Anti-aging modified asphalt and preparation method thereof

By introducing additives such as nanomontmorillonium modifiers, a composite system is constructed, which solves the problems of fast aging and easy failure of additives in traditional modified asphalt, and has achieved significant improvements in high temperature stability, low temperature flexibility and weather resistance, and is suitable for a variety of roads and infrastructures.

CN120290007AInactive Publication Date: 2025-07-11HUNAN YIBANG NEW MATERIAL CO LTD

Patent Information

Application Number
CN202510765084.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-10
Publication Date
2025-07-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional modified asphalt has fast aging rate and fast weather resistance under long-term environmental exposure conditions. In existing anti-aging technologies, additives are prone to migration, volatilization, and failure, and cannot effectively shield ultraviolet rays or capture free radicals, resulting in fast attenuation of material properties and high maintenance costs. Traditional inorganic additives fail to take into account both flexibility and long-term stability.

Method used

Additions such as nanomontmorillonite modifiers, phosphate-type flame retardant anti-aging agents, bio-based polyphenol antioxidants, silicone grafted polymers and carbon quantum dot light stabilizers are used to construct a composite system of multiple shielding, radical scavenging and polymer enhancement to improve the high-temperature stability, low-temperature flexibility and water resistance of asphalt.

Benefits of technology

It significantly delays the aging process of materials, improves service life, reduces maintenance frequency, has excellent anti-aging performance and broad application prospects, and is suitable for special scenarios such as high-grade highways, urban expressways, large bridge paving, tunnels, heavy-duty airport runways, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120290007A_ABST
    Figure CN120290007A_ABST
Patent Text Reader

Abstract

The invention discloses anti-aging modified asphalt and a preparation method thereof, and relates to the technical field of building materials, the anti-aging modified asphalt comprises the following specific components: base petroleum asphalt, a thermoplastic elastomer, an anti-stripping agent, an ultraviolet absorbent, an antioxidant and a softening agent; the additive comprises a nano montmorillonite modifier, a phosphate type flame-retardant anti-aging agent, a bio-based polyphenol antioxidant, a siloxane graft polymer and a carbon quantum dot light stabilizer; the preparation is performed based on the components. On the basis of a traditional modification system, multiple additives are cooperatively introduced, and a composite system with multiple shielding, free radical scavenging, weather-proof protection and macromolecule enhancement functions is constructed. According to the modification system, the high-temperature stability, the low-temperature flexibility and the water resistance of the asphalt material are remarkably improved on the macroscopic level, and meanwhile the aging process of the material is greatly delayed through the nanoscale barrier effect, the long-acting anti-oxidation mechanism and the light stabilization mechanism on the microscopic level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, and specifically to an anti-aging modified asphalt and a preparation method thereof. Background Art

[0002] As an important raw material for road engineering and building waterproof materials, asphalt is widely used in various environments. However, traditional modified asphalt systems usually only improve their performance by introducing thermoplastic elastomers, anti-stripping agents, conventional ultraviolet absorbers, and general-purpose antioxidants. Although this modification method improves the high-temperature stability and low-temperature crack resistance of asphalt to a certain extent, there are still obvious deficiencies under long-term environmental exposure conditions (such as ultraviolet irradiation, oxidation, thermal aging, etc.), especially manifested in problems such as fast aging rate, rapid attenuation of weather resistance, surface cracking, and aggravated peeling phenomenon. In addition, most of the ultraviolet absorbers and antioxidants used in existing anti-aging technologies are small-molecule types, which are easy to migrate, volatilize, and fail, resulting in limited durability of the materials.

[0003] Especially in the fields of anti-photoaging and deep antioxidant, the types of commonly used additives are single and their functional effects are limited. They cannot effectively shield ultraviolet rays or continuously capture free radicals at the microscopic scale, resulting in fast performance attenuation and high maintenance costs of asphalt materials in actual use. At the same time, conventional flame retardant or anti-stripping modification mostly relies on traditional inorganic additives, failing to take into account the flexibility and long-term stability of asphalt materials, further restricting the development of high-performance road materials. Summary of the Invention

[0004] Aiming at the deficiencies of the prior art, the present invention provides an anti-aging modified asphalt and a preparation method thereof to solve the problems raised in the above background art.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] An embodiment of the present invention provides an anti-aging modified asphalt, including the following specific components:

[0007] Base petroleum asphalt, thermoplastic elastomer, anti-stripping agent, ultraviolet absorber, antioxidant, and softening agent;

[0008] The modified asphalt further includes additives, and the additives specifically include:

[0009] Nanometer montmorillonite modifier, phosphoric acid ester type flame retardant and anti-aging agent, bio-based polyphenol antioxidant, silicone graft polymer, and carbon quantum dot light stabilizer.

