Multi-purpose water-based gloss oil with wide application range and preparation method of multi-purpose water-based gloss oil
By using materials such as hard acrylic film-forming resin, soft acrylic film-forming resin and polyurethane resin, combined with specific solvents and additives, a multi-purpose and wide range of water-based varnish is prepared, which solves the problems of low viscosity and large surface tension of existing water-based varnishes, achieving better printing performance and a wider range of application.
Patent Information
- Application Number
- CN202311838655.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2025-07-01
AI Technical Summary
Due to the low viscosity, existing water-based varnish can not be used as a material for flexographic printing, and the surface tension is large, and there are problems such as overprinting and hot stamping. The scope of application is low and cannot meet the diversified needs of manufacturers.
Hard acrylic film-forming resin, soft acrylic film-forming resin and polyurethane resin are used as raw materials, combined with a mixed solution of alcohol and deionized water as solvent, a small amount of ammonia water is added as auxiliary pH adjuster, and aids such as wax emulsion, wetting agent, defoaming agent and other auxiliary agents are used to prepare a multi-purpose, wide-range application and water-based varnish oil through specific stirring and emulsification processes.
It improves the leveling and stability of water-based varnish, enhances its adhesion, appropriately adjusts surface tension, improves scratch resistance, expands its use range, and meets diversified printing needs.
Smart Images

Figure BDA0004638247740000021 
Figure BDA0004638247740000041 
Figure BDA0004638247740000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of printing materials, and particularly to a water-based varnish with a wide range of multi-purpose applications and a preparation method thereof. Background Art
[0002] As a printing surface treatment material, varnish is widely used in the printing industry. By coating the varnish on the surface of an object to form a solid film layer with a certain strength and a smooth surface, it can well protect the printed graphics and texts. Therefore, varnish is widely printed on the outer surfaces of food and beverage, footwear and clothing, tobacco and alcohol packaging boxes.
[0003] Chinese Patent Application CN105368149A discloses a water-based varnish with a low alcohol addition amount suitable for high-speed gravure printing and its preparation. The water-based varnish includes the following components and weight contents: 60-75 parts of solvent and 25-40 parts of film-forming resin. Among them, the solvent is deionized water, alcohol or a mixture of deionized water and alcohol, and the film-forming resin is acrylic resin. This application scheme shows that it has good printing adaptability on the surfaces of various papers, is not prone to phenomena such as shrinkage holes, protects the integrity and beauty of printed products; has good overprinting with the ink below, has good wear resistance, a smooth surface, and non-sticking overprinting; the residual solvent odor of the printed product after drying is small and can be applied to food packaging.
[0004] Chinese Patent Application CN110028820A discloses a water-based varnish suitable for high-speed online inkjet coding and its preparation method. It is composed of the following components by weight: 70-90 parts of film-forming resin, 1-10 parts of solvent, 0.5-1 part of ammonia water, and 5-10 parts of additives. Among them, the film-forming resin is a water-based styrene-acrylic resin, the solvent is a mixed solvent of deionized water and ethanol, and the additives include wax emulsion, silicone oil, wetting agent and defoaming agent. A small amount of ammonia water is added when dissolving the resin, which improves the dissolution speed and makes the dissolution more complete, so that the varnish maintains good leveling and stability, effectively improves the cracking effect, and helps to improve its adhesion.
[0005] However, the existing water-based varnishes still have various defects and have their specific application ranges. The gravure water-based varnishes currently produced and used by major manufacturers generally cannot be used as flexographic printing materials due to their relatively low viscosity, and there are also certain problems in surface overprinting or hot stamping due to their relatively large surface tension. Their application range is relatively low and cannot meet the unified requirements of manufacturers. Summary of the Invention
[0006] The object of the present invention is to overcome the defects existing in the above-mentioned existing waterborne varnishes and provide a waterborne varnish with wide multi-purpose applicability and its preparation method.
[0007] The object of the present invention can be achieved by the following technical solutions:
[0008] The present invention provides a waterborne varnish with wide multi-purpose applicability, which is prepared by mixing the following components according to parts by weight:
[0009]
[0010] In an embodiment of the present invention, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include:
[0011] 15-35 parts of methyl methacrylate, 15-35 parts of ethyl methacrylate, 15-35 parts of tert-butyl methacrylate, 10-20 parts of methacrylic acid, 20-40 parts of caprolactone;
[0012] The initiator is benzoyl peroxide, and its dosage is 0.5-1.5% of the total amount of monomers;
[0013] The chain extender is 1,4-butanediol, and its dosage is 0.5-1.5% of the total amount of monomers;
[0014] The preparation method of the rigid acrylic film-forming resin is as follows: at a polymerization reaction temperature of 90-95 °C, various monomers, the initiator, and the chain extender are mixed and stirred evenly, and nitrogen protection is adopted. After reacting for 8-24 hours, it is cooled and poured into water to precipitate, and then vacuum dried to obtain the rigid acrylic film-forming resin.
