Gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots and preparation method thereof

By introducing p-type NiO quantum dots and n-type β-Ga2O3 into the gallium oxide ultraviolet detector to form a pn heterojunction, optimizing light absorption and carrier separation, the contradiction between the response and response speed of traditional gallium oxide ultraviolet detectors is solved, and efficient ultraviolet photoelectric detection is achieved.

CN120152400AActive Publication Date: 2025-06-13XIDIAN UNIV HANGZHOU RES INST +1

Patent Information

Application Number
CN202510593617.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2025-06-13
Estimated Expiration
2045-05-09

AI Technical Summary

Technical Problem

There is a contradiction between the responsiveness and response speed of traditional gallium oxide ultraviolet detectors, which is difficult to improve the photoresponsiveness and response speed at the same time, and there is a carrier recombination effect, affecting the stability and repeatability of the device.

Method used

By introducing p-type NiO quantum dots and n-type β-Ga2O3 to form a pn heterojunction, a gallium oxide sun-blind ultraviolet detector based on nickel oxide quantum dots is formed, which optimizes light absorption and carrier separation and reduces the recombination effect.

Benefits of technology

It significantly improves the photoresponsiveness and response speed of the gallium oxide daily blind ultraviolet detector, shortens the rise time and fall time, improves the stability and repeatability of the device, and solves the contradiction between responsiveness and response speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120152400A_ABST
    Figure CN120152400A_ABST
Patent Text Reader

Abstract

The invention provides a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots and a preparation method thereof. The preparation method comprises the following steps: S1, cleaning and drying a substrate on which gallium oxide grows; s2, performing etching on the surface of the gallium oxide to form a beta-Ga2O3 channel; s3, depositing laminated metal on the substrate as an electrode, and annealing to alloy the laminated metal so as to form ohmic contact with the gallium oxide; and S4, spin-coating p-type NiO quantum dots between the electrodes, introducing the p-type NiO quantum dots and the n-type beta-Ga2O3 through quantum dot integration to form a pn heterojunction gallium oxide ultraviolet detector, and improving the light responsivity and the response speed of the gallium oxide solar blind ultraviolet detector at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of gallium oxide solar-blind ultraviolet detectors, and particularly to a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots and a preparation method thereof. Background Art

[0002] Ultraviolet photodetectors have been widely used in many fields such as environmental monitoring, space science, flame detection, national security, etc. The ultraviolet spectrum can be divided into UVA (320 - 400 nm), UVB (280 - 320 nm) and UVC (100 - 280 nm) bands according to wavelength. Among them, the UVC band has become an ideal band for achieving high-precision detection because of the weak absorption of the atmosphere to it.

[0003] Most traditional ultraviolet photodetectors rely on wide-bandgap semiconductor materials such as Mg x Zn 1-x O, Al x Ga 1-x N, diamond, etc. Although these materials have certain light response characteristics in the ultraviolet band, they generally have problems of slow response speed and low light responsivity. For example, in some environmental monitoring scenarios with extremely high real-time requirements, the slow response speed of traditional detectors may lead to the inability to capture the rapid change of ultraviolet intensity in the environment in time. When detecting weak ultraviolet light, the low light responsivity makes it difficult for the detector to accurately detect the signal, affecting the accuracy of data.

[0004] In recent years, β -Ga 2 O 3 has emerged as a new type of wide-bandgap semiconductor material. Its bandgap width is as high as 4.9 eV, and it shows excellent light response performance and stability in the ultraviolet to deep ultraviolet bands, becoming a very potential candidate material for UVC photodetectors. Especially in the UVC band, β -Ga 2 O 3 has a high absorption efficiency, can capture ultraviolet light signals more effectively, and has stable performance, suitable for ultraviolet detection work with strict precision requirements.