[0010] Further optimizing the technical solution, the mass parts of the specific components are as follows:

[0011] Base petroleum asphalt is 80 - 120 parts;

[0012] The thermoplastic elastomer is 3 - 6 parts;

[0013] The anti - stripping agent is 0.3 - 0.8 part;

[0014] The ultraviolet absorber is 0.5 - 1.5 parts;

[0015] The antioxidant is 0.5 - 1 part;

[0016] The softening agent is 2 - 5 parts.

[0017] To further optimize this technical solution, the mass parts of the additives are as follows:

[0018] The nano - montmorillonite modifier is 1 - 3 parts;

[0019] The phosphate - type flame - retardant and anti - aging agent is 0.5 - 1.5 parts;

[0020] The bio - based polyphenol antioxidant is 1 - 2 parts;

[0021] The silicone - oxygen - alkane grafted polymer is 0.8 - 2.5 parts;

[0022] The carbon quantum dot light stabilizer is 0.1 - 0.5 part.

[0023] To further optimize this technical solution, the nano - montmorillonite modifier includes natural montmorillonite and an organic intercalating agent. Montmorillonite powder with a particle size distribution in the range of 50 - 100 nm is selected, and dodecyltrimethylammonium bromide (DTAB) is used as the organic intercalating agent;

[0024] The natural montmorillonite and the organic intercalating agent are stirred and reacted for 6 hours at 80 °C through an ion - exchange reaction to obtain organically modified nano - montmorillonite, and then ultrasonic dispersion treatment is carried out to obtain the nano - montmorillonite modifier with a lamellar structure.

[0025] To further optimize this technical solution, the phosphate - type flame - retardant and anti - aging agent is an esterification product formed with pentaerythritol, phosphoric acid and fatty alcohol as reaction monomers;

[0026] The molecular structure of the phosphate - type flame - retardant and anti - aging agent contains P - O - C bonds, the degree of esterification is in the range of 85 - 95%, and the carbon chain number of the fatty alcohol is 8 - 18.

[0027] To further optimize this technical solution, the bio - based polyphenol antioxidant adopts a micro - capsule particle structure, the coating shell material is cyclodextrin or gelatin shell material, and the internal material is epigallocatechin gallate (EGCG) and proanthocyanidins; the particle size of the micro - capsule particles is 1 - 5 μm.

[0028] To further optimize this technical solution, the siloxane-grafted polymer includes a main chain of polybutadiene PB and a siloxane PDMS side chain introduced onto the PB chain through maleic anhydride grafting reaction.

[0029] To further optimize this technical solution, in the carbon quantum dot light stabilizer, the particle size of the carbon quantum dots is less than 10 nm, the surface contains carboxyl, hydroxyl, and amino functional groups, and at the same time, chitosan is used for surface modification.

[0030] A preparation method of an anti-aging modified asphalt is based on the above-mentioned modified asphalt and includes the following specific steps:

[0031] S1. Pretreatment of the base petroleum asphalt and preliminary compounding with the thermoplastic elastomer;

[0032] S2. Compound addition of an anti-stripping agent, an ultraviolet absorber, and an antioxidant;

[0033] S3. Addition of a softening agent to improve fluidity and low-temperature performance;

[0034] S4. Compound addition of a nano-montmorillonite modifier and a phosphate ester type flame retardant and anti-aging agent;

[0035] S5. Addition of a bio-based polyphenol antioxidant and a siloxane-grafted polymer;

[0036] S6. Addition of a carbon quantum dot light stabilizer and completion of the preparation of the finished product.

[0037] To further optimize this technical solution, in this preparation method, the bio-based polyphenol antioxidant is extracted from natural plant resources, including green tea and grape seeds; the siloxane-grafted polymer is prepared by a free radical polymerization method; the carbon quantum dot light stabilizer is prepared by a citric acid pyrolysis method.

