Weather-resistant master batch as well as preparation method and application thereof

Through the coordinated use of loaded ultraviolet absorbers and modified talc powder, the problem of insufficient anti-ultraviolet aging performance of degradable plastic films is solved, and the stability and cost-effectiveness of the material are improved.

CN120289963APending Publication Date: 2025-07-11SHANDONG DAWN DEGRADABLE MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510526432.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-25
Publication Date
2025-07-11

AI Technical Summary

Technical Problem

The existing degradable plastic film has insufficient anti-ultraviolet aging performance, the ultraviolet absorber is easy to migrate and decompose, and the talc powder is poorly compatible with the resin, resulting in the rapid aging of the plastic film under ultraviolet irradiation.

Method used

The loaded ultraviolet absorber and modified talc powder are used to combine specific preparation methods to uniformly disperse and chemical bonds of the loaded ultraviolet absorber to improve the compatibility of talc powder with polyadipic acid/butylene terephthalate, and form a synergistic improvement in the material's anti-ultraviolet aging performance.

Benefits of technology

It significantly improves the anti-UV aging performance of the degradable plastic film, reduces the decomposition and migration of UV absorbers, enhances the stability and color retention of the material, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of processing of full-biodegradable high polymer materials, in particular to a weather-resistant master batch and a preparation method and application thereof, and the weather-resistant master batch comprises the following components: 40-70 parts by weight of poly (butylene adipate-co-terephthalate); 10 to 20 parts of polylactic acid; 20-40 parts by weight of a supported ultraviolet absorbent; 15-25 parts by weight of modified talcum powder; 1-3 parts by weight of a light stabilizer; 1-3 parts by weight of a lubricant; 1-3 parts by weight of an antioxidant; the invention discloses a degradable mulching film and a preparation method thereof.The degradable mulching film is prepared from, by weight, 1-3 parts of a supported ultraviolet absorbent, 1-3 parts of modified talcum powder and 1-3 parts of a chain extender, the degradable mulching film comprises weather-proof master batches and poly (adipic acid) / butylene terephthalate, and the mass ratio of the weather-proof master batches to the poly (adipic acid) / butylene terephthalate is (5-15): (85-95). The ultraviolet aging resistance of the degradable mulching film is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the processing field of fully biodegradable polymer materials, and particularly to a weather-resistant masterbatch, a preparation method thereof, and an application thereof. Background Art

[0002] With the rapid development of the polymer industry and the increasing use of plastic mulch films by people, the problem of environmental pollution is presented to mankind. Most of the discarded plastic mulch films are synthetic polymer materials, which have good corrosion resistance, but are difficult to degrade in the natural environment, thus causing serious environmental pollution. Therefore, since the 1970s, the research on degradable mulch films has become an important topic worldwide. Currently, the degradable mulch films on the market usually use poly(butylene adipate-co-terephthalate) (PBAT) as the main raw material, and can be completely degraded into carbon dioxide and water after use, posing zero harm to the soil and crops. Therefore, using degradable mulch films to replace traditional polyethylene mulch films helps to improve the soil ecology and protect the farmland environment, thus effectively promoting the green development of agriculture.

[0003] However, poly(butylene adipate-co-terephthalate) belongs to aliphatic-aromatic copolyesters. Its molecular chain contains both ester bonds and benzene ring structures. Such a special chemical structure makes it very easy to undergo a photo-degradation reaction, resulting in a reduced service life and limiting its use in the market. Currently, adding light stabilizers and ultraviolet absorbers to the mulch film is a relatively common solution, but there are still problems such as their easy migration, easy decomposition, poor compatibility with resins, and certain effects on the color of the products.

[0004] Patent CN118895036A discloses a weather-resistant fully biodegradable mulch film and a preparation method thereof. The weather-resistant fully biodegradable mulch film comprises the following raw materials in parts by weight: 60-90 parts of fully biodegradable polyester, 10-30 parts of reinforcing filler, 0.1-1 part of dispersant, 0.5-2 parts of heat stabilizer, 0.2-0.5 part of chain extender, 0.1-1 part of ultraviolet absorber, 0.1-2 parts of light stabilizer, 0.1-2 parts of antioxidant, and 0.1-2 parts of anti-hydrolysis agent. Although this mulch film has certain anti-ultraviolet aging performance, when using this ultraviolet absorber, there are problems of its easy migration and easy decomposition. During the processing, storage or use process, the ultraviolet absorber may precipitate from the mulch film, resulting in a decline in the anti-ultraviolet aging performance of the mulch film. In addition, the hydrophilic surface of talc powder in the reinforcing filler has poor compatibility with the hydrophobic resin, resulting in uneven dispersion. The interface defects will become the weak points attacked by ultraviolet rays, thus accelerating the aging of the mulch film. Therefore, the anti-ultraviolet aging performance of this degradable mulch film still needs to be further improved.

[0005] Thus, it can be seen that how to further improve the anti-ultraviolet aging performance of degradable mulch films is a technical problem to be solved urgently. Summary of the Invention

[0006] To solve the above technical problems, the present invention provides a weather-resistant masterbatch, its preparation method and application. By adopting a supported ultraviolet absorber, modified talcum powder and other multi-components in synergy, and combining with a specific preparation method, the anti-ultraviolet aging performance of the degradable ground film is further improved.

[0007] The present invention provides a weather-resistant masterbatch, and the weather-resistant masterbatch comprises the following components: Polybutylene adipate / terephthalate: 40 - 70 parts by weight; Polylactic acid: 10 - 20 parts; Supported ultraviolet absorber: 20 - 40 parts by weight; Modified talcum powder: 15 - 25 parts by weight; Light stabilizer: 1 - 3 parts by weight; Lubricant: 1 - 3 parts by weight; Antioxidant: 1 - 3 parts by weight; Chain extender: 1 - 3 parts by weight.

[0008] Furthermore, the polybutylene adipate / terephthalate and the polylactic acid serve as the compound carriers of the weather-resistant masterbatch. The polybutylene adipate / terephthalate endows the weather-resistant masterbatch with good ductility and impact resistance; the polylactic acid endows the weather-resistant masterbatch with high tensile strength.

[0009] Furthermore, the melt index of the polybutylene adipate / terephthalate under the conditions of a temperature of 190 °C and a load of 2.16 kg is 2 - 5 g / 10 min, and the content of terminal carboxyl groups < 15 mol / t.

[0010] Furthermore, the melt index of the polylactic acid under the conditions of a temperature of 190 °C and a load of 2.16 kg is 7 - 10 g / 10 min.

[0011] Furthermore, the supported ultraviolet absorber absorbs ultraviolet rays and converts them into harmless heat energy, so that the weather-resistant masterbatch has good anti-ultraviolet aging performance.

