layer was restored to its state before the test in step ②; Replace the standard sample in step ② with the sample to be tested, and measure the micro-strain of the sample to be tested according to the operation in step ②. Based on K determined in step ②, + The conversion formula between concentration and microstrain is used to calculate K of the test sample. + concentration; In steps ② and ③, the temperature of the standard sample and the test sample is controlled to be the same as the temperature of the hot stage. The temperature of the hot stage is controlled to be a constant value between 25 and 40°C. The amount of standard sample and test sample added is controlled to be the same. The test sample is a serum sample.

10. The rapid and convenient quantitative detection method for trace blood potassium according to claim 9, characterized in that, In steps ② and ③, the amount of standard sample and test sample added should be at least K. + The responsive hydrogel layer provides complete coverage.

Citation Information

Patent Citations

  • Stimulus-responsive ionic conductive hydrogel as well as preparation method and application thereof

    CN119119514A

  • Hydrogel electrochemical strain sensor and preparation method and application thereof

    CN119509336A