[0015] In an embodiment of the present invention, the soft acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 20-35 parts of acrylic resin, 20-35 parts of styrene-propylene, 10-25 parts of ethyl acrylate, 5-25 parts of water.
[0016] In one embodiment of the present invention, the polyurethane tree is a water-based blocked polyurethane emulsion, and the preparation method of the water-based blocked polyurethane emulsion is as follows: add toluene-2,4-diisocyanate to tetrahydrofuran according to a ratio, mix well, and obtain a toluene-2,4-diisocyanate solution; add polyethylene glycol-400 to the tetrahydrofuran solution, mix well, and obtain a polyethylene glycol solution; mix the toluene-2,4-diisocyanate solution with the polyethylene glycol solution, and react the reaction system at 50-70°C under nitrogen protection for 50-200 minutes, add 2,4,6-tris(dimethylaminomethyl)phenol to the reaction system, and when the -NCO content is less than 0.05wt%, terminate the reaction, cool the reaction system to room temperature, and then add distilled water or deionized water under high-speed shear stirring conditions for emulsification; after the emulsification is completed, remove the solvent in vacuum to obtain the water-based blocked polyurethane emulsion. Among them, the amount of each component can be flexibly adjusted.
[0017] In one embodiment of the present invention, the aqueous solvent is a mixed solution of alcohol and deionized water, preferably, the volume ratio of alcohol to deionized water is 1:1.
[0018] In one embodiment of the present invention, the pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0019] In one embodiment of the present invention, the auxiliary agent is composed of the following components in parts by weight: 0.5-2 parts of wetting agent, 0.5-1.5 parts of defoaming agent, 0.5-2 parts of leveling agent, 0.5-2 parts of surfactant, and 0.5-1.5 parts of anti-scratch agent.
[0020] In one embodiment of the present invention, the wetting agent is isopropyl alcohol.
[0021] In one embodiment of the present invention, the anti-scratch agent is a wax emulsion.
[0022] In one embodiment of the present invention, the defoaming agent is polydimethylsiloxane.
[0023] In one embodiment of the present invention, the surfactant is disodium dodecylbenzene sulfonate.
[0024] In one embodiment of the present invention, the leveling agent is dioctyl sodium sulfosuccinate.
[0025] The present invention further provides a method for preparing the multi-purpose water-based varnish with a wide application range, comprising the following steps:
[0026] (1) Pre-dispersion of ingredients:
[0027] Mix the rigid acrylic film-forming resin and polyurethane resin, stir evenly at high speed, and grind to a fineness of <10μm to obtain the first semi-finished varnish; mix the flexible acrylic film-forming resin with the aqueous solvent, stir evenly at high speed, and after mixing evenly, obtain the second semi-finished varnish.
[0028] (2) Varnish adjustment: After mixing and dispersing the first semi-finished varnish and the second semi-finished varnish, add additives, and then add a pH regulator to adjust the pH value to 8-9, stir and disperse to obtain the water-based varnish with a wide range of multi-purpose applications.
[0029] In an embodiment of the present invention, in step (1), the rotation speed of high-speed stirring when preparing the first semi-finished varnish is 500-800 rpm, and the rotation speed of mixing and stirring when preparing the second semi-finished varnish is 300-500 rpm, and the time is 20-30 min.
[0030] In an embodiment of the present invention, in step (2), the conditions of the stirring and dispersing process are: the rotation speed is 300-500 revolutions per minute, the temperature is 20-30°C, and the stirring time is 30 minutes.
[0031] Compared with the prior art, the advantages of the present invention are reflected in the following aspects:
[0032] The present invention selects rigid acrylic film-forming resin, flexible acrylic film-forming resin and polyurethane resin as raw materials, a mixed solution of alcohol and deionized water as a solvent, a small amount of ammonia water as an auxiliary pH regulator, wax emulsion, wetting agent, and defoaming agent as additives. A small amount of ammonia water is added during the dissolution of the resin, which improves the dissolution speed and makes the dissolution more complete, so that the varnish maintains good leveling and stability, and helps to improve its adhesion.
[0033] All the raw materials of the present invention are water-based materials, and no toxic solvents are used, reducing the physical harm to production workers and users. And the printing performance is stable, the printed graphics and texts are clear, the colors are full, the adhesion is strong, and the printing effect is good.
