Asymmetric magnetic mesoporous carbon superstructure material as well as preparation method and application thereof

By designing and preparing asymmetric magnetic mesoporous carbon superstructure materials, the problems of limitation of structural symmetry and insufficient microcontrol of existing magnetic mesoporous carbon materials are solved, and the efficient catalytic degradation performance and selective adsorption ability of the material are achieved.

CN120189963APending Publication Date: 2025-06-24INNER MONGOLIA UNIVERSITY

Patent Information

Application Number
CN202510363798.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-26
Publication Date
2025-06-24

AI Technical Summary

Technical Problem

The existing magnetic mesoporous carbon materials have limitations on structural symmetry, and the magnetic components are wrapped by external composition, resulting in insufficient performance, especially in the fields of drug delivery and targeted therapy; in addition, insufficient structural control of the material at the microscopic or nanoscale limits its competitiveness in high-end applications.

Method used

Using the design and preparation method of asymmetric magnetic mesoporous carbon superstructure materials, SiO2 is grown in direction on Fe3O4 nanoparticles through CTAB as a structural guide, combined with PS-PVP-PEO single micelle and polydopamine, asymmetric magnetic nanocarbon particles are formed by using the single micelle interface assembly method to achieve accurate control of mesoporous size.

Benefits of technology

It improves the surface chemistry of the material, enhances hydrophilicity and catalytic degradation ability, is suitable for chemical catalytic degradation, avoids the generation of intermediate by-products, simplifies the synthesis process, and achieves selective catalytic degradation of organic pollutants of different molecular weights.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120189963A_ABST
    Figure CN120189963A_ABST
Patent Text Reader

Abstract

The invention discloses an asymmetric magnetic mesoporous carbon superstructure material as well as a preparation method and application thereof. The preparation method comprises the following steps: (1) preparing Fe3O4amp; a SiO2 alcohol dispersion liquid; (2) preparing Fe3O4 < 4 > amp; the preparation method comprises the following steps: preparing a SiO2 (at) micro single micelle superstructure alcohol solution; (3) preparing Fe3O4 < 4 > amp; a SiO2 (at) C superstructure material; the specific surface area of the material is 87-116 m < 2 > / g, the aperture is 22.8-50 nm, and the length is 330-400 nm. The material is applied to catalytic degradation of organic dyes. The method has the beneficial effects that the surface chemical property is more active, the hydrophilicity and the catalytic degradation capability are stronger, the method is suitable for chemical catalytic degradation, the whole synthesis process is simple and convenient to operate, and intermediate byproducts cannot be generated to cause secondary pollution; in addition, in the dopamine carbonization process, high-temperature carbonization is carried out in nitrogen (inert atmosphere), and the operation is safe; by adjusting the type of the PS-PVP-PEO single micelle, accurate control of the mesoporous size can be realized, so that the PS-PVP-PEO single micelle is suitable for catalytic degradation of organic pollutants with different molecular weights, and selective catalytic degradation is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field:

[0001] This invention patent belongs to the technical field of nanomaterials, and particularly relates to an asymmetric magnetic mesoporous carbon superstructure material, its preparation method and application. Background Art:

[0002] In recent years, mesoporous carbon materials have shown extensive application potential in the fields of energy storage, catalysis, sensing, and environmental protection due to their unique pore structures, high specific surface areas, and adjustable pore sizes. These materials are usually synthesized by the template method, which can precisely control the pore size and specific surface area, providing a solid foundation for various applications. Nevertheless, mesoporous carbon materials still face challenges in functionalization, property regulation, and efficient application. To enhance the multifunctionality of mesoporous carbon materials, the research on magnetic mesoporous carbon materials has become increasingly important. This kind of material combines the electrical conductivity and mechanical strength of carbon materials with the adjustable properties of magnetic substances, showing potential application value in magnetic separation, drug delivery, magnetic catalysis, and electromagnetic shielding. The synthesis of magnetic mesoporous carbon materials usually involves adding magnetic substances, such as iron oxide, iron-based alloys, or rare earth metal oxides, during the preparation of mesoporous carbon, and optimizing the material properties by adjusting the content and distribution of these magnetic components. However, the existing magnetic mesoporous carbon materials have some limitations. Traditional materials often have symmetric structures, and the magnetic components are usually shielded by the outer composition, which may limit their performance in specific applications. For example, in the fields of drug delivery and targeted therapy, an asymmetric magnetic structure may be more ideal because it provides more degrees of freedom for control. In addition, the structural design of magnetic mesoporous carbon usually focuses on macroscopic properties and lacks precise control at the micro or nanoscale, which limits their competitiveness in high-end applications.