[0012] Furthermore, the supported ultraviolet absorber comprises silica and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, and the mass ratio of the silica to the 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol is 1:(0.3 - 0.5).

[0013] Furthermore, the preparation method of the supported ultraviolet absorber is: dissolving the silica and the 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol in acetone, then drying, and finally grinding and sieving to obtain the product.

[0014] Further, the time for the silica white and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol to dissolve in the acetone is 0.5 - 1 h.

[0015] Further, the drying temperature is 60 - 100 °C and the time is 4 - 6 h.

[0016] Further, the mesh number of the sieving is 200 - 400 meshes.

[0017] Further, the modified talcum powder is used to enhance the stiffness and heat resistance of the weather-resistant masterbatch.

[0018] Further, the modified talcum powder comprises talcum powder and a modifier, and the mass ratio of the talcum powder to the modifier is (98.5 - 98.8):(0.2 - 0.5).

[0019] The preparation method of the modified talcum powder is: adding the talcum powder and the modifier into a high-speed mixer, stirring and mixing evenly to obtain the modified talcum powder.

[0020] Further, the temperature of the high-speed mixer is 80 - 100 °C, the stirring speed is 300 - 500 r / min, and the stirring time is 5 - 8 min.

[0021] Further, the modifier is a titanate coupling agent, a silane coupling agent or an aluminate coupling agent.

[0022] Further, the light stabilizer inhibits the progress of the chain reaction by capturing free radicals generated in the photo-oxidation reaction, so that the weather-resistant masterbatch has good anti-ultraviolet aging performance.

[0023] Further, the light stabilizer is bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate or 2,2,6,6-tetramethylpiperidinol.

[0024] Further, the lubricant is used to form an isolation layer on the surface of the weather-resistant masterbatch to prevent adhesion at high temperatures.

[0025] Further, the lubricant is erucic acid amide, oleic acid amide or ethylene bisstearamide.

[0026] Further, the antioxidant is used to inhibit the oxidation reaction of poly(butylene adipate-co-terephthalate) at high temperatures and extend the service life of the weather-resistant masterbatch.

[0027] Further, the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0028] Further, the chain extender is used to react with the hydroxyl groups or carboxyl groups in the compound carrier, so as to enhance the interfacial adhesion between the polybutylene adipate / terephthalate and the polylactic acid.

[0029] Further, the chain extender is polycarbodiimide, diphenylmethane diisocyanate or diisobutyl peroxide.

[0030] The present invention provides a method for preparing a weather-resistant masterbatch, and the method includes the following steps: Step 1: Preparation of compound carrier powder: Mix the polybutylene adipate / terephthalate and the polylactic acid, then dry and grind them to obtain the compound carrier powder. Step 2: Preparation of weather-resistant masterbatch premix: Add the compound carrier powder, the supported ultraviolet absorber, the modified talc powder, the light stabilizer, the lubricant, the antioxidant and the chain extender into a mixer for mixing and stirring to obtain the weather-resistant masterbatch premix. Step 3: Preparation of weather-resistant masterbatch: Extrude the weather-resistant masterbatch premix through a twin-screw extruder, then cool, pelletize and dry to obtain the weather-resistant masterbatch.

[0031] Further, in Step 1, the drying temperature is 50-70°C and the time is 6-10 h.

[0032] Further, in Step 2, the stirring speed is 300-500 r / min and the stirring time is 3-5 min.

[0033] Further, in Step 3, the twin-screw extruder is divided into 12 temperature zones. The temperature of the first temperature zone is 90-100°C, the temperature of the second temperature zone is 100-110°C, the temperature of the third temperature zone is 110-130°C, the temperature of the fourth temperature zone is 130-150°C, the temperature of the fifth temperature zone is 140-160°C, the temperature of the sixth temperature zone is 150-170°C, the temperature of the seventh temperature zone is 170-180°C, the temperature of the eighth temperature zone is 170-180°C, the temperature of the ninth temperature zone is 170-180°C, the temperature of the tenth temperature zone is 170-180°C, the temperature of the eleventh temperature zone is 170-180°C, and the temperature of the twelfth temperature zone is 170-180°C.

[0034] Further, in Step 3, the ratio of the length to the diameter of the twin-screw extruder is 48:1, and the screw diameter is 35 mm.

[0035] Further, in the step 3, the screw speed of the twin-screw extruder is 200 - 300 r / min.

[0036] Further, in the step 3, the drying temperature is 50 - 70 °C, and the time is 6 - 10 h.

[0037] The present invention provides a degradable plastic film, which comprises the weather-resistant masterbatch and poly(butylene adipate-co-terephthalate). After ultraviolet aging, the transverse tensile strength of the degradable plastic film is 20.6 - 23.3 MPa, the longitudinal tensile strength is 17.9 - 20.8 MPa, the transverse elongation at break is 323.1 - 346.2%, and the longitudinal elongation at break is 229.3 - 265.2%.

[0038] Further, the mass ratio of the weather-resistant masterbatch to poly(butylene adipate-co-terephthalate) is (5 - 15):(85 - 95).

[0039] The present invention provides a method for preparing a degradable plastic film, which comprises the following steps: Step 1: Raw material treatment: Take the poly(butylene adipate-co-terephthalate) for drying treatment. Step 2: Preparation of the degradable plastic film premix: Take the dried poly(butylene adipate-co-terephthalate) and the weather-resistant masterbatch and add them into a mixer for mixing and stirring to obtain the degradable plastic film premix. Step 3: Preparation of the degradable plastic film: Take the film premix and blow it into a film by a blown film machine to obtain the degradable plastic film.

[0040] Further, in the step 1, the drying temperature is 50 - 70 °C, and the time is 6 - 10 h.

[0041] Further, in the step 2, the stirring speed is 300 - 500 r / min, and the stirring time is 3 - 5 min.

[0042] Further, in the step 3, the blown film machine is divided into 5 temperature zones. The temperature of the first temperature zone is 135 - 145 °C, the temperature of the second temperature zone is 145 - 155 °C, the temperature of the third temperature zone is 155 - 165 °C, the temperature of the fourth temperature zone is 165 - 175 °C, and the temperature of the fifth temperature zone is 165 - 175 °C.