[0034] Through the mutual synergistic effect of the three emulsions and the cooperation of other components, the water-based varnish can have a more appropriate surface tension and good scratch resistance, and its printing leveling, adhesion, fastness, hardness and other properties can all reach a good level. The appropriate surface tension also enables most inks to be printed on the normal water-based varnish, greatly expanding the use range of the varnish.
[0035] The present invention clearly defines the preparation process. First, the resins are mixed and stirred evenly, and then various additives are added, aiming to prevent the additives from combining too tightly with a single resin, resulting in uneven mixing and greatly affecting the varnish performance.
[0036] The present invention defines the stirring speed. When the stirring speed is too high, the resin structure inside the varnish will be damaged, affecting the quality of the varnish. The stirring speed defined in this application can optimize the performance of the obtained water-based varnish with a wide range of multi-purpose applications. Detailed Embodiments
[0037] The present invention will be described in detail below with reference to specific embodiments.
[0038] Example 1:
[0039] This example provides a water-based varnish with a wide range of multi-purpose applications, which is prepared from the following components according to the weight percentage:
[0040]
[0041] In this example, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include: 15 parts of methyl methacrylate, 15 parts of ethyl methacrylate, 15 parts of tert-butyl methacrylate, 10 parts of methacrylic acid, and 20 parts of caprolactone; the initiator is benzoyl peroxide, and its dosage is 0.5% of the total amount of monomers; the chain extender is 1,4-butanediol, and its dosage is 0.5% of the total amount of monomers; the preparation method of the rigid acrylic film-forming resin is: at a polymerization reaction temperature of 90 °C, after mixing various monomers, the initiator, and the chain extender evenly and under nitrogen protection, after reacting for 24 hours, it is cooled and poured into water to precipitate, and then vacuum dried to obtain the rigid acrylic film-forming resin.
[0042] In this example, the flexible acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 20 parts of acrylic resin, 20 parts of styrene-propylene, 10 parts of ethyl acrylate, and 5 parts of water.
[0043] In this embodiment, the polyurethane resin is an aqueous blocked polyurethane emulsion, and the preparation method of the aqueous blocked polyurethane emulsion is as follows: toluene-2,4-diisocyanate is added to tetrahydrofuran, and mixed to obtain a toluene-2,4-diisocyanate solution; polyethylene glycol-400 is added to the tetrahydrofuran solution, and mixed to obtain a polyethylene glycol solution; the toluene-2,4-diisocyanate solution and the polyethylene glycol solution are mixed (the molar ratio of toluene-2,4-diisocyanate to polyethylene glycol is 4:1), and the reaction system is reacted at 50° C. under nitrogen protection for 200 minutes, and the reaction system is added to the Add 2,4,6-tris(dimethylaminomethyl)phenol, wherein the 2,4,6-tris(dimethylaminomethyl)phenol is added in the form of a tetrahydrofuran solution of 2,4,6-tris(dimethylaminomethyl)phenol, wherein: the concentration of the THF solution of 2,4,6-tris(dimethylaminomethyl)phenol is 10wt%; when the -NCO content is less than 0.05wt%, terminate the reaction, cool the reaction system to room temperature, and then add distilled water or deionized water for emulsification under high-speed shear stirring conditions; after the emulsification is completed, remove the solvent in vacuum to obtain the water-based blocked polyurethane emulsion. The amount of each component can be flexibly adjusted.
[0044] In this embodiment, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0045] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0046] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0047] (1) Pre-dispersion of ingredients:
[0048] A hard acrylic film-forming resin and a polyurethane resin are mixed, stirred at high speed and uniformly, and ground to a fineness of <10 μm to obtain a varnish semi-finished product 1; a soft acrylic film-forming resin and an aqueous solvent are mixed, stirred at high speed and uniformly, and after mixing uniformly, a varnish semi-finished product 2 is obtained;
[0049] (2) Varnish adjustment: After the varnish semi-finished product 1 and the varnish semi-finished product 2 are mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0050] Among them, in step (1), the rotation speed of high-speed stirring is 500 - 800 rpm. After adding the aqueous styrene-acrylic soft resin emulsion, the rotation speed of mixing and stirring is 300 - 500 rpm, and the time is 20 - 30 min. In step (2), the conditions of the stirring and dispersion process are: the rotation speed is 300 - 500 revolutions per minute, the temperature is 20 - 30 °C, and the stirring time is 30 minutes.