[0038] Compared with the prior art, the present invention provides an anti-aging modified asphalt and a preparation method thereof, having the following beneficial effects:

[0039] This anti-aging modified asphalt and its preparation method, by synergistically introducing additives such as a nano-montmorillonite modifier, a phosphate ester type flame retardant and anti-aging agent, a bio-based polyphenol antioxidant, a siloxane-grafted polymer, and a carbon quantum dot light stabilizer on the basis of the traditional modification system, construct a composite system with multiple shielding, free radical scavenging, weather protection, and polymer strengthening functions. The above-mentioned modification system not only significantly improves the high-temperature stability, low-temperature flexibility, and water resistance of the asphalt material at the macroscopic level, but also greatly delays the material aging process, significantly improves the service life, reduces the maintenance frequency, has excellent anti-aging performance, and broad application prospects through the nano-scale barrier effect, long-term antioxidant mechanism, and light stabilization mechanism at the microscopic level. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] To more clearly illustrate the technical solutions of the embodiments of the present invention, the following will briefly introduce the drawings required for the description of the embodiments. Obviously, the drawings in the following description are only some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.

[0041] Figure 1 Schematic diagram of the composition of an anti-aging modified asphalt proposed by the present invention;

[0042] Figure 2 Schematic flow chart of a preparation method of an anti-aging modified asphalt proposed by the present invention. Detailed implementation manners

[0043] To make the above objects, features, and advantages of the present invention more obvious and understandable, the following will make a detailed description of the specific implementation manners of the present invention in conjunction with the drawings of the specification.

[0044] Many specific details are set forth in the following description to facilitate a thorough understanding of the present invention. However, the present invention can also be implemented in other ways different from those described herein. Those skilled in the art can make similar extensions without departing from the connotation of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed below.

[0045] Secondly, the so-called "one embodiment" or "embodiment" herein refers to a specific feature, structure, or characteristic that can be included in at least one implementation manner of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it an independent or selectively exclusive embodiment from other embodiments.

[0046] Embodiment 1:

[0047] Referring to Figure 1 , this is the first embodiment of the present invention. This embodiment provides an anti-aging modified asphalt, which includes the following specific components:

[0048] Base petroleum asphalt, thermoplastic elastomer, anti-stripping agent, ultraviolet absorber, antioxidant, and softening agent.

[0049] The base petroleum asphalt is a heavy fraction residue obtained by atmospheric distillation or vacuum distillation, and is a black or brownish-black high-viscosity semi-solid substance prepared after solvent deasphalting or air oxidation treatment. The base petroleum asphalt serves as the overall matrix material, providing a continuous bonding structure and imparting preliminary bonding force, ductility, and water resistance to the material; at the same time, it provides a basic environment for the dispersion and synergy of subsequent additives.

[0050] The thermoplastic elastomer uses SBS and has a microstructure with coexisting rubber segments and plastic segments, endowing the modified asphalt with a higher elastic recovery rate and fatigue resistance.

[0051] The anti-stripping agent uses organic amines, phosphate esters, or silane coupling agents, which have an amphiphilic molecular structure, improve the hydrophilicity of the asphalt and the aggregate surface, enhance the adhesion between the asphalt and the aggregate, and delay the problems of stripping and falling off caused by water erosion.

[0052] The ultraviolet absorber uses organic compounds such as benzophenones, benzotriazoles, or hydroxyphenylbenzotriazoles to absorb and attenuate harmful ultraviolet radiation in sunlight and prevent the asphalt matrix from aging due to photooxidation.

[0053] The antioxidant is a hindered phenol compound (such as BHT), which captures free radicals during the aging process of asphalt, delays the thermal oxidation reaction, and synergistically acts with the ultraviolet absorber to enhance the overall anti-aging ability.

[0054] The softening agent, namely the plasticizer, is used to adjust the rheological properties of the asphalt.

[0055] In this embodiment, the mass parts of the specific components are as follows:

[0056] The base petroleum asphalt is 80 parts;

[0057] The thermoplastic elastomer is 3 parts;

[0058] The anti-stripping agent is 0.3 part;

[0059] The ultraviolet absorber is 0.5 part;

[0060] The antioxidant is 0.5 part;

[0061] The softening agent is 2 parts.

[0062] The modified asphalt further includes additives, and the additives specifically include:

[0063] Nanometer montmorillonite modifier, phosphate ester type flame retardant and anti-aging agent, bio-based polyphenol antioxidant, siloxane grafted polymer, and carbon quantum dot light stabilizer CQDs.