[0005] However, gallium oxide has the problem of low intrinsic carrier mobility (<10 cm² / V·s), which severely limits the transport efficiency of photo-generated charges and further restricts the improvement of the device response speed. In previous gallium oxide ultraviolet detectors, although they have excellent light response performance in the ultraviolet band, they have always faced the contradiction between responsivity and response speed. To improve the light responsivity, a common approach is to increase the thickness of the light absorption layer or optimize the light absorption characteristics of the material. However, this will increase the carrier migration distance and lead to a decrease in the response speed. Moreover, a high light responsivity is prone to cause carrier recombination effects, especially when the carrier migration path is long, the recombination rate increases significantly, further slowing down the response speed.

[0006] In addition, traditional gallium oxide ultraviolet detectors mostly adopt the metal-semiconductor-metal (MSM) structure. This structure has certain limitations in pursuing high sensitivity and ultrafast response. Although the performance can be improved to a certain extent by improving the material quality and optimizing the device design, the balance problem between responsivity and response speed remains difficult to overcome. This bottleneck restricts the application of gallium oxide ultraviolet detectors in high-performance fields.

[0007] Therefore, there is an urgent need to explore new methods to optimize the device performance, achieve the effect of simultaneously improving the light responsivity and response speed, and effectively suppress the recombination effect. Summary of the Invention

[0008] The purpose of the present invention is to provide a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots and a preparation method thereof. By integrating quantum dots, a p-type NiO quantum dot and an n-type β -Ga 2 O 3 are used to form a pn heterojunction gallium oxide ultraviolet detector, which simultaneously improves the light responsivity and response speed of the gallium oxide solar-blind ultraviolet detector.

[0009] To achieve the above purpose, the present technical solution provides a preparation method of a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, including the following steps: S1: Clean and dry the substrate grown with gallium oxide; S2: Etch the surface of gallium oxide to form β -Ga 2 O 3 channels; S3: Deposit a stacked metal on the substrate as an electrode, and anneal to alloy the stacked metal to form an ohmic contact with gallium oxide; S4: Spin-coat p-type NiO quantum dots between the electrodes.

[0010] In addition, the present solution provides a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, including: Substrate; Gallium oxide grown on a substrate; Electrodes deposited on both sides of the gallium oxide and forming ohmic contacts with the gallium oxide, where the electrodes are laminated metals; p-type NiO quantum dots spin-coated on the top surface of the gallium oxide and located between the two electrodes.

[0011] Compared with the prior art, the present technical solution has the following characteristics and beneficial effects: The manufacturing process of the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots provided by the present invention is simple. By introducing p-type NiO quantum dots (NQDs) and β -Ga 2 O 3 forming a type-II heterojunction, the performance of the gallium oxide solar-blind ultraviolet detector is significantly improved. First of all, the NQDs enhance the absorption of ultraviolet light, especially in the UVC band, improving the optical responsivity and detectivity of the device, while maintaining a fast response speed. By optimizing the light absorption and carrier separation, the rise time and fall time of the device are greatly shortened, being 0.024 seconds and 0.008 seconds respectively, greatly improving the response speed. Secondly, the built-in electric field in the type-II heterojunction structure effectively promotes the separation and transport of photo-generated carriers, reducing the recombination effect, thereby improving the stability and repeatability of the device. In addition, the surface passivation effect of the NQDs reduces the defect recombination, further enhancing the long-term stability of the device. This design provides a new idea for the development of high-performance ultraviolet photodetectors, solves the contradiction between responsivity and response speed, has broad application prospects, and provides a new idea for the design and optimization of high-performance gallium oxide solar-blind photodetectors. Description of the Drawings

[0012] Figure 1 is a schematic structural diagram of the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots prepared by this solution.

[0013] Figure 2 is the I-V curve obtained by testing the conventional MSM-type gallium oxide ultraviolet detector and the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots under 250 nm 1 μW / cm 2 ultraviolet light.

[0014] Figure 3 is the multi-period I-t curve of the conventional MSM-type gallium oxide ultraviolet detector and the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots under 250 nm ultraviolet light.

