High-elastic coated thermofuse adhesive lining cloth and preparation process thereof
Through the double-layer structure design and optimized preparation process, the high elastic-covered hot fuse bonding lining fabric solves the shortcomings of traditional bonding lining fabrics in terms of elasticity, bond strength and breathability, providing high elastic recovery, excellent bonding strength and breathability, and is suitable for a variety of fabric types, especially silk, knitted and outdoor functional fabrics.
Patent Information
- Application Number
- CN202510430391.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-08
- Publication Date
- 2025-08-05
AI Technical Summary
Traditional bonding lining cloth has shortcomings in elasticity, bonding strength, breathability and washing resistance, and it is difficult to meet the application needs of modern clothing, especially functional clothing.
A high-elastic clad hot fuse adhesive lining fabric designed with a double-layer structure, the core layer consists of polyamide, polyester and nanoscale silica particles and ethylene-vinyl acetate, and the shell layer consists of thermoplastic polyurethane elastomer and modification additives. The material composition and process flow are optimized through specific preparation processes including coaxial double-layer spinning, base fabric pretreatment and hot fuse composite.
It achieves high elastic recovery rate (91-95%), excellent bond strength (16.5-21.5N/5cm) and excellent breathability (95-135cm3/cm2/s), has good feel and drape, excellent washing resistance (strength retention rate 87-90% after 50 washes), and is suitable for a variety of fabric types.
Smart Images

Figure CN120425470A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of textile technology, in particular to a high-elasticity coated hot-melt type adhesive interlining cloth and a preparation process thereof. Background Art
[0002] Fusible interlining, a crucial accessory in garment manufacturing, is widely used in collars, cuffs, and lapels of various garments to enhance their crispness, shape retention, and comfort. However, with the rapid development of the apparel industry and rising consumer demand for clothing quality, traditional fusible interlining has exposed numerous shortcomings in its application.
[0003] Currently, the most common fusible interlinings on the market are divided into two main categories: hot melt spot coating and hot melt powder coating. Hot melt spot coating interlinings are applied to the base fabric surface in a dotted pattern using hot melt adhesive. While this type offers good breathability, it lacks adhesive strength and is prone to debonding after repeated washing, affecting the appearance and wearability of garments. Hot melt powder coating interlinings use hot melt powder evenly distributed on the base fabric surface. This provides high adhesive strength, but poor breathability and uneven contact with the fabric, which can easily produce an "orange peel effect," affecting the feel and drape of garments.
[0004] Furthermore, with the widespread use of elastic and functional fabrics in clothing, traditional fusible interlinings suffer from insufficient elasticity and poor resilience, making them unable to meet the demands of these new fabrics. This is particularly true for thin, soft fabrics like silk and knitwear, as well as stretch fabrics. Traditional fusible interlinings often exhibit excessive rigidity and insufficient elasticity, easily causing deformation and a stiff feel.
[0005] Some improved adhesive interlinings have also appeared in the existing technology, such as two-component hot-melt powder interlinings, elastic hot-melt adhesive interlinings, etc. However, while these products solve the elasticity problem, they often sacrifice bonding strength or breathability. In addition, the production process is complex and the cost is high, making it difficult to achieve large-scale industrial production.
[0006] Furthermore, traditional fusible interlinings are prone to hot melt adhesive dissolution, discoloration, and decreased bond strength during laundering, impacting the garment's lifespan and appearance. Existing fusible interlinings are particularly poorly resistant to aging and weathering, making them difficult to meet the demands of specialized environments.
[0007] Therefore, there is an urgent need to develop a new type of fusible interlining with high elasticity, high bonding strength, good air permeability and washing resistance to meet the application needs of the modern clothing industry for different types of fabrics and improve the wearing comfort and service life of clothing. Summary of the Invention
[0008] Based on the above purpose, the present invention provides a high elastic coated hot melt type adhesive interlining and its preparation process
[0009] A high-elastic coated hot-melt fusible interlining fabric, wherein the hot-melt fusible lining has a double-layer structure, including a hot-melt core layer and an elastic outer shell layer; wherein the core layer is composed of polyamide, polyester, nano-scale silica particles and ethylene-vinyl acetate, and the outer shell layer is composed of thermoplastic polyurethane elastomer and modified additives.
