Method for extracting lithium from lithium-containing glass
Through the method of mixing glass-sulfate-sulfuric acid calcination and water extraction of lithium, the problems of low lithium extraction efficiency and environmental pollution are solved, and efficient and low-cost lithium extraction is achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202510687782.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-27
- Publication Date
- 2025-08-12
AI Technical Summary
The existing lithium extraction technology is inefficient and has serious environmental pollution, making it difficult to efficiently extract lithium from waste, and the traditional methods are costly and have serious waste of resources.
The glass-sulfate-sulfuric acid mixed roasting and marination process is adopted, combined with the method of water extraction and lithium extraction, lithium is extracted from lithium-containing glass, and the glass structure is destroyed by sulfate. The sulfuric acid is converted into a soluble lithium salt, and subsequently extracted through water extraction.
It realizes efficient separation of lithium and other elements, reduces acid and water consumption, improves lithium extraction rate, is suitable for industrial production, meets environmental protection requirements, and reduces environmental burden.
Smart Images

Figure CN120464875A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium extraction, and in particular to a method for extracting lithium from lithium-containing glass. Background Art
[0002] With the rapid development of high-tech industries, lithium batteries are widely used in various industries. Lithium, a scarce element, is commonly used in the manufacture of high-refractive-index glass and ceramic materials, and as a catalyst. Furthermore, as a key element in modern energy applications, especially in lithium-ion batteries, demand for lithium is increasing.
[0003] Therefore, developing an efficient process for lithium recovery has important practical significance and market potential.
[0004] Traditional lithium extraction technologies, such as chemical extraction from lithium ores or electrochemical extraction from salt lakes, face the dual challenges of low efficiency and environmental damage.
[0005] In this demand context, extracting lithium from waste while reducing costs and optimizing the original process will play an important role in promoting the future of rare earth processing and lithium resource recovery. Summary of the Invention
[0006] In view of the shortcomings of the existing technology, the purpose of the present invention is to provide a method for extracting lithium from lithium-containing glass, which can not only efficiently extract lithium from waste, but also reduce costs and environmental pollution, meet the requirements of green chemistry and sustainable development, and play an important role in promoting the future of rare earth processing and lithium resource recovery.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for extracting lithium from lithium-containing glass, the method comprising the following steps:
[0009] (1) mixing lithium-containing glass powder, sulfate and sulfuric acid, and calcining and aging to obtain an aging powder;
[0010] (2) extracting lithium from the aging powder in step (1) by water to obtain a lithium-rich solution.
[0011] The method for extracting lithium from lithium-containing glass provided by the present invention only requires a process of glass-sulfate-sulfuric acid mixed roasting and aging, and lithium can be subsequently extracted by water leaching, which greatly reduces acid consumption and has high separation efficiency between lithium and other elements. It is suitable for industrial production and has broad application prospects.
[0012] Furthermore, the lithium in the lithium-containing glass powder mainly exists in the form of ions and / or lithium aluminum silicate crystals, while silicon mainly exists in the form of silicon dioxide and / or silicate. A composition of sulfuric acid and sulfate is added during the roasting and aging process, wherein the sulfate can destroy the glass crystal structure during the roasting and aging process, and the sulfuric acid can convert the lithium in the lithium-containing glass powder into a water-soluble lithium salt. The two work together to convert the lithium into a water-soluble form during the roasting and aging process, so that the lithium can be directly extracted by water leaching subsequently; and during the roasting and aging process, the acid will not react with silicon oxide. In the subsequent water leaching process, other elements such as silicon are difficult to dissolve in water, thereby achieving efficient separation of lithium from other elements.
[0013] Preferably, the particle size of the lithium-containing glass powder in step (1) is less than 100 mesh.
[0014] Preferably, the lithium content in the lithium-containing glass powder is 1.5-5.2 wt%.
[0015] Preferably, the lithium in the lithium-containing glass powder exists in the form of ions and / or lithium aluminum silicate crystalline oxide.
[0016] Preferably, the lithium-containing glass powder in step (1) further comprises aluminum, silicon and sodium.
[0017] Preferably, the aluminum content in the lithium-containing glass powder is 2.0-15.0 wt%.
[0018] Preferably, the silicon content in the lithium-containing glass powder is 10-30 wt%.
[0019] Preferably, the sodium content in the lithium-containing glass powder is 2-10 wt%.
[0020] Preferably, the sulfuric acid in step (1) is concentrated sulfuric acid.
[0021] Preferably, the concentration of the sulfuric acid is 60-98 wt%.
[0022] Preferably, the sulfate comprises sodium sulfate and / or potassium sulfate.
[0023] Preferably, the mass ratio of sodium sulfate to potassium sulfate in the sulfate is 0.8 to 1:1, preferably 1:1.
[0024] Preferably, the mass ratio of the sulfate to the lithium-containing glass powder is 0.5-0.7:1.
[0025] Preferably, the molar ratio of the acid in the acid solution in step (1) to the acid theoretically required to form lithium sulfate with respect to the lithium in the lithium-containing glass powder is 1 to 1.2:1.
[0026] Preferably, the calcination and aging temperature in step (1) is 550-650°C.
[0027] Preferably, the holding time of the roasting and aging is 1.5 to 3 hours.
[0028] Preferably, the heating rate of the calcination and aging is 1-10°C / min.