[0043] Advantages of the present invention The present invention uses a supported ultraviolet absorber. Compared with the sole use of an ultraviolet absorber, the present invention has the following advantages in enhancing the anti-ultraviolet aging performance of the material: ① Fumed silica has a high specific surface area and pore structure, which can uniformly disperse the ultraviolet absorber, thus avoiding agglomeration; ② Fumed silica fixes the ultraviolet absorber through chemical bonds or physical adsorption, which can reduce its decomposition under high temperature or strong light, thereby prolonging the effective action time. For example, when using the ultraviolet absorber alone, it is easy to migrate and decompose, and has poor compatibility with polybutylene adipate / terephthalate; ③ The supported ultraviolet absorber is not easy to precipitate from the material and can maintain an effective concentration for a long time; ④ Fumed silica has ultraviolet shielding ability. After combining with the ultraviolet absorber, it can synergistically enhance the anti-ultraviolet aging performance of the material. In addition, a light stabilizer is added to the weather-resistant masterbatch, further enhancing the anti-ultraviolet aging performance of the material.

[0044] The present invention uses modified talc powder. Compared with the sole use of talc powder, the present invention has the following advantages: ① The modifier, as a surface treatment agent, can improve the compatibility of talc powder with polybutylene adipate / terephthalate, thereby significantly enhancing its dispersibility, contributing to the formation of a uniform composite material system, and thus overall enhancing various properties of the material; ② The modifier can form a monolayer on the surface of talc powder, changing its hydrophilic nature, thereby enhancing the interfacial bonding force with polybutylene adipate / terephthalate, that is, reducing interfacial defects, making the material less likely to generate microcracks or structural damage under ultraviolet irradiation, thus delaying the aging process; ③ The protective effect of the modifier can reduce the direct degradation of talc powder by ultraviolet rays, thereby improving its stability, making the material have better color retention and glossiness.

[0045] The present invention adopts a specific preparation method, that is, first preparing a weather-resistant masterbatch by the "two-step method" and then preparing a degradable mulch film. Compared with directly preparing a degradable mulch film by the "one-step method", the present invention has the following advantages: ① The proportion of polybutylene adipate / terephthalate in the degradable mulch film is extremely large. If directly mixed with other materials, it is very easy to mix unevenly, thus affecting various properties of the material. By first preparing the weather-resistant masterbatch, a small part of polybutylene adipate / terephthalate can be first mixed evenly with other materials and then mixed evenly with the remaining majority of polybutylene adipate / terephthalate. That is, the specific preparation method adopted by the present invention improves the mixing uniformity of various materials in the degradable mulch film; ② Preparing the weather-resistant masterbatch requires extrusion by a twin-screw extruder, while the polybutylene adipate / terephthalate added during the preparation of the degradable mulch film does not require extrusion by a twin-screw extruder. If preparing the degradable mulch film by the "one-step method", all of the polybutylene adipate / terephthalate needs to be extruded by a twin-screw extruder, which significantly increases the production cost. That is, the specific preparation method adopted by the present invention reduces the production cost of the degradable mulch film. Specific embodiments

[0046] Example 1 The weather-resistant masterbatch comprises the following components: 40 parts by weight of polybutylene adipate / terephthalate; 15 parts by weight of polylactic acid; 30 parts by weight of a supported ultraviolet absorber; 20 parts by weight of modified talc powder; 2 parts by weight of a light stabilizer; 1 part by weight of a lubricant; 2.5 parts by weight of an antioxidant; 3 parts by weight of a chain extender.

[0047] Method for preparing the weather-resistant masterbatch: Step 1: Preparation of the compound carrier powder: Mix polybutylene adipate / terephthalate and polylactic acid, then dry and grind them to obtain the compound carrier powder. The drying temperature is 50°C and the time is 6 h. Step 2: Preparation of the supported ultraviolet absorber: Dissolve 23.1 parts by weight of silica and 6.9 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol in acetone for 0.5 h, then dry at 60°C for 4 h, and finally grind and sieve with a mesh size of 200 to obtain the supported ultraviolet absorber. Step 3: Preparation of the modified talc powder: Add 19.7 parts by weight of talc powder and 0.3 parts by weight of titanate coupling agent to a high-speed mixer, stir and mix evenly at 80°C with a stirring speed of 300 r / min for 5 min to obtain the modified talc powder. Step 4: Preparation of the weather-resistant masterbatch premix: Add the compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, erucamide, tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide to a mixer and mix and stir at a stirring speed of 300 r / min for 3 min to obtain the weather-resistant masterbatch premix. Step 5: Preparation of the weather-resistant masterbatch: Extrude the weather-resistant masterbatch premix through a twin-screw extruder, then cool, pelletize and dry. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 90°C, the second zone is 100°C, the third zone is 110°C, the fourth zone is 130°C, the fifth zone is 140°C, the sixth zone is 150°C, the seventh zone is 170°C, the eighth zone is 170°C, the ninth zone is 170°C, the tenth zone is 170°C, the eleventh zone is 170°C, and the twelfth zone is 170°C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 200 r / min, the drying temperature is 50°C and the time is 6 h to obtain the weather-resistant masterbatch.

[0048] The degradable ground film comprises the following components: 15 parts by weight of the weather-resistant masterbatch and 85 parts by weight of polybutylene adipate / terephthalate.

[0049] Preparation method of degradable plastic film: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate for drying treatment, the drying temperature is 50 °C, and the time is 6 h; Step 2: Preparation of degradable plastic film premix: Take the dried polybutylene adipate / terephthalate and weather-resistant masterbatch and add them to a mixer for mixing and stirring. The stirring speed is 300 r / min, and the stirring time is 3 min, thus obtaining the degradable plastic film premix; Step 3: Preparation of degradable plastic film: Take the degradable plastic film premix and blow it into film by a film blowing machine, thus obtaining the degradable plastic film. The film blowing machine is divided into 5 temperature zones. The temperature of the first temperature zone is 135 °C, the temperature of the second temperature zone is 145 °C, the temperature of the third temperature zone is 155 °C, the temperature of the fourth temperature zone is 165 °C, and the temperature of the fifth temperature zone is 165 °C.

[0050] Example 2 The weather-resistant masterbatch includes the following components: 55 parts by weight of polybutylene adipate / terephthalate; 10 parts by weight of polylactic acid; 28 parts by weight of supported ultraviolet absorber; 18 parts by weight of modified talc powder; 1.8 parts by weight of light stabilizer; 2.2 parts by weight of lubricant; 1 part by weight of antioxidant; 2.7 parts by weight of chain extender.