[0010] Furthermore, the core layer material composition is: 58-70 parts by weight of polyamide (PA6), 25-32 parts by weight of polyester (PET), 1.0-2.5 parts by weight of nano-silica particles, 3.5-7.0 parts by weight of ethylene vinyl acetate (EVA), and optionally 0-1.5 parts by weight of a compatibilizer.
[0011] Furthermore, the outer shell material is composed of: 95.0-98.5 parts by weight of thermoplastic polyurethane elastomer (TPU), 0.5-1.0 parts by weight of alkyl silicone oil modifier, 0.5-0.8 parts by weight of antioxidant, 0-1.0 parts by weight of ultraviolet stabilizer, and optionally 0-2.5 parts by weight of waterproofing agent or 0-2.0 parts by weight of modifier.
[0012] Furthermore, the base fabric is polyester non-woven fabric or polyester / cotton blended non-woven fabric, with a unit area mass of 25-40g / m 2 After the hot melt wire is compounded with the base fabric, the amount of hot melt wire used is 7-15g / m 2 .
[0013] The preparation process of the high-elastic coated hot-melt type adhesive interlining includes the following steps: preparation of core layer material, preparation of outer shell material, coaxial double-layer spinning, base fabric pretreatment, hot-melt and base fabric compounding, and post-processing process.
[0014] Furthermore, the core layer material preparation steps include: mixing the components, vacuum drying at 80°C for 2 hours, using a twin-screw extruder for mixing and extrusion, the extrusion temperature range is 220°C in the feeding section, 230°C in the mixing section, and 240°C in the discharging section, and the extrudate is cooled in a water bath and then pelletized.
[0015] Furthermore, the steps for preparing the outer shell material include: mixing the components evenly, vacuum drying at 60°C for 4 hours to reduce the moisture content to less than 0.03%, using a single-screw extruder for mixing, and the extrusion temperature is 170°C in the feed section, 180°C in the mixing section, and 190°C in the discharge section, and the extrudate is cooled and pelletized.
[0016] Furthermore, the coaxial double-layer spinning step includes: loading the core layer material and the shell layer material into the two barrels of the coaxial spinning machine respectively, the core layer barrel temperature is 235-250°C, and the shell layer barrel temperature is 185-195°C, using a special coaxial spinneret for spinning, the spinning pressure is 3.5MPa for the core layer and 2.8MPa for the shell layer, the pulling speed is 1800m / min, and the cooling system adopts three-stage gradient cooling air cooling.
[0017] Furthermore, the base fabric pretreatment step includes: performing surface activation treatment on the base fabric in a low-pressure plasma device, with a processing power of 200-250W, oxygen as the processing gas, a processing time of 30-40 seconds, and a processing pressure of 20Pa; immersing the treated base fabric in a 0.8% silane coupling agent KH-550 aqueous solution, adjusting the pH value to 4.5, the immersion time for 40 seconds, and controlling the residual rate at 100%; and drying the base fabric with hot air at 80°C for 2 minutes.
[0018] Furthermore, the step of compounding the hot melt wire and the base fabric includes: using an electrostatic flocking device to evenly distribute the cut hot melt wire on the surface of the pretreated base fabric, and the electrostatic flocking voltage is 14-17kV; using a pulse hot pressing process to fix the hot melt wire, the hot pressing temperature is 85-95°C, the pressure is 0.15-0.3MPa, the pulse time is 5-6 seconds on, 2-3 seconds off, and the total hot pressing time is 25-30 seconds; the post-processing process includes immersing the composite lining fabric in a 2% silicone oil emulsion for softening and finishing, the rolling rate is controlled at 70%, the heat setting treatment temperature is 115-130°C, the time is 38-50 seconds, and the tension is controlled at 102% of the original width of the base fabric.