[0064] In this embodiment, the mass parts of the additives are as follows:

[0065] The nanometer montmorillonite modifier is 1 part;

[0066] The phosphate ester type flame retardant and anti-aging agent is 0.5 part;

[0067] The bio-based polyphenol antioxidant is 1 part;

[0068] The siloxane grafted polymer is 0.8 part;

[0069] The carbon quantum dot light stabilizer is 0.1 part.

[0070] Furthermore, the nano-montmorillonite modifier includes natural montmorillonite and an organic intercalating agent. Montmorillonite powder with a particle size distribution in the range of 50 - 100 nm is selected, and dodecyltrimethylammonium bromide (DTAB) is used as the organic intercalating agent. The intercalation amount of the nano-montmorillonite is 0.5 - 2.0 mmol / g.

[0071] The nano-montmorillonite modifier can form a two-dimensional barrier with staggered arrangement inside the asphalt matrix, significantly enhancing the barrier property of asphalt to small molecules such as water molecules and oxygen, reducing the oxidation reaction rate, and extending the path for external aging factors to enter the interior of asphalt, thereby effectively delaying the thermal-oxidative aging and ultraviolet aging of asphalt. In addition, nano-montmorillonite itself has excellent thermal stability and mechanical strengthening ability, which can improve the high-temperature stability and anti-cracking performance of asphalt. Compared with conventional inorganic fillers (such as talcum powder and carbon black), nano-montmorillonite has a unique two-dimensional layered structure.

[0072] Furthermore, the phosphate ester type flame retardant and anti-aging agent is an esterification product formed by using pentaerythritol, phosphoric acid, and fatty alcohol as reaction monomers; the molecular structure of the phosphate ester type flame retardant and anti-aging agent contains a P - O - C bond. This additive has low volatility, a stable molecular structure, can withstand high-temperature environments, and is suitable for application in road asphalt materials under high-temperature working conditions. The esterification degree is in the range of 85 - 95%, and the carbon chain number of the fatty alcohol is 8 - 18.

[0073] During the asphalt aging process, the phosphate ester type anti-aging agent blocks the molecular chain breakage process by capturing free radicals. At the same time, in a high-temperature environment, this additive can generate a phosphate-based protective film that covers the surface of the asphalt, inhibiting the direct erosion of oxygen and ultraviolet light, thereby significantly delaying the aging process. In addition, the phosphate film has flame retardant properties, which can improve the overall fire resistance of the asphalt material. Compared with the traditional use of a single antioxidant (such as hindered phenol), the phosphate ester type additive not only provides antioxidant protection but also has a dual function of flame retardancy.

[0074] Furthermore, the bio-based polyphenol antioxidant adopts a microcapsule particle structure, the coating shell material is cyclodextrin or gelatin shell material, and the internal material is epigallocatechin gallate (EGCG) and proanthocyanidins; the particle size of the microcapsule particles is 1 - 5 μm.

[0075] Natural polyphenol molecules can quickly neutralize free radicals through hydrogen donation reactions, interrupting the oxidation chain reaction of asphalt molecular chains and delaying the deterioration of material properties. The microcapsule technology enables the antioxidant to exist stably during the high-temperature mixing process and achieve slow release during long-term use, continuously playing an antioxidant protection role. Different from conventional petrochemical-based antioxidants, bio-based polyphenols have stronger antioxidant ability (high ORAC value).

[0076] Furthermore, the siloxane-grafted polymer includes a polybutadiene (PB) main chain and a polydimethylsiloxane (PDMS) side chain introduced onto the PB chain through maleic anhydride grafting reaction.

[0077] The grafted siloxane segments endow the asphalt with extremely strong hydrophobic properties and UV resistance, effectively reducing water erosion and UV degradation. At the same time, the polybutadiene main chain provides the asphalt with excellent elastic recovery characteristics, enhancing the low-temperature anti-cracking performance. Overall, a network reinforcement system with aging resistance and fatigue resistance is formed. Compared with traditional thermoplastic elastomers, the siloxane-grafted polymer is superior in weather resistance and high and low temperature resistance.

[0078] Furthermore, in the carbon quantum dot light stabilizer, the particle size of the carbon quantum dots is less than 10 nm, and the surface contains carboxyl (-COOH), hydroxyl (-OH) and amino (-NH2) functional groups, and is surface-modified with chitosan at the same time.