[0051] Example 2:
[0052] A water-based varnish with a wide range of multi-purpose applications is prepared from the following components according to the weight percentage:
[0053]
[0054] In this example, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include:
[0055] 35 parts of methyl methacrylate, 35 parts of ethyl methacrylate, 35 parts of tert-butyl methacrylate, 20 parts of methacrylic acid, 40 parts of caprolactone; the initiator benzoyl peroxide, and its dosage is 1.5% of the total amount of monomers; the chain extender 1,4-butanediol, and its dosage is 1.5% of the total amount of monomers; the preparation method of the rigid acrylic film-forming resin is: at a polymerization reaction temperature of 95 °C, after mixing various monomers, the initiator and the chain extender evenly and protecting with nitrogen, after reacting for 8 hours, cooling and pouring into water for precipitation, and then vacuum drying to obtain the rigid acrylic film-forming resin.
[0056] In this example, the soft acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 35 parts of acrylic resin, 35 parts of styrene-propylene, 25 parts of ethyl acrylate, and 25 parts of water.
[0057] In this embodiment, the polyurethane resin is an aqueous blocked polyurethane emulsion, and the preparation method of the aqueous blocked polyurethane emulsion is as follows: toluene-2,4-diisocyanate is added to tetrahydrofuran, and mixed to obtain a toluene-2,4-diisocyanate solution; polyethylene glycol-400 is added to the tetrahydrofuran solution, and mixed to obtain a polyethylene glycol solution; the toluene-2,4-diisocyanate solution and the polyethylene glycol solution are mixed (the molar ratio of toluene-2,4-diisocyanate to polyethylene glycol is 4:1), and the reaction system is reacted at 70° C. under nitrogen protection for 50 minutes, and the reaction system is added 2,4,6-tris(dimethylaminomethyl)phenol is added, wherein the 2,4,6-tris(dimethylaminomethyl)phenol is added in the form of a tetrahydrofuran solution of 2,4,6-tris(dimethylaminomethyl)phenol, wherein: the concentration of the THF solution of 2,4,6-tris(dimethylaminomethyl)phenol is 10wt%; when the -NCO content is less than 0.05wt%, the reaction is terminated, the reaction system is cooled to room temperature, and then distilled water or deionized water is added under high-speed shear stirring conditions for emulsification; after the emulsification is completed, the solvent is evaporated in vacuum to obtain the water-based blocked polyurethane emulsion. The amount of each component can be flexibly adjusted.
[0058] In this embodiment, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0059] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0060] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0061] (1) Pre-dispersion of ingredients:
[0062] A hard acrylic film-forming resin and a polyurethane resin are mixed, stirred at high speed and uniformly, and ground to a fineness of <10 μm to obtain a varnish semi-finished product 1; a soft acrylic film-forming resin and an aqueous solvent are mixed, stirred at high speed and uniformly, and after mixing uniformly, a varnish semi-finished product 2 is obtained;
[0063] (2) Varnish adjustment: After the varnish semi-finished product 1 and the varnish semi-finished product 2 are mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0064] In an embodiment of the present invention, in step (1), the rotation speed of high-speed stirring when preparing the first varnish semi-finished product is 500 - 800 rpm, and the rotation speed of mixing and stirring when preparing the second varnish semi-finished product is 300 - 500 rpm, and the time is 20 - 30 min. In step (2), the conditions of the stirring and dispersion process are: the rotation speed is 300 - 500 revolutions per minute, the temperature is 20 - 30 °C, and the stirring time is 30 minutes.
[0065] Example 3:
[0066] A multi-purpose waterborne varnish with a wide range of applications is prepared from the following components according to the weight percentage:
[0067]
[0068]
[0069] In this embodiment, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include: 20 parts of methyl methacrylate, 25 parts of ethyl methacrylate, 25 parts of tert-butyl methacrylate, 15 parts of methacrylic acid, and 30 parts of caprolactone; the initiator is benzoyl peroxide, and its dosage is 1% of the total amount of monomers; the chain extender is 1,4-butanediol, and its dosage is 1% of the total amount of monomers; the preparation method of the rigid acrylic film-forming resin is: at a polymerization reaction temperature of 90 - 95 °C, after mixing various monomers, the initiator, and the chain extender evenly and using nitrogen protection, after reacting for 16 hours, it is cooled and poured into water to precipitate, and after vacuum drying, the rigid acrylic film-forming resin can be obtained.
[0070] In this embodiment, the soft acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 30 parts of acrylic resin, 30 parts of styrene-propylene, 20 parts of ethyl acrylate, and 10 parts of water.