[0015] Figure 4 is the rising and decaying edge diagram of the I-t curve of the conventional MSM-type gallium oxide ultraviolet detector and the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots under 250 nm ultraviolet light. Detailed implementation mode

[0016] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art belong to the scope of protection of the present invention.

[0017] Those skilled in the art should understand that in the disclosure of the present invention, the orientation or positional relationship indicated by terms such as "longitudinal", "transverse", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc. is based on the orientation or positional relationship shown in the accompanying drawings. It is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, the above terms should not be construed as limiting the present invention.

[0018] Embodiment 1 This solution provides a preparation method of a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, including the following steps: S1: Clean and dry the substrate on which gallium oxide is grown; S2: Etch the surface of gallium oxide to form β -Ga 2 O 3 channel; S3: Deposit a stacked metal on the substrate as an electrode, and anneal to alloy the stacked metal to form an ohmic contact with gallium oxide; S4: Spin-coat p-type NiO quantum dots between the electrodes.

[0019] In step S1, the material of the substrate is selected from one of sapphire, silicon, silicon carbide, and quartz. In a preferred embodiment, the material of the substrate is selected from sapphire.

[0020] As Figure 1 shown, gallium oxide grows on the substrate and there is a gap with the side of the substrate. In some embodiments, the thickness of gallium oxide is 424 ± 5 nm, and the thickness of the substrate is 100 ± 5 um.

[0021] In some embodiments, the substrate is ultrasonically cleaned with acetone, isopropyl alcohol, and deionized water for 5 minutes respectively, and then dried with a nitrogen gun after cleaning. In addition, after cleaning the substrate, it is further cleaned with a piranha solution for a period of time to remove the dangling bonds, surface states, and stubborn contaminants existing on the surface of the substrate. The piranha solution in this solution is a solution of concentrated sulfuric acid and hydrogen peroxide mixed in a ratio of 3:1, and the piranha solution can be used for 30 minutes.

[0022] In step S2, a channel image is formed by photolithography on the surface of gallium oxide and etched to form a β -Ga 2 O 3 channel. Specifically, a layer of photoresist is evenly coated on the surface of gallium oxide. The mask plate with the channel pattern is precisely aligned with the substrate coated with photoresist, and then irradiated with light of a specific wavelength. The light passes through the pattern on the mask plate, causing a chemical reaction in the photoresist. The exposed substrate is placed in the developer, and the chemically changed part of the photoresist exposed to light will be dissolved, thus transferring the channel pattern on the mask plate to the photoresist, forming the pattern of the channel on the photoresist layer. Subsequently, gallium oxide is etched using the photoresist pattern as a mask. During the etching process, the surface part of gallium oxide not covered by the photoresist will be gradually removed, thereby forming a channel corresponding to the photoresist pattern on the surface of gallium oxide.

[0023] In some embodiments, step S2 is etched using one or a combination of inductively coupled plasma etching or reactive ion etching.

[0024] When step S2 is etched using inductively coupled plasma etching, the etching gas is BCl 3 and one or more of Ar. Preferably, the flow rate of BCl 3 is 20 sccm, the flow rate of Ar is 10 sccm, the etching pressure is 15 mTorr, the radio frequency power is 10 W, the ICP power is 80 W, and the etching time is 30 s.

[0025] In some embodiments, the length of the channel etched in step S2 is 180 ± 5 um and the width is 30 ± 5 um. Preferably, the length of the channel etched in step S2 is 180 um and the width is 30 um.

[0026] In some embodiments, the thickness of the channel etched in step S2 is 420 ± 5 nm. Preferably, the thickness of the channel etched in step S2 is 420 nm.

[0027] In step S3, an electrode pattern is formed by photolithography, a laminated metal is deposited on the substrate as an electrode, and annealing is performed to alloy the laminated metal to form an ohmic contact with gallium oxide.

[0028] In some embodiments, electron beam evaporation, thermal evaporation or magnetron sputtering is used to deposit a laminated metal on the substrate as an electrode. Preferably, magnetron sputtering is used to deposit a laminated metal on the substrate as an electrode.