[0079] Carbon quantum dots have excellent light absorption and emission characteristics, can absorb high-energy ultraviolet light and convert it into low-energy heat energy, reducing the damage of asphalt by ultraviolet radiation. In addition, CQDs can capture free radicals generated by ultraviolet irradiation, further inhibiting the chain aging reaction and effectively improving the photo-oxidation resistance of asphalt. Compared with traditional inorganic UV shielding agents, CQDs have better dispersibility and smaller addition amounts.

[0080] An anti-aging modified asphalt provided by the present invention combines basic petroleum asphalt, thermoplastic elastomer, anti-stripping agent, ultraviolet absorber, antioxidant, softening agent, and a variety of innovative functional additives, significantly improving the comprehensive performance of asphalt materials, especially showing excellent technical advantages in high temperature resistance, anti-ultraviolet aging, heat-oxygen aging resistance and low-temperature flexibility. Compared with traditional modified asphalt materials, the product of the present invention can maintain good structural stability and physical properties under long-term high-temperature operation, strong ultraviolet radiation and extreme climate change conditions, greatly extending the service life of roads and reducing the maintenance frequency and maintenance cost.

[0081] Since the present invention uses cutting-edge functional materials such as nano-montmorillonite modifier, bio-based polyphenol antioxidant, phosphate ester type flame retardant and anti-aging agent, siloxane-grafted polymer and carbon quantum dot light stabilizer, these additives not only have excellent stability performance, but also take into account green development requirements such as environmental protection and low VOC emissions, meeting the dual requirements of sustainability and high performance in the current road material field. Therefore, the anti-aging modified asphalt of the present invention is not only applicable to infrastructure construction fields with extremely high durability requirements such as high-grade highways, urban expressways, and large bridge pavements, but also applicable to special application scenarios such as tunnels, heavy-duty airport runways, and roads in extreme climate regions, having broad market promotion prospects and industrial application values.

[0082] Example Two:

[0083] Refer to Figure 2 , which is the second embodiment of the present invention. This embodiment provides a preparation method of anti-aging modified asphalt, which is prepared based on the modified asphalt described in Example One, and includes the following specific steps:

[0084] S1. Pretreatment of base petroleum asphalt and preliminary compounding with thermoplastic elastomer;

[0085] Heat the base petroleum asphalt to 150 - 160 °C for melting treatment, continuously stir and slightly evacuate to remove volatile components, forming a uniformly flowing molten asphalt. Subsequently, slowly add the thermoplastic elastomer, raise the temperature to 160 - 180 °C, and increase the stirring rate to 500 - 700 rpm, and continue stirring for 30 - 60 minutes to form a uniformly compounded thermoplastic network structure.

[0086] By melting the base petroleum asphalt, volatile impurities are removed, the initial fluidity of the material is improved, and a thermoplastic elastomer is introduced to form a physical crosslinking network. This network not only improves the elasticity and deformation recovery ability of the asphalt, but also provides a physical support framework for the uniform dispersion of subsequent functional materials.

[0087] S2. Compound addition of anti-stripping agent, ultraviolet absorber and antioxidant;

[0088] In the system obtained in step S1, sequentially add the anti-stripping agent, ultraviolet absorber and antioxidant, maintain the temperature at 160 - 170 °C, and keep the stirring rate at 400 - 600 rpm. After each component is added one by one, continuously stir for 30 - 40 minutes to make the functional additives fully dispersed in the matrix, forming a uniformly stable functional composite system.

[0089] In the base asphalt enhanced by thermoplastic elastomer, compoundly introduce an anti-stripping agent, an ultraviolet absorber and an antioxidant. The anti-stripping agent improves the adhesion of aggregates, the ultraviolet absorber inhibits photoaging, and the antioxidant delays thermo-oxidative aging, thereby comprehensively enhancing the environmental stability and structural durability of the asphalt system.

[0090] S3. Add softening agent to improve fluidity and low-temperature performance;

[0091] Slowly drip the softening agent into the asphalt system obtained in step S2, maintain the temperature at 160 - 170 °C, the stirring rate at 300 - 500 rpm, and continuously stir for 20 - 30 minutes to make the softening agent fully penetrate and interact with the asphalt polymer segments, improving the overall fluidity and toughness.