[0003] Among them, Patent No. 201710873510.3 discloses a preparation method and application of a nano zero-valent iron mesoporous carbon asymmetric structure material for removing persistent organic pollutants in water; specifically discloses. The preparation method is as follows: Hydrothermally prepare Fe3O4 magnetic nanoparticles with uniform size and easy dispersion; disperse the Fe3O4 magnetic nanoparticles in ethanol to obtain an Fe3O4 ethanol solution; disperse the Fe3O4 ethanol solution in a solution containing a surfactant, and then add an organosilicon source, and obtain a core-shell material with asymmetric organosilicon-coated magnetic nanoparticles through mechanical stirring and centrifugal separation; calcine and reduce the core-shell material at high temperature to obtain a core-shell material with a nano zero-valent iron mesoporous carbon asymmetric structure. The obtained nano zero-valent iron mesoporous carbon asymmetric structure material has uniform size, ordered pores, good dispersion, strong magnetism, the nano zero-valent iron is well protected, has good recyclability, and strong ability to remove persistent organic pollutants. However, the mesoporous carbon in this patent is prepared from an organosilicon source (silane coupling agent), and its molecular structure is mainly Si-O-C or Si-C bonds, and the carbon source mainly comes from the carbon chain in the organic matter. During the carbonization process, it is calcined at high temperature in a reducing atmosphere of H2 (gas with low molecular weight and extremely easy to explode) / Ar mixed gas. After carbonization, it mainly forms sp 2 carbon skeleton (graphite-like structure), with a small amount of oxygen-containing functional groups (such as hydroxyl groups, carboxyl groups) on the surface, and almost no nitrogen. And the functional groups are mainly composed of hydrophobic carbon layers, with few types of functional groups, focusing on physical adsorption, and the treatment efficiency for polar organic compounds (such as complex organic compounds with halogens and benzene rings) is limited. In addition, intermediate products may be generated during the reduction of nano zero-valent iron, such as chlorinated by-products, and these intermediate products are more toxic. If the intermediate products are not effectively treated, secondary pollution may be caused.

[0004] To solve these problems, researchers have begun to explore the design and preparation of asymmetric magnetic mesoporous carbon superstructures. The asymmetric structure can bring more surface and interface effects to the magnetic mesoporous carbon material, thereby improving its performance. For example, the asymmetric structure can promote the distribution of magnetic substances in a specific direction, increase the surface activity of the material, or enhance its response ability in a magnetic field. This enables asymmetric magnetic mesoporous carbon materials to be expected to exhibit more excellent performance in fields such as catalysis, drug delivery, sensing, and magnetic separation. Therefore, developing magnetic mesoporous carbon superstructures with asymmetric structures, adjustable magnetism, and excellent pore structures is of great scientific and engineering significance for improving their multifunctionality and expanding their application fields. Summary of the Invention:

[0005] In view of this, the object of the present invention is to provide an asymmetric magnetic mesoporous carbon superstructure material, a preparation method thereof and an application thereof. The material prepared by the preparation method provided by the present invention has more active surface chemical properties, stronger hydrophilicity and catalytic degradation ability, and is suitable for chemical catalytic degradation; the entire synthesis process is simple to operate and will not produce intermediate by-products to cause secondary pollution; by adjusting the type of PS-PVP-PEO single micelle, precise control of the mesopore size can be achieved, so that it is applicable to adsorb organic pollutants with different molecular weights and realize selective catalytic degradation.

[0006] One aspect of the technical solution of the present invention discloses a preparation method of an asymmetric magnetic mesoporous carbon superstructure material, which comprises the following steps:

[0007] (1) Prepare a Fe3O4&SiO2 alcohol dispersion: Disperse Fe3O4 nanoparticles and cetyltrimethylammonium bromide (CTAB) in a mass ratio of 3-7.5:10-15 into 20-40 mL of deionized water, stir and mix for 5-20 min and then ultrasonically mix for 20-40 min in sequence, then add 0.5-2 mL of ammonia water and 100-250 μL of tetraethyl orthosilicate (TEOS), and react in a stirred oil bath at 40-60 °C for 4-36 h; then centrifuge, wash with water, and wash with ethanol to obtain a Fe3O4&SiO2 alcohol dispersion with a concentration of 2-5 mg / mL;