[0071] In this embodiment, the polyurethane resin is an aqueous blocked polyurethane emulsion, and the preparation method of the aqueous blocked polyurethane emulsion is as follows: toluene-2,4-diisocyanate is added to tetrahydrofuran, and mixed to obtain a toluene-2,4-diisocyanate solution; polyethylene glycol-400 is added to the tetrahydrofuran solution, and mixed to obtain a polyethylene glycol solution; the toluene-2,4-diisocyanate solution and the polyethylene glycol solution are mixed (the molar ratio of toluene-2,4-diisocyanate to polyethylene glycol is 4:1), and the reaction system is reacted at 60° C. under nitrogen protection for 100 minutes, and the reaction system is added with 1% tantalum. Add 2,4,6-tris(dimethylaminomethyl)phenol, wherein the 2,4,6-tris(dimethylaminomethyl)phenol is added in the form of a tetrahydrofuran solution of 2,4,6-tris(dimethylaminomethyl)phenol, wherein: the concentration of the THF solution of 2,4,6-tris(dimethylaminomethyl)phenol is 10wt%; when the -NCO content is less than 0.05wt%, terminate the reaction, cool the reaction system to room temperature, and then add distilled water or deionized water for emulsification under high-speed shear stirring conditions; after the emulsification is completed, remove the solvent in vacuum to obtain the water-based blocked polyurethane emulsion. The amount of each component can be flexibly adjusted.
[0072] In this embodiment, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0073] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0074] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0075] (1) Pre-dispersion of ingredients:
[0076] A hard acrylic film-forming resin and a polyurethane resin are mixed, stirred at high speed and uniformly, and ground to a fineness of <10 μm to obtain a varnish semi-finished product 1; a soft acrylic film-forming resin and an aqueous solvent are mixed, stirred at high speed and uniformly, and after mixing uniformly, a varnish semi-finished product 2 is obtained;
[0077] (2) Varnish adjustment: After the varnish semi-finished product 1 and the varnish semi-finished product 2 are mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0078] In one embodiment of the present invention, in step (1), the rotation speed for high-speed stirring when preparing the first varnish semi-finished product is 500 - 800 rpm, and the rotation speed for mixing and stirring when preparing the second varnish semi-finished product is 300 - 500 rpm, and the time is 20 - 30 min. In step (2), the conditions for the stirring and dispersion process are: rotation speed 300 - 500 revolutions per minute, temperature 20 - 30 °C, and stirring time 30 minutes.
[0079] Comparative Example 1
[0080] This comparative example provides an aqueous varnish, which is prepared from the following components according to the weight percentage:
[0081]
[0082] In this comparative example, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include: 15 parts of methyl methacrylate, 15 parts of ethyl methacrylate, 15 parts of tert-butyl methacrylate, 10 parts of methacrylic acid, and 20 parts of caprolactone; the initiator is benzoyl peroxide, and its dosage is 0.5% of the total amount of monomers; the chain extender is 1,4-butanediol, and its dosage is 0.5% of the total amount of monomers; the preparation method of the rigid acrylic film-forming resin is: at a polymerization reaction temperature of 90 °C, after mixing various monomers, the initiator, and the chain extender evenly and under nitrogen protection, after reacting for 24 hours, cooling and pouring into water for precipitation, and then vacuum drying to obtain the rigid acrylic film-forming resin.
[0083] In this comparative example, the polyurethane resin is an aqueous blocked polyurethane emulsion. The preparation method of the aqueous blocked polyurethane emulsion is: adding toluene-2,4-diisocyanate into tetrahydrofuran, mixing evenly to obtain a toluene-2,4-diisocyanate solution; adding polyethylene glycol-400 into the tetrahydrofuran solution, mixing evenly to obtain a polyethylene glycol solution; mixing the toluene-2,4-diisocyanate solution and the polyethylene glycol solution (the molar ratio of toluene-2,4-diisocyanate to polyethylene glycol is 4:1), reacting the reaction system at 50 °C under nitrogen protection for 200 min, adding 2,4,6-tris(dimethylaminomethyl)phenol to the reaction system, and the 2,4,6-tris(dimethylaminomethyl)phenol is added in the form of a tetrahydrofuran solution of 2,4,6-tris(dimethylaminomethyl)phenol, where: the concentration of the THF solution of 2,4,6-tris(dimethylaminomethyl)phenol is 10 wt%; when the -NCO content is less than 0.05 wt%, the reaction is terminated, the reaction system is cooled to room temperature, and then distilled water or deionized water is added for emulsification under high-speed shear stirring conditions; after the emulsification is completed, the solvent is removed by vacuum evaporation to obtain the aqueous blocked polyurethane emulsion. Among them, the dosage of each component can be adjusted flexibly.