[0092] A softening agent is introduced to reduce the internal friction of the system, improve the flexibility of the asphalt and its construction performance at low temperatures. Meanwhile, it provides a better matrix environment for the subsequent introduction of highly dispersed nanomaterials to ensure the subsequent dispersion effect.

[0093] S4. Compound nanometer montmorillonite modifier and phosphate ester type flame retardant and anti-aging agent are added;

[0094] In the product of step S3, the nanometer montmorillonite modifier is first added after ultrasonic dispersion, and then the phosphate ester type flame retardant and anti-aging agent is added. The temperature is maintained at 160 - 170 °C, and it is dispersed by a high-shear mixer (rotation speed 3000 - 5000 rpm) for 30 - 60 minutes to ensure that each component is fully exfoliated, dispersed and combined with the matrix.

[0095] By introducing the nanometer montmorillonite modifier, a nanobarrier is formed to enhance the gas barrier property and thermal stability of the asphalt. Meanwhile, the phosphate ester type flame retardant and anti-aging agent is introduced to endow the material with excellent flame retardant performance and high-temperature anti-aging ability, synergistically enhancing the comprehensive durability of the asphalt system.

[0096] S5. Bio-based polyphenol antioxidant and siloxane grafted polymer are added;

[0097] In the system obtained in step S4, the bio-based polyphenol antioxidant and siloxane grafted polymer are introduced in sequence. The temperature is maintained at 160 - 170 °C, the stirring rate is 300 - 500 rpm, and ultrasonic dispersion is carried out for 30 minutes to ensure that the bio-polyphenol is evenly distributed and interacts with the siloxane grafted structure to form a stable composite system.

[0098] By compounding and introducing the bio-based polyphenol antioxidant and siloxane grafted polymer, the former has a natural free radical scavenging effect and significantly enhances the antioxidant stability, while the latter forms a hybrid network to improve the water resistance, weather resistance and surface hydrophobicity, synergistically enhancing the comprehensive environmental adaptability of the material.

[0099] S6. Carbon quantum dot light stabilizer is added to complete the preparation of the finished product.

[0100] The carbon quantum dot light stabilizer is slowly added to the mixed system of step S5 after ultrasonic dispersion, and ultrasonic treatment is continued for 30 minutes. The temperature is maintained at 160 - 170 °C, and low-speed stirring is carried out for 5 - 10 minutes to finally obtain a uniform, dense modified asphalt finished product with excellent anti-aging performance.

[0101] After completing the basic strengthening and functional synergy, the carbon quantum dot light stabilizer is finally introduced, which can efficiently absorb ultraviolet rays and scavenge photo-excited free radicals, maximizing the delay of the photo-aging process and enhancing the ultra-long service life of the finished product in the outdoor environment.

[0102] In this embodiment, the preparation methods of each additive are also given:

[0103] The nano-montmorillonite is prepared by organically intercalating and modifying natural montmorillonite. Montmorillonite powder and an organic intercalating agent are stirred and reacted for 6 hours at 80 °C through an ion-exchange reaction to obtain organically modified nano-montmorillonite. Subsequently, ultrasonic dispersion treatment is carried out to obtain a highly exfoliated and uniformly dispersed lamellar structure.

[0104] The phosphate ester type anti-aging agent is prepared by an esterification reaction of pentaerythritol, phosphoric acid and fatty alcohol under the action of a catalyst.

[0105] The bio-based polyphenol antioxidant is extracted from natural plant resources such as green tea and grape seeds, and its main components are epigallocatechin gallate (EGCG) and proanthocyanidins. To improve its thermal stability and dispersibility, microencapsulation technology is used for treatment to form microencapsulated particles.

[0106] The silicone graft polymer is prepared by a free radical polymerization method. The main chain is polybutadiene (PB), and a silicone (PDMS) side chain is introduced onto the PB chain through maleic anhydride grafting reaction. The product has a typical organic-inorganic hybrid structure, in which the inorganic part is the Si-O-Si chain segment, endowing the material with excellent weather resistance and flexibility.

[0107] The carbon quantum dot light stabilizer is prepared by a citric acid pyrolysis method, with particle size less than 10 nm and the surface being rich in carboxyl, hydroxyl and amino functional groups. To improve its dispersibility in asphalt, chitosan is used for surface modification so that it can be well dispersed in a polar environment.