[0029] In some embodiments, a standard ultraviolet photolithography is used to form the electrode pattern.

[0030] In some embodiments, the material of the stacked metal is selected from one of Ti / Au and Ti / Al / Ni / Au. In a preferred embodiment, the material of the stacked metal is the Ti / Au stacked metal.

[0031] As Figure 1 shown, in this solution, the stacked metal is deposited on both sides of gallium oxide, and the bottom of the stacked metal on each side of gallium oxide covers the top surface of the substrate, and the top covers both ends of the top surface of gallium oxide and contacts the side surface of gallium oxide.

[0032] In some embodiments, the stacked metal covers both ends of the top surface of gallium oxide by 20 μm.

[0033] In some embodiments, the stacked metals deposited on both sides of gallium oxide are symmetrically arranged with respect to gallium oxide.

[0034] In addition, this solution uses a rapid thermal annealing equipment (RTP) or a tube annealing furnace equipment to anneal the deposited stacked metal to alloy the stacked metal to form an ohmic contact with gallium oxide. Preferably, when using the rapid thermal annealing equipment (RTP) to anneal the deposited stacked metal, it is annealed for 1 min at an annealing temperature of 470 °C in a nitrogen atmosphere.

[0035] After annealing, this solution forms a lateral MSM structure, where the lateral MSM structure uses gallium oxide as the semiconductor layer and the electrodes on both sides as metal electrodes. When the detector is irradiated with solar-blind ultraviolet light, gallium oxide absorbs the photon energy. If the photon energy is greater than the bandgap of the semiconductor, electron-hole pairs will be generated. These electron-hole pairs are the photo-generated carriers. After applying a bias voltage across the metal electrodes, a lateral electric field will be formed in the semiconductor layer. Under the action of this lateral electric field, the photo-generated electrons and holes move towards the positive and negative electrodes respectively and are finally collected by the electrodes to form a photocurrent. By detecting the magnitude of the photocurrent, the detection of ultraviolet light signals can be achieved.

[0036] In step S4, a p-type NiO solution is spin-coated between the electrodes on the top surface of gallium oxide to form p-type NiO quantum dots.

[0037] In some embodiments, lithography defines Ga 2 O 3The pattern of the area where NiO quantum dots are required on the thin film is placed in the middle of the chuck of the spin coater. The vacuum pump is turned on to evacuate the air, and the thin film is adsorbed and fixed on the chuck. Use a pipette to extract 15 μL of the precursor solution and drop it on the surface of the thin film. The spin coating is divided into two parts. The first part rotates at a speed of 550 revolutions per minute for 15 seconds, and the second part rotates at a speed of 2500 revolutions per minute for 45 seconds. Rotating at two different speeds can obtain a more uniform thin film. After spin coating, it is placed on the annealing table in the fume hood for annealing. The annealing temperature is 100 °C and the duration is 20 minutes, and then it is peeled off in acetone to obtain the lithographed NiO quantum dot area.

[0038] In some embodiments, the concentration of the p-type NiO solution is 20 g / L.

[0039] In some embodiments, the density of the quantum dots is 3.67×10 17 per square centimeter, and the thickness is 24 nm.

[0040] This solution introduces p-type NiO quantum dots and n-type β -Ga 2 O 3 to form a pn heterojunction gallium oxide ultraviolet detector. Among them, due to its small size and high specific surface area, NiO quantum dots can effectively enhance the absorption of ultraviolet light, especially in the deep ultraviolet (UVC) band. Compared with NiO thin films, quantum dots can capture and absorb ultraviolet light more efficiently, thereby improving the responsivity of the photodetector, enabling the device to maintain high sensitivity even under low light conditions, and the introduction of quantum dots can effectively improve the carrier separation efficiency, especially in the case of forming a heterojunction.