[0008] (2) Prepare a Fe3O4&SiO2@micelle single micelle superstructure alcohol solution: Ultrasonically mix 10-20 mL of the Fe3O4&SiO2 alcohol dispersion in step (1) with 1-15 mL of a single micelle solution with a concentration of 1-20 mg / mL for 20-40 min, then add ammonia water to adjust the pH value to 8-12, and then stir and react at room temperature for 6-24 h; then centrifuge, wash with water, and wash with ethanol to obtain a Fe3O4&SiO2@micelle single micelle superstructure alcohol solution with a concentration of 1-10 mg / mL;

[0009] (3) Prepare a Fe3O4&SiO2@C superstructure material: Mix 5-15 mL of the Fe3O4&SiO2@micelle single micelle superstructure alcohol solution in step (2) with a bis(2-hydroxyethyl)amino tris(hydroxymethyl)methane (Tris) buffer solution with a concentration of 2-25 mg / mL to make the pH value of the solution 7-12, then add 2-10 mg of polydopamine (mPDA), and stir and react at room temperature for 6-24 h; then centrifuge, wash with water, wash with ethanol and dry, and the dried material is calcined in a nitrogen atmosphere to obtain an asymmetric Fe3O4&SiO2@C superstructure material.

[0010] First, using CTAB as a structure-directing agent, SiO2 is directionally grown on magnetic nanoparticles Fe3O4 to form an asymmetric Fe3O4&SiO2 structure; then, using the asymmetric Fe3O4&SiO2 structure as a substrate, PS-PVP-PEO single micelles as assembly units, and polydopamine as a carbon source, an asymmetric magnetic carbon nanoparticle is formed by the single micelle interface assembly method.

[0011] Further, the preparation method of the Fe3O4 nanoparticles in step (1) includes the following steps: adding 3 - 4.5 g of ferric chloride hexahydrate, 0.7 - 0.9 g of trisodium citrate, and 4.5 - 5.5 g of sodium acetate trihydrate to 110 - 220 mL of ethylene glycol, stirring well to dissolve; transferring the dissolved solution to a polytetrafluoroethylene inner liner, setting high-pressure and high-temperature conditions, reacting for 12 - 17 h, and then through centrifugation, washing with water, washing with ethanol, and drying, Fe3O4 nanoparticles with a particle size of 100 - 150 nm are obtained.

[0012] Further, the high-pressure condition is 10 - 15 MPa, and the high-temperature condition is 200 - 250 °C.

[0013] Further, the preparation method of the single micelle solution in step (2) includes the following steps: dissolving the block copolymer polystyrene-poly(4-vinylpyridine)-poly(ethylene oxide) (PEO-PVP-PS) in a solvent to obtain a block copolymer solution, then putting the block copolymer solution into an oven, keeping it at 30 - 110 °C for 3 - 10 h, and then naturally cooling to room temperature to obtain a single micelle solution.

[0014] Further, the polystyrene-poly(4-vinylpyridine)-poly(ethylene oxide) is one of PEO 113 -PVP 60 -PS 28 、PEO 113 -PVP 68 -PS 60 、PEO 113 -PVP 44 -PS 97 and PEO 113 -PVP 98 -PS 142 ; the solvent is one of acetic acid, absolute ethanol, water, DMF, and a mixture of water and DMF.

[0015] Further, the calcination process in step (3) is divided into two stages. The calcination temperature in the first stage is 330 - 450 °C, and the calcination time is 3 - 9 h. The calcination temperature in the second stage is 600 - 800 °C, and the calcination time is 3 - 12 h.

[0016] Further, the stirring speed in steps (1), (2), and (3) is 300 - 500 rpm; the frequency of ultrasonic mixing in steps (1) and (2) is 10 - 50 kHz.

[0017] Further, the centrifugation conditions in steps (1) - (3) and the process of preparing Fe3O4 nanoparticles: the centrifugation speed is 8000 - 15000 r / min, and the centrifugation time is 5 - 12 min; the washing conditions: wash with deionized water 3 - 6 times and wash with 95% ethanol solution 3 - 6 times.

[0018] Another aspect of the technical solution of the present invention discloses an asymmetric magnetic mesoporous carbon superstructure material with a specific surface area of 87 - 116 m 2 / g, a pore diameter of 22.8 - 50 nm, and a length of 330 - 400 nm.