[0051] Preparation method of weather-resistant masterbatch: Step 1: Preparation of compound carrier powder: Take polybutylene adipate / terephthalate and polylactic acid, mix them, dry them and grind them into powder, thus obtaining the compound carrier powder. The drying temperature is 70 °C, and the time is 10 h; Step 2: Preparation of supported ultraviolet absorber: Take 21.5 parts by weight of silica and 6.5 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol and dissolve them in acetone for 1 h, then dry them at a temperature of 100 °C for 6 h, and finally grind and sieve them. The sieve mesh number is 400 meshes, thus obtaining the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: Add 17.9 parts by weight of talc powder and 0.1 part by weight of titanate coupling agent to a high-speed mixer, stir and mix them at a temperature of 100 °C, a stirring speed of 500 r / min, and a stirring time of 8 min, thus obtaining the modified talc powder; Step 4: Preparation of weather-resistant masterbatch premix: Take the compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, erucamide, tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide and add them to a mixer for mixing and stirring. The stirring speed is 500 r / min, and the time is 5 min, thus obtaining the weather-resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: Take the pre-mixed weather-resistant masterbatch, extrude it through a twin-screw extruder, then cool, pelletize, and dry it. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 100°C, the second zone is 110°C, the third zone is 130°C, the fourth zone is 150°C, the fifth zone is 160°C, the sixth zone is 170°C, the seventh zone is 180°C, the eighth zone is 180°C, the ninth zone is 180°C, the tenth zone is 180°C, the eleventh zone is 180°C, and the twelfth zone is 180°C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 300 r / min, the drying temperature is 70°C, and the time is 10 h, thus obtaining the weather-resistant masterbatch.

[0052] The degradable mulch film comprises the following components: 10 parts by weight of weather-resistant masterbatch and 90 parts by weight of polybutylene adipate / terephthalate.

[0053] Preparation method of the degradable mulch film: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate and conduct drying treatment. The drying temperature is 70°C and the time is 10 h; Step 2: Preparation of the degradable mulch film pre-mix: Take the dried polybutylene adipate / terephthalate and the weather-resistant masterbatch, add them to a mixer for mixing and stirring. The stirring speed is 500 r / min and the stirring time is 5 min, thus obtaining the degradable mulch film pre-mix; Step 3: Preparation of the degradable mulch film: Take the degradable mulch film pre-mix and blow it into a film through a blown film machine, thus obtaining the degradable mulch film. The blown film machine is divided into 5 temperature zones. The temperature of the first zone is 145°C, the second zone is 155°C, the third zone is 165°C, the fourth zone is 175°C, and the fifth zone is 175°C.

[0054] Example 3 The weather-resistant masterbatch comprises the following components: 60 parts by weight of polybutylene adipate / terephthalate; 12 parts by weight of polylactic acid; 20 parts by weight of supported ultraviolet absorber; 25 parts by weight of modified talc powder; 3 parts by weight of light stabilizer; 1.5 parts by weight of lubricant; 3 parts by weight of antioxidant; 1.2 parts by weight of chain extender.

[0055] Preparation method of the weather-resistant masterbatch: Step 1: Preparation of the compounded carrier powder: Take polybutylene adipate / terephthalate and polylactic acid, mix them, dry them, and grind them into powder, thus obtaining the compounded carrier powder. The drying temperature is 60°C and the time is 8 h; Step 2: Preparation of supported ultraviolet absorber: Take 14.3 parts by weight of silica and 5.7 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol and dissolve them in acetone for 0.8 h, then dry them at 80 °C for 5 h, and finally grind and sieve them. The sieve mesh size is 300 meshes to obtain the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: Add 24.8 parts by weight of talc powder and 0.2 parts by weight of titanate coupling agent to a high-speed mixer, stir and mix them at 90 °C, with a stirring speed of 400 r / min and a stirring time of 6 min to obtain the modified talc powder; Step 4: Preparation of weather-resistant masterbatch premix: Take the compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, erucamide, tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide and add them to a mixer for mixing and stirring. The stirring speed is 400 r / min and the time is 4 min to obtain the weather-resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: Take the weather-resistant masterbatch premix and extrude it through a twin-screw extruder, then cool, pelletize and dry it. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first temperature zone is 95 °C, the temperature of the second temperature zone is 105 °C, the temperature of the third temperature zone is 120 °C, the temperature of the fourth temperature zone is 140 °C, the temperature of the fifth temperature zone is 150 °C, the temperature of the sixth temperature zone is 160 °C, the temperature of the seventh temperature zone is 175 °C, the temperature of the eighth temperature zone is 175 °C, the temperature of the ninth temperature zone is 175 °C, the temperature of the tenth temperature zone is 175 °C, the temperature of the eleventh temperature zone is 175 °C, the temperature of the twelfth temperature zone is 175 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 250 r / min, and the drying temperature is 60 °C for 8 h to obtain the weather-resistant masterbatch.

[0056] The degradable mulch film comprises the following components: 5 parts by weight of weather-resistant masterbatch and 95 parts by weight of polybutylene adipate / terephthalate.

[0057] Preparation method of degradable mulch film: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate and perform a drying treatment at 60 °C for 8 h; Step 2: Preparation of degradable mulch film premix: Take the dried polybutylene adipate / terephthalate and weather-resistant masterbatch and add them to a mixer for mixing and stirring. The stirring speed is 400 r / min and the stirring time is 4 min to obtain the degradable mulch film premix; Step 3: Preparation of Degradable Mulch Film: The degradable mulch film premix is taken and blown into film by a film blowing machine to obtain the degradable mulch film. The film blowing machine is divided into 5 temperature zones. The temperature of the first temperature zone is 140 °C, the temperature of the second temperature zone is 150 °C, the temperature of the third temperature zone is 160 °C, the temperature of the fourth temperature zone is 170 °C, and the temperature of the fifth temperature zone is 170 °C.

[0058] Example 4 The weather-resistant masterbatch comprises the following components: 70 parts by weight of polybutylene adipate / terephthalate; 18 parts by weight of polylactic acid; 35 parts by weight of supported ultraviolet absorber; 16 parts by weight of modified talc powder; 1 part by weight of light stabilizer; 3 parts by weight of lubricant; 2 parts by weight of antioxidant; 2.3 parts by weight of chain extender.

[0059] Preparation method of the weather-resistant masterbatch: Step 1: Preparation of compound carrier powder: Polybutylene adipate / terephthalate and polylactic acid are taken, mixed, dried, and ground to obtain the compound carrier powder. The drying temperature is 55 °C and the time is 7 h; Step 2: Preparation of supported ultraviolet absorber: 25 parts by weight of white carbon black and 10 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol are dissolved in acetone for 0.6 h, then dried at a temperature of 70 °C for 5 h, and finally ground and sieved. The sieve mesh number is 250 meshes to obtain the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: 15.9 parts by weight of talc powder and 0.1 part by weight of silane coupling agent are added to a high-speed mixer, stirred and mixed at a temperature of 85 °C, a stirring speed of 450 r / min, and a stirring time of 7 min to obtain the modified talc powder; Step 4: Preparation of weather-resistant masterbatch premix: The compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, oleamide, dilauryl thiodipropionate, and diphenylmethane diisocyanate are added to a mixer and mixed and stirred at a stirring speed of 350 r / min for 4 min to obtain the weather-resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: The weather-resistant masterbatch premix is extruded through a twin-screw extruder, then cooled, pelletized, and dried. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 90°C, the second zone is 110°C, the third zone is 120°C, the fourth zone is 140°C, the fifth zone is 155°C, the sixth zone is 165°C, the seventh zone is 170°C, the eighth zone is 175°C, the ninth zone is 175°C, the tenth zone is 175°C, the eleventh zone is 175°C, and the twelfth zone is 175°C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 220 r / min, the drying temperature is 55°C, and the time is 9 h, thus obtaining the weather-resistant masterbatch.