[0108] Example 3:

[0109] To comprehensively evaluate the performance of the anti-aging modified asphalt provided by the present invention, performance tests are carried out on the modified asphalt, and this test is carried out for detection and comparison based on the following items:

[0110] 1. Softening point (°C)

[0111] Test basis: GB / T 4507-2014 standard.

[0112] Test content: The softening temperature of the asphalt under heating conditions is measured by the ring and ball method, reflecting the thermal stability of the asphalt material in a high-temperature environment.

[0113] 2. Ductility (5 °C) (cm)

[0114] Test basis: GB / T 4508-2010 standard.

[0115] Test content: The length of the asphalt spline when stretched to break is measured under low-temperature conditions to evaluate the low-temperature flexibility and crack resistance of the material.

[0116] 3. Penetration (25 °C) (0.1 mm)

[0117] Test basis: GB / T 4509-2010 standard.

[0118] Test content: At standard temperature, measure the depth of a standard needle piercing into the asphalt sample under its own weight to reflect the hardness and consistency of the asphalt.

[0119] 4. Mass loss (TFOT) (%)

[0120] Test basis: GB / T 5304-2001 standard.

[0121] Test content: Evaluate the volatile loss and thermal aging characteristics of asphalt at high temperature through the Thin-Film Oven Test (TFOT).

[0122] 5. Thermal stability (180°C, 5h) (%)

[0123] Test basis: ASTM D2872 standard.

[0124] Test content: Measure the mass loss rate of asphalt under continuous high-temperature heating conditions to evaluate its long-term high-temperature stability.

[0125] 6. Adhesion (grade)

[0126] Test basis: ASTM D3625 standard.

[0127] Test content: Evaluate the adhesion performance between asphalt and aggregates, and grade the adhesion and stripping resistance ability.

[0128] The above test results are shown in Table 1.

[0129] Table 1 Test results of modified asphalt performance

[0130]

[0131] The results of this test show that the anti-aging modified asphalt of the present invention has a significant improvement in various performance indicators compared with conventional modified asphalt, and the specific summary is as follows:

[0132] 1. Significantly improved high-temperature performance:

[0133] The softening point is increased to 78°C, which is about 14.7% higher than that of conventional modified asphalt, indicating that the material has better stability at high temperature, can effectively prevent asphalt from softening and flowing, and is suitable for high-temperature climate or heavy traffic environment.

[0134] 2. Greatly enhanced low-temperature flexibility:

[0135] The ductility reaches 55 cm at 5°C, which is 71.9% higher than that of the comparative sample, significantly improving the low-temperature ductility of the material and reducing the risk of winter cracking.

[0136] 3. Excellent aging resistance:

[0137] The mass loss (TFOT) is reduced to 0.38%, and the mass loss rate in the thermal stability test is only 0.42%, indicating that the asphalt of the present invention has excellent durability under high temperature, ultraviolet and oxidation environments, and significantly extends the service life of the material.

[0138] 4. Optimized adhesion performance:

[0139] The adhesion grade reaches Grade 1, which has obvious advantages compared with conventional materials (Grade 3), effectively improving the bonding force between asphalt and aggregates and reducing water damage and spalling phenomena.

[0140] In summary, by introducing innovative additives such as nano-montmorillonite modifier, bio-based polyphenol antioxidant, phosphate ester type flame retardant and anti-aging agent, silicone graft polymer and carbon quantum dot light stabilizer, the anti-aging modified asphalt of the present invention has achieved significant improvements in key properties such as thermal stability, anti-ultraviolet aging, low-temperature flexibility and adhesion. Its comprehensive performance is far superior to existing conventional modified asphalt products, and has broad application prospects and industrialization value.

[0141] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to the preferred embodiments, those of ordinary skill in the art should understand that the technical solutions of the present invention can be modified or equivalently replaced without departing from the spirit and scope of the technical solutions of the present invention, and they should all be covered by the scope of the claims of the present invention.

Claims

1. A modified asphalt for anti-aging, characterized in that, It includes the following specific components: Base petroleum asphalt, thermoplastic elastomer, anti-stripping agent, ultraviolet absorber, antioxidant, and softening agent; The modified asphalt further includes additives, and the additives specifically include: Nanometer montmorillonite modifier, phosphate ester type flame retardant and anti-aging agent, bio-based polyphenol antioxidant, siloxane grafted polymer, and carbon quantum dot light stabilizer.