[0019] Beneficial effects of the present invention: The high-elastic coated hot-melt fusible interlining of the present invention achieves excellent elasticity (elastic recovery rate 91-95%), excellent bonding strength (16.5-21.5N / 5cm), and excellent air permeability (95-135cm) through innovative double-layer structure design and optimized preparation process. 3 / cm 2 / s) and remarkable washing resistance (strength retention of 87-90% after 50 washes). This interlining solves the technical problems of traditional products such as insufficient elasticity, reduced bonding strength, poor breathability, and stiff feel. It has good feel and drape (drape coefficient of 72-82%) and is suitable for a variety of types of fabrics, from silk and knitwear to stretch fabrics and outdoor functional fabrics. It also has the comprehensive advantages of strong environmental adaptability, high process feasibility, and environmental sustainability. It provides an ideal interlining solution for modern clothing, especially functional clothing, and has important application value and industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 A schematic diagram of the cross-sectional structure of a sheathed thermal fuse according to an embodiment of the present invention;
[0022] Figure 2 Schematic diagram of the coaxial double-layer spinning process according to an embodiment of the present invention;
[0023] Figure 3 The figure is a schematic diagram of the process flow for preparing the high-elastic coated hot-melt adhesive interlining according to an embodiment of the present invention.
[0024] In the figure: 1. Hot-melt core layer; 2. Elastic outer shell layer. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. It is also noted that, to provide a more detailed description, the following embodiments are best and preferred embodiments, and those skilled in the art may employ alternative methods for implementing certain known technologies. Furthermore, the accompanying drawings are intended only to provide a more detailed description of the embodiments and are not intended to limit the present invention.
[0026] It should be noted that references in the specification to "one embodiment," "an embodiment," "an exemplary embodiment," "some embodiments," etc. indicate that the described embodiments may include specific features, structures, or characteristics, but not every embodiment necessarily includes such specific features, structures, or characteristics. In addition, when specific features, structures, or characteristics are described in conjunction with an embodiment, it is within the knowledge of persons skilled in the relevant art to implement such features, structures, or characteristics in conjunction with other embodiments (whether or not explicitly described).
[0027] In general, terms can be understood, at least in part, from their use in context. For example, depending at least in part on the context, the term "one or more" as used herein can be used to describe any feature, structure, or characteristic in the singular sense, or can be used to describe a combination of features, structures, or characteristics in the plural sense. Additionally, the term "based on" can be understood as not necessarily intended to convey an exclusive set of factors, but can instead, depending at least in part on the context, allow for the presence of other factors that are not necessarily explicitly described.
[0028] See Figure 1
[0029] Implementation method 1: basic implementation plan
[0030] 1. Material Preparation
[0031] 1.1 Thermal fuse core layer (1) material
[0032] Polyamide (PA6): 65 parts by weight
[0033] Polyester (PET): 30 parts by weight
[0034] Nano-sized silica particles (average particle size 20 nm): 1.5 parts by weight
[0035] Ethylene vinyl acetate (EVA, vinyl acetate content 18%): 3.5 parts by weight
[0036] 1.2 Elastic shell layer (2) material
[0037] Thermoplastic polyurethane elastomer (TPU, hardness 85A): 97 parts by weight
[0038] Alkyl silicone oil modifier (molecular weight about 8000): 0.8 parts by weight
[0039] Antioxidant: 0.5 parts by weight
[0040] UV stabilizer: 0.7 parts by weight
[0041] Dispersant: 1.0 parts by weight
[0042] 1.3 Base fabric material
[0043] Polyester / cotton blended non-woven fabric (70 / 30 ratio)
[0044] Mass per unit area: 32g / m 2
[0045] Silane coupling agent (KH-550): 0.8% aqueous solution
[0046] See Figure 3 shown
[0047] 2. Preparation Process
[0048] 2.1 Preparation of core layer materials
[0049] PA6, PET particles and EVA copolymer are mixed according to the proportion, and nano-SiO2 particles are added.
[0050] The mixture was dried under vacuum at 80°C for 2 hours to remove moisture.
[0051] The mixed extrusion was carried out using a twin-screw extruder (screw diameter 45 mm, L / D ratio 32:1).
[0052] Extrusion temperature range settings: feeding section 220℃, mixing section 230℃, discharging section 240℃.
[0053] The extrudate is cooled in a water bath and then pelletized to obtain the core layer material.
[0054] 2.2 Preparation of outer shell material
[0055] Mix TPU chips with silicone oil modifier and other additives evenly.
[0056] Dry under vacuum at 60°C for 4 hours to ensure the moisture content is less than 0.03%.
[0057] The mixing was performed using a single screw extruder (screw diameter 38 mm, L / D ratio 26:1).