[0060] The degradable mulch film comprises the following components: 12 parts by weight of weather-resistant masterbatch and 88 parts by weight of polybutylene adipate / terephthalate.

[0061] Preparation method of the degradable mulch film: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate for drying treatment, the drying temperature is 55°C, and the time is 7 h; Step 2: Preparation of the degradable mulch film premix: Take the dried polybutylene adipate / terephthalate and the weather-resistant masterbatch and add them to a mixer for mixing and stirring. The stirring speed is 450 r / min, and the stirring time is 3.5 min, thus obtaining the degradable mulch film premix; Step 3: Preparation of the degradable mulch film: Take the degradable mulch film premix and blow it into a film through a blown film machine, thus obtaining the degradable mulch film. The blown film machine is divided into 5 temperature zones. The temperature of the first zone is 138°C, the second zone is 148°C, the third zone is 158°C, the fourth zone is 168°C, and the fifth zone is 170°C.

[0062] Example 5 The weather-resistant masterbatch comprises the following components: 48 parts by weight of polybutylene adipate / terephthalate; 20 parts by weight of polylactic acid; 40 parts by weight of supported ultraviolet absorber; 22 parts by weight of modified talc powder; 2.8 parts by weight of light stabilizer; 2 parts by weight of lubricant; 1.7 parts by weight of antioxidant; 1 part by weight of chain extender.

[0063] Preparation method of the weather-resistant masterbatch: Step 1: Preparation of the compound carrier powder: Take polybutylene adipate / terephthalate and polylactic acid, mix them and then dry and grind them to obtain the compound carrier powder. The drying temperature is 65°C, and the time is 9 h; Step 2: Preparation of supported ultraviolet absorber: Take 26.7 parts by weight of silica and 13.3 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol and dissolve them in acetone for 0.9 h, then dry at 90 °C for 5 h, and finally grind and sieve with a sieve mesh of 350 meshes to obtain the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: Add 21.8 parts by weight of talc powder and 0.2 parts by weight of silane coupling agent to a high-speed mixer, stir and mix evenly at 95 °C with a stirring speed of 380 r / min for 5.5 min to obtain the modified talc powder; Step 4: Preparation of weather-resistant masterbatch premix: Take the compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, oleic acid amide, dilauryl thiodipropionate and diphenylmethane diisocyanate and add them to a mixer for mixing and stirring at a stirring speed of 480 r / min for 4.2 min to obtain the weather-resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: Take the weather-resistant masterbatch premix, extrude it through a twin-screw extruder, then cool, pelletize and dry. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 100 °C, the second zone is 105 °C, the third zone is 125 °C, the fourth zone is 145 °C, the fifth zone is 155 °C, the sixth zone is 165 °C, the seventh zone is 172 °C, the eighth zone is 178 °C, the ninth zone is 178 °C, the tenth zone is 178 °C, the eleventh zone is 178 °C, and the twelfth zone is 178 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 280 r / min, and the drying temperature is 65 °C for 7 h to obtain the weather-resistant masterbatch.

[0064] The degradable ground film comprises the following components: 10 parts by weight of weather-resistant masterbatch and 90 parts by weight of poly(butylene adipate-co-terephthalate).

[0065] Preparation method of degradable ground film: Step 1: Raw material treatment: Take poly(butylene adipate-co-terephthalate) for drying treatment at 65 °C for 9 h; Step 2: Preparation of degradable ground film premix: Take the dried poly(butylene adipate-co-terephthalate) and weather-resistant masterbatch and add them to a mixer for mixing and stirring at a stirring speed of 380 r / min for 4.8 min to obtain the degradable ground film premix; Step 3: Preparation of degradable mulch film: Take the pre - mixture of degradable mulch film and blow it into film by a film blowing machine. The film blowing machine is divided into 5 temperature zones. The temperature of the first zone is 142 °C, the second zone is 152 °C, the third zone is 162 °C, the fourth zone is 172 °C, and the fifth zone is 175 °C.

[0066] Example 6 The weather - resistant masterbatch includes the following components: Poly(butylene adipate - co - terephthalate) 52 parts by weight; polylactic acid 17 parts by weight; supported ultraviolet absorber 25 parts by weight; modified talc powder 15 parts by weight; light stabilizer 1.3 parts by weight; lubricant 1 part by weight; antioxidant 3 parts by weight; chain extender 2.5 parts by weight.

[0067] Preparation method of the weather - resistant masterbatch: Step 1: Preparation of compound carrier powder: Take poly(butylene adipate - co - terephthalate) and polylactic acid, mix them and then dry and grind them to obtain the compound carrier powder. The drying temperature is 50 °C and the time is 10 h; Step 2: Preparation of supported ultraviolet absorber: Take 19.2 parts by weight of silica and 5.8 parts by weight of 2 - (4,6 - diphenyl - 1,3,5 - triazin - 2 - yl) - 5 - hexyloxyphenol, dissolve them in acetone for 0.5 h, then dry at 100 °C for 4 h, and finally grind and sieve them. The sieve mesh size is 300 meshes to obtain the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: Add 14.9 parts by weight of talc powder and 0.1 part by weight of silane coupling agent to a high - speed mixer, stir and mix them at 80 °C, the stirring speed is 500 r / min, and the stirring time is 6 min to obtain the modified talc powder; Step 4: Preparation of weather - resistant masterbatch premix: Take the compound carrier powder, supported ultraviolet absorber, modified talc powder, bis(1,2,2,6,6 - pentamethyl - 4 - piperidyl) sebacate, oleic acid amide, dilauryl thiodipropionate and diphenylmethane diisocyanate, add them to a mixer and mix and stir at a stirring speed of 300 r / min for 5 min to obtain the weather - resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: The weather-resistant masterbatch premix is extruded by a twin-screw extruder, then cooled, pelletized, and dried. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 90 °C, the second zone is 100 °C, the third zone is 110 °C, the fourth zone is 130 °C, the fifth zone is 160 °C, the sixth zone is 170 °C, the seventh zone is 180 °C, the eighth zone is 180 °C, the ninth zone is 180 °C, the tenth zone is 180 °C, the eleventh zone is 180 °C, and the twelfth zone is 180 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 200 r / min, the drying temperature is 70 °C, and the time is 6 h, thus obtaining the weather-resistant masterbatch.