[0084] In this comparative example, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0085] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0086] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0087] (1) Pre-dispersion of ingredients:
[0088] Mix the hard acrylic film-forming resin and the polyurethane resin, stir evenly at high speed, and grind to a fineness of <10 μm to obtain a varnish semi-finished product;
[0089] (2) Varnish adjustment: After the varnish semi-finished product is mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0090] In one embodiment of the present invention, in step (1), the high-speed stirring speed is 500-800 rpm and the time is 20-30 min when the semi-finished varnish is obtained. In step (2), the conditions of the stirring and dispersing process are: speed 300-500 rpm, temperature 20-30° C., and stirring time 30 minutes.
[0091] Comparative Example 2
[0092] This comparative example provides a water-based varnish, which is prepared by the following components according to weight percentage:
[0093]
[0094] In this comparative example, the soft acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 20 parts of acrylic resin, 20 parts of styrene-acrylic resin, 10 parts of ethyl acrylate, and 5 parts of water.
[0095] In this comparative example, the polyurethane resin is an aqueous blocked polyurethane emulsion, and the preparation method of the aqueous blocked polyurethane emulsion is as follows: toluene-2,4-diisocyanate is added to tetrahydrofuran, and mixed to obtain a toluene-2,4-diisocyanate solution; polyethylene glycol-400 is added to the tetrahydrofuran solution, and mixed to obtain a polyethylene glycol solution; the toluene-2,4-diisocyanate solution and the polyethylene glycol solution are mixed (the molar ratio of toluene-2,4-diisocyanate to polyethylene glycol is 4:1), and the reaction system is reacted at 50° C. under nitrogen protection for 200 minutes, and the reaction system is added with 1% tantalum. Add 2,4,6-tris(dimethylaminomethyl)phenol, wherein the 2,4,6-tris(dimethylaminomethyl)phenol is added in the form of a tetrahydrofuran solution of 2,4,6-tris(dimethylaminomethyl)phenol, wherein: the concentration of the THF solution of 2,4,6-tris(dimethylaminomethyl)phenol is 10wt%; when the -NCO content is less than 0.05wt%, terminate the reaction, cool the reaction system to room temperature, and then add distilled water or deionized water for emulsification under high-speed shear stirring conditions; after the emulsification is completed, remove the solvent in vacuum to obtain the water-based blocked polyurethane emulsion. The amount of each component can be flexibly adjusted.
[0096] In this comparative example, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0097] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0098] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0099] (1) Pre-dispersion of ingredients:
[0100] Mix the soft acrylic film-forming resin with the aqueous solvent, stir at high speed to make it uniform, and then mix it with the polyurethane resin to make a varnish semi-finished product;
[0101] (2) Varnish adjustment: After the varnish semi-finished product is mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0102] In one embodiment of the present invention, in step (1), when preparing the semi-finished varnish, the rotation speed of high-speed stirring is 500 - 800 rpm. In step (2), the conditions of the stirring and dispersion process are: rotation speed 300 - 500 revolutions per minute, temperature 20 - 30 °C, and stirring time 30 minutes.
[0103] Comparative Example 3
[0104] This comparative example provides an aqueous varnish, which is prepared from the following components according to the weight percentage:
[0105]
[0106]
[0107] In this comparative example, the rigid acrylic film-forming resin is an acrylic resin composition, which is polymerized from the following monomers under the action of an initiator and a chain extender. Among them, the monomers include: 15 parts of methyl methacrylate, 15 parts of ethyl methacrylate, 15 parts of tert-butyl methacrylate, 10 parts of methacrylic acid, and 20 parts of caprolactone; the initiator is benzoyl peroxide, and its dosage is 0.5% of the total amount of monomers; the chain extender is 1,4-butanediol, and its dosage is 0.5% of the total amount of monomers; the preparation method of the rigid acrylic film-forming resin is: at a polymerization reaction temperature of 90 °C, after mixing various monomers, the initiator, and the chain extender evenly and using nitrogen protection, after reacting for 24 hours, cooling and pouring into water for precipitation, and then vacuum drying to obtain the rigid acrylic film-forming resin.
[0108] In this comparative example, the soft acrylic film-forming resin is an aqueous styrene-acrylic soft resin emulsion, and the aqueous styrene-acrylic soft resin emulsion is composed of the following components in parts by weight: 20 parts of acrylic resin, 20 parts of styrene-propylene, 10 parts of ethyl acrylate, and 5 parts of water.