[0058] Extrusion temperature settings: feeding section 170℃, mixing section 180℃, discharging section 190℃.
[0059] The extrudate is cooled and pelletized to obtain the shell material.
[0060] See Figure 2
[0061] 2.3 Coaxial double-layer spinning
[0062] The prepared core layer material and shell layer material are respectively loaded into two barrels of a coaxial spinning machine.
[0063] The core layer barrel temperature was set to 240°C, and the shell layer barrel temperature was set to 190°C.
[0064] Spinning was performed using a special coaxial spinneret (spinneret diameter 0.3 mm, outer annular gap 0.08 mm).
[0065] Spinning pressure: core layer 3.5MPa, shell layer 2.8MPa.
[0066] The pulling speed was set to 1800 m / min.
[0067] The cooling system adopts three-stage gradient cooling air cooling, with temperatures of 90℃, 60℃ and 30℃ respectively.
[0068] The formed double-layer hot melt wire is collected by winding and cut into segments with a length of 1.5 mm.
[0069] 2.4 Base fabric pretreatment
[0070] The polyester / cotton blended nonwoven fabric was surface activated in a low-pressure plasma device.
[0071] Plasma power: 200W
[0072] Process gas: oxygen
[0073] Processing time: 30 seconds
[0074] Processing pressure: 20Pa
[0075] The treated base fabric was immersed in a 0.8% silane coupling agent KH-550 aqueous solution (the pH value was adjusted to 4.5).
[0076] The soaking time is 40 seconds and the rolling rate is controlled at 100%.
[0077] The base fabric was dried with hot air at 80°C for 2 minutes.
[0078] 2.5 Thermal fuse and base fabric composite
[0079] The cut hot melt wires were evenly distributed on the surface of the pretreated base fabric using an electrostatic flocking device (voltage 15 kV, electrode distance 15 cm).
[0080] The amount of hot melt wire is controlled at 8-10g / m 2 .
[0081] The pulse hot pressing process is used to fix the thermal fuse:
[0082] Hot pressing temperature: 90℃
[0083] Pressure: 0.2MPa
[0084] Pulse time: 5 seconds on, 2 seconds off
[0085] Total hot pressing time: 25 seconds
[0086] The lining cloth that has completed the preliminary compounding is cooled to room temperature by a cooling roller.
[0087] 2.6 Post-processing process
[0088] The composite interlining was immersed in 2% silicone oil emulsion for softening finishing.
[0089] The margin rate is controlled at 70%.
[0090] Heat setting treatment:
[0091] Temperature: 120℃
[0092] Time: 40 seconds
[0093] Tension: controlled at 102% of the original width of the base fabric
[0094] After cooling by the cooling roller, the product is rolled up to obtain the finished product of high elastic coated hot melt type adhesive interlining. Example 1: Material ratio of high elastic coated hot melt type adhesive interlining suitable for silk fabrics
[0095] Core layer material
[0096] Polyamide (PA6): 70 parts by weight
[0097] Polyester (PET): 25 parts by weight
[0098] Nano-sized silica particles (average particle size 15 nm): 1.0 parts by weight Ethylene vinyl acetate (EVA, vinyl acetate content 20%): 4.0 parts by weight Shell material
[0099] Thermoplastic polyurethane elastomer (TPU, hardness 80A): 98.5 parts by weight
[0100] Alkyl silicone oil modifier (molecular weight about 10,000): 1.0 part by weight
[0101] Antioxidant: 0.5 parts by weight
[0102] Base fabric material
[0103] Pure polyester non-woven fabric
[0104] Mass per unit area: 25g / m 2
[0105] Preparation process parameters Coaxial spinning temperature: core layer 235℃, shell layer 185℃
[0106] Thermal fuse diameter: core layer 15μm, shell layer 3μm
[0107] Electrostatic flocking voltage: 14kV
[0108] Hot melt wire dosage: 7g / m 2
[0109] Pulse hot pressing process: temperature 85°C, pressure 0.15 MPa, time 5 seconds on, 3 seconds off, total time 25 seconds
[0110] Heat setting temperature: 115℃, time 38 seconds
[0111] Performance test results
[0112] Adhesion strength: 16.5N / 5cm
[0113] Adhesive strength retention after 50 washes: 90%
[0114] Peel strength: 9.5N / 5cm
[0115] Breathability: 135cm 3 / cm 2 / s
[0116] Softness (Drape Coefficient): 82%
[0117] Elastic recovery rate: 95%
[0118] Rating of the feel after bonding with silk fabric: Excellent
[0119] Example 2: High-elasticity coated hot-melt fusible interlining suitable for elastic fabrics