[0041] Moreover, in the type-II heterojunction structure formed by the NiO quantum dots of this solution and β -Ga 2 O 3 due to the size effect of the quantum dots, it can accelerate the separation and transport of photo-generated carriers, thereby significantly shortening the rise time and fall time (rise time 0.024 s, fall time 0.008 s), improving the response speed. This solves the problem of slow carrier migration speed in traditional nickel oxide thin films, enabling the photodetector to perform excellently in fast response applications, and successfully solving the trade-off problem between optical response and response speed in traditional structures.

[0042] In addition, the surface states of nickel oxide quantum dots are relatively many, but due to their high specific surface area and size effect, surface passivation can effectively reduce surface defects and recombination effects. Compared with nickel oxide thin films, the surface defects of quantum dots are fewer, and through the surface passivation of quantum dots, the stability and repeatability of the device have been significantly improved. This enables quantum dots to improve the stability of the photodetector while reducing the performance degradation during long-term operation.

[0043] In summary, by optimizing light absorption and carrier transport, this method successfully overcomes the defects of traditional gallium oxide detectors, achieving a dual improvement in responsivity and response speed. Moreover, compared with the method of depositing NiO growth films, the method of spin-coating NiO quantum dots has a simpler process flow and lower cost.

[0044] Example Two As Figure 1 shown, this solution provides a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, prepared according to the above method, including: A substrate; Gallium oxide grown on the substrate; Electrodes deposited on both sides of gallium oxide and forming ohmic contacts with gallium oxide, where the electrodes are laminated metals; P-type NiO quantum dots spin-coated on the top surface of gallium oxide and located between the two electrodes.

[0045] Regarding the same content as in Example One in this Example Two, it will not be repeated and explained in a cumbersome manner.

[0046] Example Three In order to verify the performance optimization of the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots in this solution compared with the conventional MSM-type gallium oxide ultraviolet detector, the following example is designed The gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots in this solution: Step (1): Ultrasonically clean gallium oxide grown on sapphire material with acetone, isopropyl alcohol, and deionized water for 5 min respectively. After organic cleaning, use piranha solution (concentrated H 2 SO 4 :H 2 O 2 =3:1) to clean for 30 min, and then dry with a nitrogen gun after cleaning; Step (2): Lithographically form a channel pattern, and use the ICP method to etch a channel on the substrate, where the BCl 3 flow rate is 20 sccm, the Ar flow rate is 10 sccm, the etching pressure is 15 mTorr, the radio frequency power is 10 W, the ICP power is 80 W, and the etching time is 30 s; Step (3): Lithographically form an electrode pattern, use magnetron sputtering to deposit a Ti / Au laminated metal, and strip to form an electrode; Step (4): Use the RTP method to form an ohmic contact, and anneal for 1 min in a nitrogen atmosphere at an annealing temperature of 470 °C; Step (5): Lithographically define Ga 2 O 3The area pattern of NiO quantum dots is required on the thin film. Place it in the middle of the chuck of the spin coater, turn on the vacuum pump to evacuate, and the thin film is adsorbed and fixed on the chuck. Use a pipette to extract 15 μL of the precursor solution and drop it on the surface of the thin film. The spin coating is divided into two parts. The first part rotates at a speed of 550 revolutions per minute for 15 seconds, and the second part rotates at a speed of 2500 revolutions per minute for 45 seconds. Rotation at two different speeds can obtain a more uniform thin film. After spin coating, place it on the annealing table in the fume hood for annealing at an annealing temperature of 100 °C for 20 minutes, and complete the stripping in acetone to obtain the lithographed NiO quantum dot area.