[0109] In this comparative example, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1:1. The pH regulator is dilute ammonia water with a concentration of 5 g / 100 ml.
[0110] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sulfosuccinate leveling agent, 1.2 parts of sodium dodecylbenzenesulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0111] The preparation method of the multi-purpose and wide-application aqueous varnish includes the following steps:
[0112] (1) Ingredient pre-dispersion:
[0113] Take a hard acrylic film-forming resin, stir it evenly at high speed, grind it to a fineness of less than 10 μm, and prepare a varnish semi-finished product 1; take a soft acrylic film-forming resin and mix it with an aqueous solvent, stir it evenly at high speed, and after mixing evenly, prepare a varnish semi-finished product 2;
[0114] (2) Varnish adjustment: After the varnish semi-finished product 1 and the varnish semi-finished product 2 are mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0115] In one embodiment of the present invention, in step (1), the speed of high-speed stirring when preparing the semi-finished varnish product 1 is 500-800 rpm, and the speed of mixing and stirring when preparing the semi-finished varnish product 2 is 300-500 rpm, and the time is 20-30 minutes. In step (2), the conditions of the stirring and dispersing process are: speed 300-500 rpm, temperature 20-30° C., and stirring time 30 minutes.
[0116] Comparative Example 4
[0117] This comparative example provides a multi-purpose varnish with a wide range of applications, which is prepared by the following components in percentage by weight:
[0118]
[0119] In this embodiment, the aqueous solvent is a mixed solution of alcohol and deionized water, and the volume ratio of alcohol to deionized water is 1: 1. The pH adjuster is dilute ammonia water with a concentration of 5 g / 100 ml.
[0120] The auxiliary agent is composed of the following components in parts by weight: 1 part of isopropyl alcohol wetting agent, 0.8 part of polydimethylsiloxane defoaming agent, 0.5 part of dioctyl sodium sulfosuccinate leveling agent, 1.2 parts of disodium dodecylbenzene sulfonate surfactant, 1 part of wax emulsion anti-scratch agent, and 0.5 part of pH regulator.
[0121] The preparation method of the multi-purpose water-based varnish with a wide application range comprises the following steps:
[0122] (1) Pre-dispersion of ingredients:
[0123] Acrylic resin and polyurethane resin are mixed, stirred at high speed, and then mixed with aqueous solvent, stirred at high speed, and after mixing evenly, a varnish semi-finished product is obtained;
[0124] (2) Varnish adjustment: After the varnish semi-finished product is mixed and dispersed, an auxiliary agent is added, and then a pH adjuster is added to adjust the pH value to 8-9, and the mixture is stirred and dispersed to obtain the multi-purpose water-based varnish with a wide range of applications.
[0125] Wherein, in step (1), the speed of high-speed stirring is 500-800 rpm, and the time is 20-30 min. In step (2), the conditions of the stirring and dispersing process are: speed 300-500 rpm, temperature 20-30° C., and stirring time 30 minutes.
[0126] The performance tests of the water-based varnish obtained in the above examples and comparative examples are as follows:
[0127] 1) Abrasion resistance: The printed matter coated with water-based varnish is rubbed back and forth with a load of 4 pounds, and the number of frictions is accumulated (one round trip is one time). When the printed matter begins to fade, the quality of the water-based varnish is judged by the current accumulated number of frictions (i.e. the number of abrasions). The more abrasions, the better the quality.
[0128] 2) Hot stamping effect: Use the multi-purpose water-based varnish with a wide range of applications for hot stamping, and observe whether the hot stamping pattern is clear, whether there is any breakage, and whether the color fades.
[0129] 3) Anti-adhesion test of the coating after coating: Cut the sample into a certain size, place it in an environment with a relative humidity of 85% and a temperature of 60°C, and apply 1kg / cm 2 Press face to face for 24 hours to observe whether the coating is sticky.
[0130] 4) Leveling: about its appearance leveling.
[0131]
[0132]
[0133] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A water-based varnish with a wide range of multi-purpose applications, characterized in that, It is prepared by the following components in parts by weight:
2. The waterborne varnish with wide multi-purpose application scope according to claim 1, characterized in that, The hard acrylic film-forming resin is an acrylic resin composition, which is formed by polymerization reaction of the following monomers under the action of an initiator and a chain extender, wherein the monomers include: 15-35 parts of methyl methacrylate, 15-35 parts of ethyl methacrylate, 15-35 parts of tert-butyl methacrylate, 10-20 parts of methacrylic acid, and 20-40 parts of caprolactone; The initiator is benzoyl peroxide, the amount of which is 0.5-1.5% of the total amount of monomers; Chain extender 1,4-butanediol, the amount of which is 0.5-1.5% of the total amount of monomers; The preparation method of the hard acrylic film-forming resin is as follows: at a polymerization reaction temperature of 90 to 95° C., various monomers, initiators and chain extenders are mixed and stirred evenly, and nitrogen protection is adopted; after reacting for 8 to 24 hours, the mixture is cooled and poured into water for precipitation; and the hard acrylic film-forming resin is obtained after vacuum drying.