[0019] Another aspect of the technical solution of the present invention discloses the application of an asymmetric magnetic mesoporous carbon superstructure material in the catalytic degradation of organic dyes, and the application is used for catalytically degrading the macromolecular organic dye Rhodamine B in wastewater.

[0020] Advantages of the present invention:

[0021] 1. The present invention discloses a preparation method of an asymmetric magnetic mesoporous carbon superstructure material. The synthesis of mesoporous carbon uses the carbonization of dopamine as a synthesis template. Dopamine is an organic compound containing benzene rings, amino groups, and hydroxyl groups, and its molecular structure is rich in C, N, and O. The amino group and benzene ring structure of dopamine are pyrolyzed to form a nitrogen-doped carbon material, retaining a large number of nitrogen-containing functional groups (pyridine nitrogen, pyrrole nitrogen, amino group) and oxygen-containing groups (hydroxyl group, carbonyl group). The surface chemical properties are more active, the hydrophilicity and catalytic degradation ability are stronger, and it is suitable for chemical catalytic degradation.

[0022] 2. The present invention discloses a preparation method of an asymmetric magnetic mesoporous carbon superstructure material. The entire synthesis process is simple to operate and will not produce intermediate by-products to cause secondary pollution. In addition, the carbonization process of dopamine is carried out by high-temperature carbonization in nitrogen (inert atmosphere), and the operation is safe.

[0023] 3. The present invention discloses a preparation method of an asymmetric magnetic mesoporous carbon superstructure material. By adjusting the type of PS-PVP-PEO single micelles, the precise control of the mesopore size can be achieved, and then it is suitable for catalytically degrading organic pollutants with different molecular weights, realizing selective catalytic degradation.

[0024] 4. The present invention discloses an asymmetric magnetic mesoporous carbon superstructure material with a large specific surface area. Spherical mesopores are regularly arranged on its carbon shell layer, greatly increasing the number of active sites. Moreover, the asymmetric morphology is conducive to promoting mass transfer, improving the efficiency of catalytic reactions, and thus enhancing the catalytic degradation performance; Fe3O4 is encapsulated by the mesoporous carbon material, greatly improving the aggregation problem that occurs during the catalytic process. Brief Description of the Drawings:

[0025] Figure 1 Scanning electron microscope image of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 1.

[0026] Figure 2 Element mapping image of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 1.

[0027] Figure 3 Transmission electron microscope image of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 1.

[0028] Figure 4 Transmission electron microscope image of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 2.

[0029] Figure 5 Transmission electron microscope image of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 3.

[0030] Figure 6 Schematic diagram of the degradation rate of Rhodamine B catalyzed by the asymmetric Fe3O4&SiO2@C superstructure materials prepared in Examples 1 - 3. Detailed Description of the Invention:

[0031] The present invention will be further described in detail below through examples.

[0032] Example 1:

[0033] (1) Add 3.25 g of ferric chloride hexahydrate, 0.9 g of trisodium citrate, and 5.5 g of sodium acetate trihydrate to 110 mL of ethylene glycol, sonicate for 2 hours, and stir vigorously for 2 hours to dissolve. Transfer the dissolved solution to a polytetrafluoroethylene inner liner, set the pressure to 10 - 15 MPa, and react at a temperature of 200 - 250 °C for 12 - 17 hours. After centrifugation, washing with water, washing with ethanol, and drying, Fe3O4 nanoparticles with a size of 100 - 150 nm are obtained.

[0034] (2) Disperse 50 mg of Fe3O4 nanoparticles and 0.1 g of CTAB into 20 mL of deionized water. Stir and mix for 5 - 20 min and then ultrasonically mix for 20 - 40 min in sequence. Then add 1 mL of ammonia water and 180 μL of TEOS. React at 40 - 60 °C in an oil bath with mechanical stirring at 300 - 500 rpm for 4 - 36 h. After that, centrifuge, wash with water, wash with ethanol, and finally dissolve in 20 mL of absolute ethanol for storage to obtain an Fe3O4&SiO2 alcohol dispersion with a concentration of 2 - 5 mg / mL;

[0035] (3) Add 80 mg of the block copolymer PS 69 -PVP 42 -PEO 113 to 40 mL of absolute ethanol solution. Place the block copolymer solution in an oven and keep it at 30 - 110 °C for 3 - 10 hours to form a uniform and monodisperse single micelle ethanol solution; Let the temperature of the block copolymer solution cool naturally to 25 °C to obtain a super-stable and monodisperse PS 69 -PVP 42 -PEO 113 single micelle solution with a concentration of 1 - 20 mg / mL.