[0047] Conventional MSM-type gallium oxide ultraviolet detector: Step (1): Ultrasonically clean gallium oxide grown on sapphire material in acetone, isopropyl alcohol, and deionized water for 5 min respectively. After organic cleaning, use piranha solution (concentrated H 2 SO 4 :H 2 O 2 =3:1) to clean for 30 min, and blow dry with a nitrogen gun after cleaning; Step (2): Lithographically form a channel pattern, and use the ICP method to etch a channel on the substrate. Among them, the flow rate of BCl 3 is 20 sccm, the flow rate of Ar is 10 sccm, the etching pressure is 15 mTorr, the radio frequency power is 10 W, the ICP power is 80 W, and the etching time is 30 s; Step (3): Lithographically form an electrode pattern, use magnetron sputtering deposition technology to deposit a Ti / Au stacked metal, and strip to form an electrode; Step (4): Use the RTP method to form an ohmic contact, and anneal in a nitrogen atmosphere at an annealing temperature of 470 °C for 1 min.

[0048] Place the conventional MSM-type gallium oxide ultraviolet detector and the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots of the present invention under 250 nm 1 μW / cm 2 ultraviolet light for testing to obtain the I-V curve as Figure 2 shown, the I-t curve under 250 nm ultraviolet light is as Figure 3 shown, and the rising and decay edges of the I-t curve under 250 nm ultraviolet light are as Figure 4 shown. It can be seen that the gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots of this solution solves the contradiction between the responsivity and the response speed.

[0049] Those skilled in the art should understand that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity of description, not all possible combinations of the technical features in the above embodiments are described. However, as long as the combinations of these technical features do not conflict, they should all be considered to be within the scope described in this specification.

[0050] The above embodiments merely illustrate several implementation manners of the present application. The description thereof is relatively specific and detailed, but it should not be construed as a limitation to the scope of the present application. It should be noted that for those of ordinary skill in the art, without departing from the concept of the present application, several modifications and improvements can still be made, and these all fall within the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the appended claims.

Claims

1. A method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, characterized in that: The following steps are involved: S1: cleaning and drying the substrate on which gallium oxide is grown; S2: Etching on the surface of gallium oxide β -Ga2O3 channel; S3: depositing a stacked metal as an electrode on the substrate, and annealing the stacked metal to alloy the stacked metal to form an ohmic contact with gallium oxide; S4: Spin coating p-type NiO quantum dots between electrodes.

2. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: Gallium oxide grows on a substrate with a gap between the gallium oxide film and the substrate. The thickness of the gallium oxide film is 424±5 nm, and the thickness of the substrate is 100±5 um.

3. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: The length of the channel formed by etching in step S2 is 180±5 um and the width is 30±5 um.

4. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: The channel intervals formed by etching in step S2 are arranged laterally in the gallium oxide layer, and the channels are connected to the substrate.

5. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: A stacked metal is deposited on both sides of the gallium oxide, and the bottom of the stacked metal on each side of the gallium oxide covers the top surface of the substrate, and the top covers the top surface of the gallium oxide and contacts the side surface of the gallium oxide.

6. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: After annealing, a lateral MSM structure is formed, wherein the lateral MSM structure uses gallium oxide as a semiconductor layer and electrodes on both sides are metal electrodes.

7. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: The spin coating was divided into two parts, the first part was spun at 550 rpm for 15 sec, and the second part was spun at 2500 rpm for 45 sec.

8. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: The concentration of the p-type NiO solution was 20 g / L.

9. The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to claim 1, characterized in that: The density of quantum dots is 3.67×10 17 / square centimeter, and the thickness is 24 nm.

10. A gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots, characterized in that: The method for preparing a gallium oxide solar-blind ultraviolet detector based on nickel oxide quantum dots according to any one of claims 1 to 9 above comprises: substrate; Gallium oxide grown on a substrate; Electrodes deposited on both sides of the gallium oxide and forming ohmic contact with the gallium oxide, wherein the electrodes are laminated metals; p-type NiO quantum dots spin-coated on the top surface of gallium oxide and located between two electrodes.

Citation Information

Patent Citations

  • Ultraviolet photoelectric detector and preparation method thereof

    CN110265504A

  • Self-powered gallium oxide solar blind detector and preparation method thereof

    CN117525198A

Cited By

  • Gallium oxide photoelectric detector preparation method for enhancing synaptic effect based on reactive ion etching