3. A waterborne varnish with a wide range of multi-purpose applications according to claim 1, characterized in that, The soft acrylic film-forming resin is a water-based styrene-acrylic soft resin emulsion, which is composed of the following components in parts by weight: 20-35 parts of acrylic resin, 20-35 parts of styrene-acrylic resin, 10-25 parts of ethyl acrylate, and 5-25 parts of water.
4. A water-based varnish with a wide range of multi-purpose applications, as described in claim 1, characterized in that The polyurethane resin is a water-based blocked polyurethane emulsion. The preparation method of the water-based blocked polyurethane emulsion is as follows: toluene-2,4-diisocyanate is added to tetrahydrofuran according to a ratio, and mixed to obtain a toluene-2,4-diisocyanate solution; polyethylene glycol-400 is added to the tetrahydrofuran solution, and mixed to obtain a polyethylene glycol solution; the toluene-2,4-diisocyanate solution and the polyethylene glycol solution are mixed, and the reaction system is reacted at 50-70° C. under nitrogen protection for 50-200 minutes, 2,4,6-tris(dimethylaminomethyl)phenol is added to the reaction system, and when the -NCO content is less than 0.05wt%, the reaction is terminated, the reaction system is cooled to room temperature, and distilled water or deionized water is added under high-speed shear stirring conditions for emulsification; after the emulsification is completed, the solvent is evaporated in vacuum to obtain the water-based blocked polyurethane emulsion.
5. A water-based varnish with a wide range of multi-purpose applications according to claim 1, characterized in that, The aqueous solvent is a mixed solution of alcohol and deionized water.
6. The waterborne varnish with a wide range of multi - purpose applications according to claim 1, characterized in that, The pH regulator is dilute ammonia water with a concentration of 5g / 100ml.
7. A waterborne varnish with a wide range of multi-purpose applications according to claim 1, characterized in that, The auxiliary agent is composed of the following components in parts by weight: 0.5-2 parts of a wetting agent, 0.5-1.5 parts of a defoaming agent, 0.5-2 parts of a leveling agent, 0.5-2 parts of a surfactant, and 0.5-1.5 parts of an anti-scratch agent.
8. A water-based varnish with a wide range of multi-purpose applications according to claim 7, characterized in that, The wetting agent is isopropyl alcohol; The anti-scratch agent is a wax emulsion; The defoaming agent is polydimethylsiloxane; The surfactant is disodium dodecylbenzene sulfonate; The leveling agent is dioctyl sodium sulfosuccinate.
9. The preparation method of the water-based varnish with wide multi-purpose application scope according to any one of claims 1-8, characterized in that, The following steps are involved: (1) Pre-dispersion of ingredients: A hard acrylic film-forming resin and a polyurethane resin are mixed, stirred at high speed and uniformly, and ground to a fineness of <10 μm to obtain a varnish semi-finished product 1; a soft acrylic film-forming resin and an aqueous solvent are mixed, stirred at high speed and uniformly, and after mixing uniformly, a varnish semi-finished product 2 is obtained; (2) Varnish adjustment: After mixing and dispersing varnish semi-finished product one and varnish semi-finished product two, additives are added, and then a pH regulator is added to adjust the pH value to 8-9, followed by stirring and dispersing to obtain the water-based varnish with wide multi-purpose applicability.
10. The preparation method of the water-based varnish with wide multi-purpose application scope according to claim 9, characterized in that, In step (1), when preparing varnish semi-finished product one, the rotation speed of high-speed stirring is 500-800 rpm, and when preparing varnish semi-finished product two, the rotation speed of mixing and stirring is 300-500 rpm, and the time is 20-30 min; In step (2), the conditions for the stirring and dispersing process are: the rotation speed is 300-500 revolutions per minute, the temperature is 20-30 °C, and the stirring time is 30 minutes.
Citation Information
Patent Citations
Low alcohol additive amount water-based polishing oil suitable for high speed gravure printing, and preparation thereof
CN105368149A
Aqueous varnish suitable for high-speed online ink jetting, and preparation method thereof
CN110028820A