[0036] (4) Dropwise add 1 mL of the PS 69 -PVP 42 -PEO 113 single micelle solution to 10 mL of the Fe3O4&SiO2 alcohol dispersion. Ultrasonically mix for 20 - 40 min, then add 1 mL of ammonia water to adjust the pH value to 8 - 12. Subsequently, react at room temperature with mechanical stirring at 300 - 500 rpm for 6 - 24 h. After that, centrifuge again, wash with water, wash with ethanol, and finally dissolve in 30 mL of absolute ethanol for storage to obtain an Fe3O4&SiO2@micelle single micelle superstructure alcohol solution with a concentration of 1 - 10 mg / mL.

[0037] (5) Take 10 mL of the Fe3O4&SiO2@micelle single micelle superstructure alcohol solution and ultrasonically mix it with 10 mL of deionized water. Then add 0.018 g of Tris buffer and 15 mL of deionized water to adjust the pH value of the solution to 8 - 10. Then add 7 mg of polydopamine and react at room temperature with mechanical stirring at 300 - 500 rpm until the solution turns black. Subsequently, centrifuge, wash with water, wash with ethanol, and dry.

[0038] (6) Heat-treat the material dried in step (5) at 330 - 450 °C for 3 - 9 h under a nitrogen atmosphere to remove PS 69 -PVP 42 -PEO 113Single micelle soft template; then, the temperature is further raised to 600 - 800 °C for carbonization and calcined at this temperature for 3 - 12 h to obtain an asymmetric Fe3O4&SiO2@C superstructure material.

[0039] Among them, the frequency of ultrasonic mixing is 10 - 50 kHz; centrifugation conditions: centrifugation speed is 8000 - 15000 r / min, and centrifugation time is 5 - 12 min; washing conditions: washed 3 - 6 times with deionized water and 3 - 6 times with 95% ethanol solution.

[0040] The morphology of the asymmetric Fe3O4&SiO2@C superstructure material obtained in Example 1 is as shown in Figure 1 、 2 、Figure 3. As can be seen from Figure 1 and 3 , there are closely and regularly arranged superstructure protrusions on the surface of the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 1, showing a rich and uniform-sized spherical mesoporous structure. The pore diameter of the spherical mesoporous unit is about 22 nm, the carbon layer thickness is about 7 nm, and the length is 330 nm. As can be seen from Figure 2 , the diameter of Fe3O4 is 110 nm, and it is wrapped by C on the outside. And the specific surface area of the asymmetric Fe3O4&SiO2@C superstructure material in Example 1 was measured by a fully automatic gas sorption analyzer, and its specific surface area was 116 m 2 / g.

[0041] Example 2: The overall method is the same as that in Example 1, except that in step (2), 32 mg of Fe3O4 nanoparticles and 0.08 g of CTAB are dispersed in 20 mL of deionized water; in step (3), 20 mg of the block copolymer PS 106 -PVP 47 -PEO 113 is added to 10 mL of anhydrous ethanol solution.

[0042] The morphology of the asymmetric Fe3O4&SiO2@C superstructure material obtained in Example 2 is as shown in Figure 4 . As can be seen from Figure 4 , there are closely and regularly arranged superstructure protrusions on the surface of the Fe3O4&SiO2@C superstructure material prepared in Example 2, showing a rich and uniform-sized spherical mesoporous structure. The pore diameter of the spherical mesoporous unit is about 40 nm, the carbon layer thickness is about 7 nm, and the length is 370 nm. And the specific surface area of the asymmetric Fe3O4&SiO2@C superstructure material in Example 2 was measured by a fully automatic gas sorption analyzer, and its specific surface area was 94 m 2 / g.

[0043] Example 3: The overall method is the same as that of Example 2, except that in step (3), the block copolymer is PS 216 -PVP 56 -PEO 113 .

[0044] The morphology of the asymmetric Fe3O4&SiO2@C superstructure material obtained in Example 3 is shown in the attached figure. Figure 5 As shown by Figure 5 It can be seen that the surface of the Fe3O4&SiO2@C superstructure material prepared in Example 3 has densely and regularly arranged superstructure protrusions, showing a rich and uniform spherical mesoporous structure, with a spherical mesoporous unit pore size of about 50nm, a carbon layer thickness of about 7nm, and a length of 400nm; and the specific surface area of ​​the asymmetric Fe3O4&SiO2@C superstructure material of Example 3 was measured by a fully automatic gas adsorption instrument, and the specific surface area was found to be 87m 2 / g.