[0068] The degradable mulch film comprises the following components: 14 parts by weight of weather-resistant masterbatch and 86 parts by weight of polybutylene adipate / terephthalate.

[0069] Preparation method of the degradable mulch film: Step 1: Raw material treatment: Polybutylene adipate / terephthalate is taken for drying treatment, the drying temperature is 70 °C, and the time is 6 h; Step 2: Preparation of degradable mulch film premix: The dried polybutylene adipate / terephthalate and weather-resistant masterbatch are added into a mixer for mixing and stirring. The stirring speed is 500 r / min, and the stirring time is 3 min, thus obtaining the degradable mulch film premix; Step 3: Preparation of degradable mulch film: The degradable mulch film premix is blown into film by a blown film machine, thus obtaining the degradable mulch film. The blown film machine is divided into 5 temperature zones. The temperature of the first zone is 135 °C, the second zone is 155 °C, the third zone is 165 °C, the fourth zone is 170 °C, and the fifth zone is 175 °C.

[0070] Example 7 The weather-resistant masterbatch comprises the following components: 43 parts by weight of polybutylene adipate / terephthalate; 13 parts by weight of polylactic acid; 38 parts by weight of supported ultraviolet absorber; 24 parts by weight of modified talc powder; 3 parts by weight of light stabilizer; 2.9 parts by weight of lubricant; 1.1 parts by weight of antioxidant; 1 part by weight of chain extender.

[0071] Preparation method of the weather-resistant masterbatch: Step 1: Preparation of compound carrier powder: Polybutylene adipate / terephthalate and polylactic acid are mixed, then dried and ground into powder, thus obtaining the compound carrier powder. The drying temperature is 70 °C, and the time is 6 h; Step 2: Preparation of supported ultraviolet absorber: Take 27.1 parts by weight of silica and 10.9 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol and dissolve them in acetone for 1 h, then dry them at a temperature of 60 °C for 6 h, and finally grind and screen them. The mesh number of the screen is 400 meshes, and the supported ultraviolet absorber is obtained; Step 3: Preparation of modified talc powder: Add 23.8 parts by weight of talc powder and 0.2 parts by weight of aluminate coupling agent to a high-speed mixer, stir and mix evenly at a temperature of 100 °C, a stirring speed of 300 r / min, and a stirring time of 8 min, and the modified talc powder is obtained; Step 4: Preparation of weather-resistant masterbatch premix: Take the compound carrier powder, supported ultraviolet absorber, modified talc powder, 2,2,6,6-tetramethylpiperidinol, ethylene bisstearamide, pentaerythritol tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and diisobutyl peroxide and add them to a mixer for mixing and stirring at a stirring speed of 500 r / min for 3 min, and the weather-resistant masterbatch premix is obtained; Step 5: Preparation of weather-resistant masterbatch: Take the weather-resistant masterbatch premix, extrude it through a twin-screw extruder, then cool, pelletize, and dry it. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first temperature zone is 95 °C, the temperature of the second temperature zone is 105 °C, the temperature of the third temperature zone is 130 °C, the temperature of the fourth temperature zone is 140 °C, the temperature of the fifth temperature zone is 150 °C, the temperature of the sixth temperature zone is 160 °C, the temperature of the seventh temperature zone is 170 °C, the temperature of the eighth temperature zone is 170 °C, the temperature of the ninth temperature zone is 170 °C, the temperature of the tenth temperature zone is 170 °C, the temperature of the eleventh temperature zone is 170 °C, and the temperature of the twelfth temperature zone is 170 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 300 r / min, the drying temperature is 50 °C, and the time is 10 h, and the weather-resistant masterbatch is obtained.

[0072] The degradable ground film comprises the following components: 6 parts by weight of weather-resistant masterbatch and 94 parts by weight of poly(butylene adipate-co-terephthalate).

[0073] Preparation method of degradable ground film: Step 1: Raw material treatment: Take poly(butylene adipate-co-terephthalate) and carry out drying treatment at a drying temperature of 50 °C for 10 h; Step 2: Preparation of degradable ground film premix: Take the dried poly(butylene adipate-co-terephthalate) and weather-resistant masterbatch and add them to a mixer for mixing and stirring at a stirring speed of 300 r / min for 5 min, and the degradable ground film premix is obtained; Step 3: Preparation of degradable mulch film: The degradable mulch film premix is taken and blown into film by a blown film machine to obtain the degradable mulch film. The blown film machine is divided into 5 temperature zones. The temperature of the first temperature zone is 145 °C, the temperature of the second temperature zone is 145 °C, the temperature of the third temperature zone is 165 °C, the temperature of the fourth temperature zone is 175 °C, and the temperature of the fifth temperature zone is 175 °C.

[0074] Example 8 The weather-resistant masterbatch comprises the following components: 65 parts by weight of polybutylene adipate / terephthalate; 19 parts by weight of polylactic acid; 22 parts by weight of supported ultraviolet absorber; 19 parts by weight of modified talc powder; 2.1 parts by weight of light stabilizer; 2.6 parts by weight of lubricant; 2.4 parts by weight of antioxidant; 3 parts by weight of chain extender.

[0075] Preparation method of the weather-resistant masterbatch: Step 1: Preparation of compound carrier powder: Polybutylene adipate / terephthalate and polylactic acid are taken, mixed, dried and ground to obtain the compound carrier powder. The drying temperature is 60 °C and the time is 7 h; Step 2: Preparation of supported ultraviolet absorber: 15.7 parts by weight of silica and 6.3 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol are dissolved in acetone for 0.7 h, then dried at a temperature of 85 °C for 4.5 h, and finally ground and sieved. The sieve mesh number is 300 meshes to obtain the supported ultraviolet absorber; Step 3: Preparation of modified talc powder: 18.9 parts by weight of talc powder and 0.1 part by weight of aluminate coupling agent are added to a high-speed mixer, stirred and mixed evenly. The temperature is 92 °C, the stirring speed is 420 r / min, and the stirring time is 7 min to obtain the modified talc powder; Step 4: Preparation of weather-resistant masterbatch premix: The compound carrier powder, supported ultraviolet absorber, modified talc powder, 2,2,6,6-tetramethylpiperidinol, ethylene bisstearamide, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and diisobutyl peroxide are added to a mixer for mixing and stirring. The stirring speed is 430 r / min and the time is 4 min to obtain the weather-resistant masterbatch premix; Step 5: Preparation of weather-resistant masterbatch: The weather-resistant masterbatch premix is extruded through a twin-screw extruder, then cooled, pelletized, and dried. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 90 °C, the second zone is 110 °C, the third zone is 120 °C, the fourth zone is 140 °C, the fifth zone is 150 °C, the sixth zone is 170 °C, the seventh zone is 175 °C, the eighth zone is 175 °C, the ninth zone is 175 °C, the tenth zone is 175 °C, the eleventh zone is 175 °C, and the twelfth zone is 175 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 240 r / min, the drying temperature is 60 °C, and the time is 9 h, thus obtaining the weather-resistant masterbatch.