[0120] Material ratio
[0121] Core layer material
[0122] Polyamide (PA6): 60 parts by weight
[0123] Polyester (PET): 30 parts by weight
[0124] Nano-sized silica particles (average particle size 25 nm): 2.0 parts by weight
[0125] Ethylene vinyl acetate (EVA, vinyl acetate content 15%): 7.0 parts by weight
[0126] Compatibilizer: 1.0 parts by weight
[0127] Shell material
[0128] Thermoplastic polyurethane elastomer (TPU, hardness 75A): 96.5 parts by weight
[0129] Alkyl silicone oil modifier (molecular weight about 6000): 0.5 parts by weight
[0130] Antioxidant: 0.5 parts by weight
[0131] UV stabilizer: 0.5 parts by weight
[0132] Modifier (polyether type): 2.0 parts by weight
[0133] Base fabric material
[0134] Polyester / cotton blended non-woven fabric (80 / 20 ratio)
[0135] Mass per unit area: 40g / m 2
[0136] Pre-softened
[0137] Preparation process parameters
[0138] Coaxial spinning temperature: core layer 245℃, shell layer 192℃
[0139] Thermal fuse diameter: core layer 22μm, shell layer 5μm
[0140] Base fabric plasma treatment power: 230W, time 35 seconds
[0141] Electrostatic flocking voltage: 16kV
[0142] Hot melt wire dosage: 12g / m 2
[0143] Pulse hot pressing process: temperature 92°C, pressure 0.25MPa, time 6 seconds on, 2 seconds off, total time 28 seconds
[0144] Heat setting temperature: 125℃, time 45 seconds
[0145] Performance test results
[0146] Adhesion strength: 18.8N / 5cm
[0147] Adhesive strength retention after 50 washes: 88%
[0148] Peel strength: 10.2N / 5cm
[0149] Breathability: 105cm 3 / cm 2 / s
[0150] Softness (Drape Coefficient): 76%
[0151] Elastic recovery rate: 93%
[0152] Elongation:>120%
[0153] Elasticity retention after bonding with elastic fabric: 95%
[0154] Example 3: Material ratio of high-elastic coated hot-melt fusible interlining suitable for outdoor functional fabrics
[0155] Core layer material
[0156] Polyamide (PA6): 58 parts by weight
[0157] Polyester (PET): 32 parts by weight
[0158] Nano-sized silica particles (average particle size 30 nm): 2.5 parts by weight
[0159] Ethylene vinyl acetate (EVA, vinyl acetate content 12%): 6.0 parts by weight Compatibilizer: 1.5 parts by weight
[0160] Shell material
[0161] Thermoplastic polyurethane elastomer (TPU, hardness 90A): 95.0 parts by weight
[0162] Alkyl silicone oil modifier (molecular weight about 9000): 0.7 parts by weight
[0163] Antioxidant: 0.8 parts by weight
[0164] UV stabilizer: 1.0 parts by weight
[0165] Waterproofing agent: 2.5 parts by weight
[0166] Base fabric material
[0167] Pure polyester non-woven fabric with special embossing treatment
[0168] Mass per unit area: 38g / m 2
[0169] Preparation process parameters Coaxial spinning temperature: core layer 250℃, shell layer 195℃
[0170] Thermal fuse diameter: core layer 25μm, shell layer 4μm
[0171] Base fabric plasma treatment power: 250W, time 40 seconds
[0172] Additional waterproof finishing (C6 fluorocarbon resin, concentration 3%) is applied to the base fabric after treatment
[0173] Electrostatic flocking voltage: 17kV
[0174] Hot melt wire dosage: 15g / m 2
[0175] Pulse hot pressing process: temperature 95°C, pressure 0.3MPa, time 5 seconds on, 2 seconds off, total time 30 seconds
[0176] Heat setting temperature: 130℃, time 50 seconds
[0177] Performance test results
[0178] Adhesion strength: 21.5N / 5cm
[0179] Adhesive strength retention after 50 washes: 87%
[0180] Peel strength: 12.8N / 5cm
[0181] Breathability: 95cm 3 / cm 2 / s
[0182] Softness (Drape Coefficient): 72%
[0183] Elastic recovery rate: 91%
[0184] Waterproof performance (hydrostatic pressure): >5000mm
[0185] Friction resistance (Martindale method): >20,000 times
[0186] Weather resistance test (strength retention after 300 hours of xenon lamp aging): 90%
[0187] Test method description
[0188] 1. Adhesion strength test
[0189] According to ISO 3758, the fusible interlining was tested with a standard test fabric (cotton cloth, density 150g / m 2 After lamination under specified conditions (temperature 150°C, pressure 0.3 MPa, time 15 seconds), the film was cut into 5cm x 10cm pieces and allowed to stand at room temperature for 24 hours before testing. The maximum force at peeling was measured using an electronic tensile testing machine at a speed of 100 mm / min.