[0045] The asymmetric Fe3O4&SiO2@C superstructure material prepared in Examples 1-3 was subjected to a Rhodamine B (RhB) degradation test. The experiment was carried out in a 100-250mL glass beaker, and 10-50mL of a 100-200mg / L RhB solution was selected, and the initial pH was adjusted to 3-6 by adding 0.1-1.0mol / L H2SO4 or NaOH solution. Subsequently, 2-10mg of asymmetric Fe3O4&SiO2@C superstructure material was added and stirred for 30-180min to achieve adsorption-desorption equilibrium. A quantitative amount of H2O2 was added to start the degradation reaction, and a constant temperature environment of 30°C was maintained for 30-150min. After the reaction was completed, 0.1-1.0mol / L NaOH was added dropwise to adjust the pH of the system to 9-12 to terminate the reaction. After standing, the supernatant was taken to determine the RhB degradation rate. The specific test results are shown in. Figure 6 , wherein the pore size of 22 nm is the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 1; the pore size of 40 nm is the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 2; and the pore size of 50 nm is the asymmetric Fe3O4&SiO2@C superstructure material prepared in Example 3.

[0046] Depend on Figure 6 It can be seen that the asymmetric Fe3O4&SiO2@C superstructure material with a pore size of 22 nm prepared in Example 1 has the best degradation rate of RhB compared with the asymmetric Fe3O4&SiO2@C superstructure materials prepared in Examples 2 and 3 under the same conditions, and has the most excellent degradation performance.

[0047] Catalytic degradation mechanism:

[0048] Adsorption enrichment: An asymmetric Fe3O4&SiO2@C superstructure material with a high specific surface area (87 - 116 m 2 / g) and a regular mesoporous structure (pore size 22.8 - 50 nm) is used to physically enrich RhB molecules through its mesoporous channels to increase the local concentration of reactants; meanwhile, polar functional groups such as pyridine nitrogen and pyrrole nitrogen on the material surface form hydrogen bonds or chemical adsorption with the benzene ring and amino groups in RhB molecules to achieve selective anchoring of target pollutants.

[0049] Oxidation degradation: Under the synergistic catalysis of Fe3O4 nanoparticles and nitrogen-doped carbon, H2O2 is activated through the following dual reaction pathways:

[0050] a) Fe 2+ Decompose H2O2 through the Fenton-like reaction to generate hydroxyl radicals (-OH)

[0051] Fe 2+ + H2O2 → Fe 3+ + OH - + -OH

[0052] b) Nitrogen-doped carbon promotes the generation of reactive oxygen species (-OH, -O2 - ) through an electron transfer mechanism

[0053] N-C + H2O2 → reactive oxygen species

[0054] The active oxygen radicals preferentially attack the conjugated chromophore groups of RhB molecules (including benzene ring and azo bond), and are gradually converted into carboxylic acid intermediate products through oxidative cleavage reactions, and finally mineralized into CO2 and H2O.

[0055] Magnetic separation step: The Fe3O4 core layer endows the material with superparamagnetism, enabling rapid solid-liquid separation and recycling of the catalyst under the action of an external magnetic field; meanwhile, the carbon shell coating structure effectively inhibits the oxidation inactivation of the Fe3O4 core and the aggregation of nanoparticles, so that the material still maintains excellent catalytic activity after multiple cycles.