[0076] The degradable mulch film comprises the following components: 10 parts by weight of weather-resistant masterbatch and 90 parts by weight of polybutylene adipate / terephthalate.

[0077] Preparation method of the degradable mulch film: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate for drying treatment, the drying temperature is 60 °C, and the time is 7 h; Step 2: Preparation of degradable mulch film premix: Take the dried polybutylene adipate / terephthalate and weather-resistant masterbatch and add them to a mixer for mixing and stirring. The stirring speed is 420 r / min, and the stirring time is 4 min, thus obtaining the degradable mulch film premix; Step 3: Preparation of degradable mulch film: Take the degradable mulch film premix and blow it into film through a blown film machine, thus obtaining the degradable mulch film. The blown film machine is divided into 5 temperature zones. The temperature of the first zone is 140 °C, the second zone is 152 °C, the third zone is 160 °C, the fourth zone is 170 °C, and the fifth zone is 172 °C.

[0078] Comparative Example 1 Masterbatch 1 comprises the following components: 40 parts by weight of polybutylene adipate / terephthalate; 15 parts by weight of polylactic acid; 30 parts by weight of ultraviolet absorber; 20 parts by weight of modified talc powder; 2 parts by weight of light stabilizer; 1 part by weight of lubricant; 2.5 parts by weight of antioxidant; 3 parts by weight of chain extender.

[0079] Preparation method of Masterbatch 1: Step 1: Preparation of compound carrier powder: Take polybutylene adipate / terephthalate and polylactic acid, mix them and then dry and grind them to obtain the compound carrier powder. The drying temperature is 50 °C, and the time is 6 h; Step 2: Preparation of modified talc powder: Add 19.7 parts by weight of talc powder and 0.3 parts by weight of titanate coupling agent into a high-speed mixer, stir and mix evenly. The temperature is 80 °C, the stirring speed is 300 r / min, and the stirring time is 5 min to obtain the modified talc powder; Step 3: Preparation of masterbatch 1 premix: Take the compound carrier powder, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, modified talc powder, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, erucamide, tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide and add them into a mixer for mixing and stirring. The stirring speed is 300 r / min and the time is 3 min to obtain the masterbatch 1 premix; Step 4: Preparation of masterbatch 1: Take the masterbatch 1 premix and extrude it through a twin-screw extruder, then cool, pelletize and dry. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first temperature zone is 90 °C, the second temperature zone is 100 °C, the third temperature zone is 110 °C, the fourth temperature zone is 130 °C, the fifth temperature zone is 140 °C, the sixth temperature zone is 150 °C, the seventh temperature zone is 170 °C, the eighth temperature zone is 170 °C, the ninth temperature zone is 170 °C, the tenth temperature zone is 170 °C, the eleventh temperature zone is 170 °C, and the twelfth temperature zone is 170 °C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 200 r / min, the drying temperature is 50 °C, and the time is 6 h to obtain masterbatch 1.

[0080] The degradable ground film 1 comprises the following components: 15 parts by weight of masterbatch 1 and 85 parts by weight of polybutylene adipate / terephthalate.

[0081] Preparation method of the degradable ground film 1: Step 1: Raw material treatment: Take polybutylene adipate / terephthalate for drying treatment. The drying temperature is 50 °C and the time is 6 h; Step 2: Preparation of the degradable ground film premix: Take the dried polybutylene adipate / terephthalate and masterbatch 1 and add them into a mixer for mixing and stirring. The stirring speed is 300 r / min and the stirring time is 3 min to obtain the degradable ground film 1 premix; Step 3: Preparation of the degradable ground film 1: Take the degradable ground film 1 premix and blow it into a film through a blown film machine to obtain the degradable ground film 1. The blown film machine is divided into 5 temperature zones. The temperature of the first temperature zone is 135 °C, the second temperature zone is 145 °C, the third temperature zone is 155 °C, the fourth temperature zone is 165 °C, and the fifth temperature zone is 165 °C.

[0082] Comparative Example 2 The degradable ground film 2 comprises the following components: 1005 parts by weight of polybutylene adipate / terephthalate; 15 parts by weight of polylactic acid; 30 parts by weight of a supported ultraviolet absorber; 20 parts by weight of modified talcum powder; 2 parts by weight of a light stabilizer; 1 part by weight of a lubricant; 2.5 parts by weight of an antioxidant; 3 parts by weight of a chain extender.

[0083] Preparation method of the degradable ground film 2: Step 1: Preparation of a compound carrier powder: Mix polybutylene adipate / terephthalate and polylactic acid, then dry and grind them to obtain the compound carrier powder. The drying temperature is 50°C and the time is 6 h. Step 2: Preparation of the supported ultraviolet absorber: Dissolve 23.1 parts by weight of silica and 6.9 parts by weight of 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol in acetone for 0.5 h, then dry at 60°C for 4 h, and finally grind and screen with a mesh number of 200 to obtain the supported ultraviolet absorber. Step 3: Preparation of the modified talcum powder: Add 19.7 parts by weight of talcum powder and 0.3 parts by weight of titanate coupling agent to a high-speed mixer, stir and mix evenly at 80°C with a stirring speed of 300 r / min for 5 min to obtain the modified talcum powder. Step 4: Preparation of the pre-mix of the degradable ground film 2: Add the compound carrier powder, the supported ultraviolet absorber, the modified talcum powder, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, erucamide, tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide to a mixer for mixing and stirring at a stirring speed of 300 r / min for 3 min to obtain the pre-mix of the degradable ground film 2. Step 5: Preparation of the modified material of the degradable ground film 2: Extrude the pre-mix of the degradable ground film 2 through a twin-screw extruder, then cool, pelletize and dry. The twin-screw extruder is divided into 12 temperature zones. The temperature of the first zone is 90°C, the second zone is 100°C, the third zone is 110°C, the fourth zone is 130°C, the fifth zone is 140°C, the sixth zone is 150°C, the seventh zone is 170°C, the eighth zone is 170°C, the ninth zone is 170°C, the tenth zone is 170°C, the eleventh zone is 170°C, and the twelfth zone is 170°C. The length-diameter ratio of the twin-screw extruder is 48:1, the screw diameter is 35 mm, the screw speed is 200 r / min, the drying temperature is 50°C and the time is 6 h to obtain the modified material of the degradable ground film 2. Step 6: Preparation of the degradable plastic film 2: After taking the modified material of the degradable plastic film 2 and blowing it into a film by a film blowing machine, the degradable plastic film 2 is obtained. The film blowing machine is divided into 5 temperature zones. The temperature of the first temperature zone is 135°C, the temperature of the second temperature zone is 145°C, the temperature of the third temperature zone is 155°C, the temperature of the fourth temperature zone is 165°C, and the temperature of the fifth temperature zone is 165°C.