[0190] 2. Washing stability test
[0191] According to ISO 6330, after 50 standard washing cycles (40°C water temperature, standard detergent, 30 minutes / time), the bonding strength was tested and the bonding strength retention rate was calculated.
[0192] 3. Air permeability test
[0193] According to ASTM D737, use an air permeability tester to measure the amount of air passing through per unit time and per unit area under a pressure difference of 100Pa.
[0194] 4. Softness test
[0195] The drape method is used for determination and the test is carried out according to GB / T 18318 standard to calculate the drape coefficient.
[0196] 5. Elastic recovery rate test
[0197] The sample was stretched to 30% deformation, held for 1 minute and then released. The recovered length was measured after 10 minutes to calculate the elastic recovery rate.
[0198] 6. Waterproof performance test
[0199] Measured using a hydrostatic pressure tester according to ISO 811.
[0200] 7. Friction resistance test
[0201] The friction test was performed using a Martindale friction tester in accordance with ISO 12947-2.
[0202] Precautions for industrial production
[0203] Temperature control: The temperature difference between the core layer and the shell layer during coaxial spinning should not exceed 60°C to prevent instability of the interlayer interface.
[0204] Spinning pressure balance: The spinning pressure of the core layer and the shell layer needs to be maintained in an appropriate ratio. It is recommended that the core layer pressure is slightly higher than the shell layer by 0.6-0.8MPa.
[0205] Electrostatic flocking uniformity: To ensure uniform distribution of the thermal fuse, a bidirectional electrostatic field design can be used and the ambient humidity can be controlled within the range of 45-55% RH.
[0206] Pulse hot pressing parameters: In the industrial production process, the on-off time ratio of pulse hot pressing should be appropriately adjusted according to the production line speed to ensure sufficient fixation without damaging the thermal fuse structure.
[0207] Quality monitoring: It is recommended to take samples every 200 meters to test the bonding strength and appearance during continuous production to ensure product stability.
[0208] Storage conditions: The finished product should be stored in an environment with a temperature of 15-25℃ and a relative humidity not exceeding 65%, away from direct sunlight. The recommended shelf life is within 12 months from the date of manufacture.
[0209] The detailed descriptions of the three examples above fully demonstrate the adaptability and superior performance of this highly elastic, coated, hot-melt fusible interlining in various applications, validating the feasibility and advancement of its technical solution. Based on specific application requirements, the material ratio and process parameters can be appropriately adjusted to achieve optimal performance.
[0210] The present invention encompasses any alternatives, modifications, equivalents, and solutions that fall within the spirit and scope of the present invention. To provide a thorough understanding of the present invention, specific details are described in detail below in connection with the preferred embodiments of the present invention, but those skilled in the art will be able to fully understand the present invention without these detailed descriptions. Furthermore, to avoid unnecessary confusion regarding the essence of the present invention, well-known methods, processes, procedures, components, and circuits have not been described in detail.
[0211] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A high elastic coated hot melt type adhesive interlining, characterized in that: The thermal fuse has a double-layer structure, including a hot-melt core layer and an elastic shell layer; wherein the core layer is composed of polyamide, polyester, nano-scale silicon dioxide particles and ethylene-vinyl acetate, and the shell layer is composed of thermoplastic polyurethane elastomer and modified additives.