[0056] The above is the preferred embodiment of the present invention. For those of ordinary skill in the art, without departing from the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing an asymmetric magnetic mesoporous carbon superstructure material, characterized in that: It includes the following steps: (1) Preparing Fe3O4 & SiO2 alcohol dispersion: Dispersing Fe3O4 nanoparticles and hexadecyltrimethylammonium bromide in a mass ratio of 3-7.5:10-15 into 20-40 mL of deionized water, stirring and mixing for 5-20 min and ultrasonic mixing for 20-40 min, then adding 0.5-2 mL of ammonia water and 100-250 μL of tetraethoxysilane, stirring and reacting in an oil bath at 40-60° C. for 4-36 h; then centrifuging, washing with water, and washing with ethanol to obtain a Fe3O4 & SiO2 alcohol dispersion with a concentration of 2-5 mg / mL; (2) Preparation of Fe3O4&SiO2@micelle single micelle superstructure alcohol solution: 10-20 mL of the Fe3O4&SiO2 alcohol dispersion in step (1) and 1-15 mL of a single micelle solution with a concentration of 1-20 mg / mL are ultrasonically mixed for 20-40 min, and then ammonia water is added to adjust the pH value to 8-12, followed by stirring at room temperature for 6-24 h; then centrifugation, water washing, and ethanol washing are performed to obtain a Fe3O4&SiO2@micelle single micelle superstructure alcohol solution with a concentration of 1-10 mg / mL; (3) Preparation of Fe3O4&SiO2@C superstructure material: 5-15 mL of the Fe3O4&SiO2@micelle single micelle superstructure alcohol solution in step (2) was mixed with 2-25 mg / mL bis(2-hydroxyethyl)aminotris(hydroxymethyl)methane buffer solution to make the solution pH 7-12, then 2-10 mg polydopamine was added and stirred at room temperature for 6-24 h; then the mixture was centrifuged, washed with water, washed with ethanol and dried, and the dried material was calcined in a nitrogen atmosphere to obtain an asymmetric Fe3O4&SiO2@C superstructure material.

2. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 1, characterized in that: The preparation method of the Fe3O4 nanoparticles in step (1) comprises the following steps: adding 3.0-4.5g of ferric chloride hexahydrate, 0.7-0.9g of trisodium citrate and 4.5-5.5g of sodium acetate hydrate to 110-220mL of ethylene glycol, and stirring to dissolve; transferring the dissolved solution to a polytetrafluoroethylene liner, setting high pressure and high temperature conditions, reacting for 12-17h, and then centrifuging, washing with water, washing with ethanol and drying to obtain Fe3O4 nanoparticles with a particle size of 100-150nm.

3. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 2, characterized in that: The high pressure condition is 10-15MPa, and the high temperature condition is 200-250℃.

4. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 1, characterized in that: The method for preparing the monomicelle solution in step (2) comprises the following steps: dissolving the block copolymer polystyrene-polytetravinylpyridine-polyethylene oxide in a solvent to obtain a block copolymer solution, then placing the block copolymer solution in an oven, keeping it warm at 30-110°C for 3-10 hours, and then naturally cooling it to room temperature to obtain a monomicelle solution.

5. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 4, characterized in that: Polystyrene-polytetravinylpyridine-polyethylene oxide is PEO 113 -PVP 60 -PS 28 、PEO 113 -PVP 68 -PS 60 、PEO 113 -PVP 44 -PS 97 and PEO 113 -PVP 98 -PS 142 The solvent is one of acetic acid, anhydrous ethanol, water, DMF and a mixture of water and DMF.

6. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 1, characterized in that: The calcination process in step (3) is divided into two stages, the first stage calcination temperature is 330-450°C, the calcination time is 3-9h, the second stage calcination temperature is 600-800°C, the calcination time is 3-12h. The nitrogen flow rate during the calcination stage is 200-300mL / min, and the pressure is maintained at normal pressure.

7. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 1, characterized in that: The stirring speed in step (1), step (2) and step (3) is 300-500 rpm; the frequency of ultrasonic mixing in step (1) and step (2) is 10-50 kHz.

8. The method for preparing an asymmetric magnetic mesoporous carbon superstructure material according to claim 2, characterized in that: The centrifugal conditions in step (1) to step (3) and the process of preparing Fe3O4 nanoparticles are as follows: the centrifugal speed is 8000-15000r / min, and the centrifugal time is 5-12min; Washing conditions: wash with deionized water 3-6 times, wash with 95% ethanol solution 3-6 times.

9. The asymmetric magnetic mesoporous carbon superstructure material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: Specific surface area is 87-116m 2 / g, pore diameter is 22.8-50nm, and length is 330-400nm.

10. The use of the asymmetric magnetic mesoporous carbon superstructure material according to claim 9 in catalytic degradation of organic dyes, characterized in that: The application is to catalyze the degradation of macromolecular organic dye Rhodamine B in wastewater.

Citation Information

Patent Citations

  • Preparation method and application of nano zero-valent iron mesoporous carbon asymmetric structure material for removing persistent organic pollutants in water

    CN107486154A

Cited By

  • Asymmetric hybrid mesoporous material as well as preparation method and application thereof

    CN122025615A