[0084] Table 1 Comparison of Tensile Properties and Production Costs of Degradable Plastic Films Prepared in Examples 1-8 and Comparative Examples 1-2 before and after UV Aging

[0085] In summary, as shown in Table 1, the tensile strength and elongation at break of the degradable plastic film in the present invention (Examples 1-8) before UV aging are generally consistent with those of the prior art (Comparative Examples 1-2). However, the decrease in the tensile strength and elongation at break of the degradable plastic film in the present invention after UV aging is significantly smaller than that of the prior art. This is because in Comparative Example 1, only 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol is used as the UV absorber, and in Comparative Example 2, the degradable plastic film is directly prepared by the "one-step method"; while the present invention uses a supported UV absorber and modified talc powder and other multi-components in cooperation, and combines a specific preparation method (the "two-step method": first prepare the weather-resistant masterbatch, and then prepare the degradable plastic film), thereby comprehensively improving the anti-UV aging performance of the degradable plastic film.

[0086] In addition, the preparation of the weather-resistant masterbatch needs to be extruded by a twin-screw extruder, and the polybutylene adipate / terephthalate added during the preparation of the degradable plastic film does not need to be extruded by a twin-screw extruder. If the degradable plastic film is prepared by the "one-step method", all the polybutylene adipate / terephthalate needs to be extruded by a twin-screw extruder, which significantly increases the production cost. That is, the specific preparation method adopted by the present invention reduces the production cost of the degradable plastic film compared with the prior art (Comparative Example 2).

[0087] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any other form. Any modification or equivalent change made according to the technical essence of the present invention still belongs to the scope protected by the present invention.

Claims

1. A weather-resistant masterbatch, characterized in that, The weather-resistant masterbatch comprises the following components: Polybutylene adipate / terephthalate: 40 - 70 parts by weight; Polylactic acid: 10 - 20 parts; Supported ultraviolet absorber: 20 - 40 parts by weight; Modified talc powder: 15 - 25 parts by weight; Light stabilizer: 1 - 3 parts by weight; Lubricant: 1 - 3 parts by weight; Antioxidant: 1 - 3 parts by weight; Chain extender: 1 - 3 parts by weight.

2. The weather-resistant masterbatch according to claim 1, characterized in that, The supported ultraviolet absorber comprises silica and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, and the mass ratio of the silica to the 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol is 1:(0.3 - 0.5).

3. The weather-resistant masterbatch according to claim 2, wherein The preparation method of the supported ultraviolet absorber is as follows: Dissolve the silica and the 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol in acetone, then dry, and finally grind and sieve to obtain it.

4. The weather-resistant masterbatch according to claim 1, wherein, The modified talc powder comprises talc powder and a modifier, and the mass ratio of the talc powder to the modifier is (98.5 - 98.8):(0.2 - 0.5).

5. The weather-resistant masterbatch according to claim 4, characterized in that, The preparation method of the modified talc powder is as follows: Add the talc powder and the modifier into a high-speed mixer, stir and mix evenly to obtain it.

6. A method for preparing the weather-resistant masterbatch according to any one of claims 1-5, characterized in that, The method comprises the following steps: Step 1: Preparation of the compound carrier powder: Mix the polybutylene adipate / terephthalate and the polylactic acid, then dry and grind into powder to obtain the compound carrier powder; Step 2: Preparation of the weather-resistant masterbatch premix: Add the compound carrier powder, the supported ultraviolet absorber, the modified talc powder, the light stabilizer, the lubricant, the antioxidant and the chain extender into a mixer, mix and stir to obtain the weather-resistant masterbatch premix; Step 3: Preparation of the weather-resistant masterbatch: Extrude the weather-resistant masterbatch premix through a twin-screw extruder, then cool, pelletize and dry to obtain the weather-resistant masterbatch.

7. The method according to claim 6, characterized in that, In Step 3, the twin-screw extruder is divided into 12 temperature zones. The temperature of the first temperature zone is 90 - 100 °C, the temperature of the second temperature zone is 100 - 110 °C, the temperature of the third temperature zone is 110 - 130 °C, the temperature of the fourth temperature zone is 130 - 150 °C, the temperature of the fifth temperature zone is 140 - 160 °C, the temperature of the sixth temperature zone is 150 - 170 °C, the temperature of the seventh temperature zone is 170 - 180 °C, the temperature of the eighth temperature zone is 170 - 180 °C, the temperature of the ninth temperature zone is 170 - 180 °C, the temperature of the tenth temperature zone is 170 - 180 °C, the temperature of the eleventh temperature zone is 170 - 180 °C, and the temperature of the twelfth temperature zone is 170 - 180 °C.

8. A degradable plastic film, characterized in that, The degradable ground film comprises the weather-resistant masterbatch and the polybutylene adipate / terephthalate. After ultraviolet aging, the transverse tensile strength of the degradable ground film is 20.6 - 23.3 MPa, the longitudinal tensile strength is 17.9 - 20.8 MPa, the transverse elongation at break is 323.1 - 346.2%, and the longitudinal elongation at break is 229.3 - 265.2%.

9. A method for preparing the degradable ground film according to claim 8, characterized in that, The method comprises the following steps: Step 1: Raw material processing: taking the polybutylene adipate / terephthalate and performing drying processing; Step 2: Preparation of a degradable mulch film premix: adding the dried polybutylene adipate / terephthalate and the weather-resistant masterbatch into a mixer, mixing and stirring to obtain a degradable mulch film premix; Step 3: Preparation of degradable mulch film: The mulch film premix is ​​blown by a film blowing machine to obtain the degradable mulch film.

10. The method according to claim 9, wherein In step 3, the film blowing machine is divided into 5 temperature zones, the temperature of the first temperature zone is 135-145°C, the temperature of the second temperature zone is 145-155°C, the temperature of the third temperature zone is 155-165°C, the temperature of the fourth temperature zone is 165-175°C, and the temperature of the fifth temperature zone is 165-175°C.

Citation Information

Cited By

  • Ultraviolet-proof degradable film for corn for seed production and preparation method of ultraviolet-proof degradable film

    CN121343335A