2. The high elastic coated hot melt type adhesive interlining according to claim 1, characterized in that: The core layer material composition is: 58-70 parts by weight of polyamide (PA6), 25-32 parts by weight of polyester (PET), 1.0-2.5 parts by weight of nano-scale silicon dioxide particles, 3.5-7.0 parts by weight of ethylene vinyl acetate (EVA), and optionally 0-1.5 parts by weight of a compatibilizer.
3. The high elastic coated hot melt type adhesive interlining according to claim 1, characterized in that: The outer shell material is composed of 95.0-98.5 parts by weight of thermoplastic polyurethane elastomer (TPU), 0.5-1.0 parts by weight of alkyl silicone oil modifier, 0.5-0.8 parts by weight of antioxidant, 0-1.0 parts by weight of ultraviolet stabilizer, and optionally 0-2.5 parts by weight of waterproofing agent or 0-2.0 parts by weight of modifier.
4. The high elastic coated hot melt type adhesive interlining according to claim 1, characterized in that: The base fabric is polyester non-woven fabric or polyester / cotton blended non-woven fabric, and the mass per unit area is 25-40g / m 2 After the hot melt is compounded with the base fabric, the amount of hot melt is 7-15g / m 2 .
5. A process for preparing the high elastic coated hot melt type adhesive interlining according to any one of claims 1 to 4, characterized in that: The following steps are involved: Preparation of core layer materials, preparation of shell layer materials, coaxial double-layer spinning, base fabric pretreatment, hot melt yarn and base fabric composite and post-processing process.
6. The preparation process according to claim 5, characterized in that: The core layer material preparation steps include: mixing the components, vacuum drying at 80°C for 2 hours, mixing and extruding using a twin-screw extruder, with the extrusion temperature range being 220°C in the feeding section, 230°C in the mixing section, and 240°C in the discharging section, and the extrudate being cooled in a water bath and then pelletized.
7. The preparation process according to claim 5, characterized in that: The shell layer material preparation steps include: after mixing the various components uniformly, vacuum drying at 60° C. for 4 hours to reduce the moisture content to less than 0.03%, mixing using a single-screw extruder, and extrusion temperatures of 170° C. in the feed section, 180° C. in the mixing section, and 190° C. in the discharge section; and cooling and pelletizing the extrudate.
8. The preparation process according to claim 5, characterized in that: The coaxial double-layer spinning step includes: loading the core layer material and the shell layer material into two barrels of a coaxial spinning machine respectively, the core layer barrel temperature is 235-250°C, the shell layer barrel temperature is 185-195°C, a special coaxial spinneret is used for spinning, the spinning pressure is 3.5MPa for the core layer and 2.8MPa for the shell layer, the pulling speed is 1800m / min, and the cooling system adopts three-stage gradient cooling air cooling.
9. The preparation process according to claim 5, characterized in that: The base fabric pretreatment step comprises: performing surface activation treatment on the base fabric in a low-pressure plasma device, with a treatment power of 200-250W, oxygen as the treatment gas, a treatment time of 30-40 seconds, and a treatment pressure of 20Pa; immersing the treated base fabric in a 0.8% silane coupling agent KH-550 aqueous solution, adjusting the pH value to 4.5, the immersion time for 40 seconds, and controlling the roll-off rate at 100%; and drying the base fabric with hot air at 80°C for 2 minutes.
10. The preparation process according to claim 5, characterized in that: The step of compounding the thermal fuse and the base fabric comprises: using an electrostatic flocking device to evenly distribute the cut thermal fuse on the surface of the pre-treated base fabric, with the electrostatic flocking voltage being 14-17 kV; using a pulse hot pressing process to fix the thermal fuse, with the hot pressing temperature being 85-95° C., the pressure being 0.15-0.3 MPa, the pulse time being 5-6 seconds on and 2-3 seconds off, and the total hot pressing time being 25-30 seconds; and the post-processing process comprising immersing the composite lining fabric in a 2% silicone oil emulsion for softening and finishing, with the rolling rate controlled at 70%, the heat setting treatment temperature being 115-130° C., the time being 38-50 seconds, and the tension being controlled at 102% of the original width of the base fabric.
Citation Information
Cited By
Three-dimensional weaving method and system for lining cloth and computer program product
CN120911220A