2. The modified asphalt with anti-aging property according to claim 1, characterized in that, The mass parts of the specific components are as follows: Base petroleum asphalt is 80 - 120 parts; Thermoplastic elastomer is 3 - 6 parts; Anti-stripping agent is 0.3 - 0.8 part; Ultraviolet absorber is 0.5 - 1.5 parts; Antioxidant is 0.5 - 1 part; Softening agent is 2 - 5 parts.

3. An anti-aging modified asphalt according to claim 1, characterized in that, The mass parts of the additives are as follows: Nanometer montmorillonite modifier is 1 - 3 parts; Phosphate ester type flame retardant and anti-aging agent is 0.5 - 1.5 parts; Bio-based polyphenol antioxidant is 1 - 2 parts; Siloxane grafted polymer is 0.8 - 2.5 parts; Carbon quantum dot light stabilizer is 0.1 - 0.5 part.

4. The modified asphalt with anti-aging property according to claim 1, characterized in that, The nanometer montmorillonite modifier includes natural montmorillonite and organic intercalating agent, and montmorillonite powder with a particle size distribution in the range of 50 - 100 nm is selected, and dodecyltrimethylammonium bromide DTAB is used as the organic intercalating agent; Natural montmorillonite and the organic intercalating agent are stirred and reacted for 6 hours at 80 °C through an ion exchange reaction to obtain organically modified nanometer montmorillonite, and then ultrasonic dispersion treatment is carried out to obtain the nanometer montmorillonite modifier with a lamellar structure.

5. The modified asphalt with anti-aging property according to claim 1, characterized in that, The phosphate ester type flame retardant and anti-aging agent is an esterification product formed by using pentaerythritol, phosphoric acid, and fatty alcohol as reaction monomers; The molecular structure of the phosphate ester type flame retardant and anti-aging agent contains P - O - C bonds, the esterification degree is in the range of 85 - 95%, and the carbon chain number of the fatty alcohol is 8 - 18.

6. The modified asphalt with anti-aging property according to claim 1, characterized in that, The bio-based polyphenol antioxidant adopts a microcapsule particle structure, the coating shell material is cyclodextrin or gelatin shell material, and the internal material is epigallocatechin gallate EGCG and procyanidin; the particle size of the microcapsule particles is 1 - 5 μm.

7. The modified asphalt with anti-aging property according to claim 1, wherein, The siloxane grafted polymer includes the main chain of polybutadiene PB, and a siloxane PDMS side chain introduced on the PB chain through maleic anhydride grafting reaction.

8. An anti-aging modified asphalt according to claim 1, characterized in that, In the carbon quantum dot light stabilizer, the particle size of the carbon quantum dots is less than 10 nm, the surface contains carboxyl, hydroxyl, and amino functional groups, and at the same time, chitosan is used for surface modification.

9. A preparation method of an anti-aging modified asphalt, which is prepared based on the modified asphalt according to any one of claims 1-8, characterized in that, It includes the following specific steps: S1. Pretreatment of base petroleum asphalt and preliminary compounding with thermoplastic elastomer; S2. Compound addition of anti-stripping agent, ultraviolet absorber, and antioxidant; S3. Addition of softening agent to improve fluidity and low-temperature performance; S4. Compound addition of nanometer montmorillonite modifier and phosphate ester type flame retardant and anti-aging agent; S5. Addition of bio-based polyphenol antioxidant and siloxane grafted polymer; S6. Addition of carbon quantum dot light stabilizer and completion of the preparation of the finished product.

10. The preparation method of an anti-aging modified asphalt according to claim 9, characterized in that, In this preparation method, the bio-based polyphenol antioxidant is extracted from natural plant resources, including green tea and grape seeds; the siloxane grafted polymer is prepared by a free radical polymerization method; the carbon quantum dot light stabilizer is prepared by a citric acid pyrolysis method.

Citation Information

Patent Citations

  • Anti-aging additive for improving asphalt aging characteristic and preparation method of anti-aging asphalt

    CN103408957A

  • Graphene oxide compounded carbon quantum dot modified asphalt and preparation method thereof

    CN109320983A

  • Modified asphalt and preparation method thereof

    CN114015249A

Cited By

  • Bio-based flame-retardant composition and application thereof in preparation of polylactic acid composite material