[0029] Preferably, after the roasting and aging, step (1) further comprises: crushing and grinding the roasted and aging material to obtain aging powder.
[0030] Preferably, the grinding obtains a cured powder having a particle size of less than 100 mesh.
[0031] Preferably, the step of water leaching lithium in step (2) comprises: mixing the aged powder and water to form a slurry, heating, stirring, leaching and solid-liquid separation.
[0032] Preferably, the water leaching of lithium in step (2) further comprises: washing the slag phase obtained by solid-liquid separation after the water leaching of lithium.
[0033] Preferably, the washing comprises at least two times.
[0034] Preferably, during the water leaching of lithium in step (2), the solid-to-liquid ratio of the aged powder to water is 0.8 to 1.2:5.
[0035] Preferably, during the water leaching of lithium, the stirring leaching temperature is 60-70°C.
[0036] Preferably, during the water leaching of lithium, the stirring leaching time is 2 to 5 hours.
[0037] Preferably, the method comprises the following steps:
[0038] (1) mixing the lithium-containing glass powder and concentrated sulfuric acid having a concentration of 60 to 98% in a molar ratio of 1 to 1.2:1 between the acid in the acid solution and the lithium in the lithium-containing glass powder to form lithium sulfate, heating the mixture to 550 to 650° C. at a rate of 1 to 10° C. / min and maintaining the temperature for 1.5 to 3 hours for calcination and aging, crushing and grinding the calcined and aging material to obtain an aging powder having a particle size of 100 to 400 mesh;
[0039] (2) mixing water and the matured powder in step (1) to form a slurry at a solid-liquid ratio of 0.8 to 1.2:5, and stirring and leaching at 60 to 70° C. for 2 to 5 hours, followed by solid-liquid separation. The slag phase obtained by the solid-liquid separation is washed with water at least twice, and the liquid phase after washing and the solid-liquid separation is a lithium-rich solution.
[0040] The present invention has no particular limitation on the solid-liquid separation in the above process. Any device and method for solid-liquid separation known to those skilled in the art can be used, and can also be adjusted according to the actual process. For example, it can be filtration, centrifugation or sedimentation separation, or a combination of different methods.
[0041] The present invention has no particular limitation on the grinding in the above process. Any device and method known to those skilled in the art for grinding may be used, and may be adjusted according to the actual process. For example, it may be ball milling, crushing, etc., or a combination of different methods.
[0042] Compared with the prior art, the present invention has at least the following beneficial effects:
[0043] (1) The method for extracting lithium from lithium-containing glass provided by the present invention adopts a technology combining hydrometallurgy and pyrometallurgy, and combines sulfate + sulfuric acid mixed aging and roasting with water leaching of lithium, so as to selectively extract lithium from waste glass. The silicon concentration in the lithium-rich solution obtained by selective lithium extraction is preferably within 0.04 g / L, the aluminum concentration is preferably within 15.6800 g / L, and further preferably within 0.2850 g / L. The sodium concentration in the lithium-rich solution is within 28.65 g / L, thereby reducing the common waste of resources and energy consumption in traditional treatment processes, and improving the economy and efficiency of the overall production while ensuring product quality.
[0044] (2) The method for extracting lithium from lithium-containing glass provided by the present invention realizes the efficient separation of lithium from silicon and aluminum. Under the preferred conditions, the lithium extraction rate is above 90%, which reduces the use of harmful chemicals and waste emissions. In addition, by extracting lithium and other elements from glass sheets, the burden on the environment is reduced, which complies with global environmental protection regulations and green chemistry requirements. By utilizing hydrometallurgical technology, it fills the gaps in the existing technology and can provide a cost-effective, environmentally friendly and technologically advanced lithium extraction method, which is expected to promote the wider industrial application of lithium and rare earth elements and support the sustainable development of the high-tech field. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a schematic flow chart of the method for extracting lithium from lithium-containing glass provided by the present invention. DETAILED DESCRIPTION
[0046] For the convenience of understanding the present invention, the present invention is given below with examples. It should be understood by those skilled in the art that the examples are only for the purpose of helping to understand the present invention and should not be regarded as specific limitations of the present invention.
[0047] As a specific embodiment of the present invention, a method for extracting lithium from lithium-containing glass is provided, the method comprising the following steps:
[0048] (1) mixing lithium-containing glass powder, sulfate and sulfuric acid, and calcining and aging to obtain an aging powder;
[0049] (2) extracting lithium from the aging powder in step (1) by water to obtain a lithium-rich solution.
[0050] The method for extracting lithium from lithium-containing glass provided by the present invention only requires the process of acid addition, roasting and aging, and lithium can be subsequently extracted by water leaching, which greatly reduces acid consumption, and has high separation efficiency between lithium and other elements. It is suitable for industrial production and has broad application prospects.
[0051] Furthermore, the lithium in the lithium-containing glass powder mainly exists in the form of ions and / or lithium aluminum silicate crystals, while silicon mainly exists in the form of silicon dioxide. Acid is added during the roasting and aging process, wherein the acid can convert the lithium in the lithium-containing glass powder into water-soluble lithium salts, so that the lithium can be directly extracted by water leaching. Moreover, during the roasting and aging process, the acid will not react with silicon oxide. In the subsequent water leaching process, other elements such as silicon are difficult to dissolve in water, thereby achieving efficient separation of lithium from other elements.
[0052] In some specific embodiments, the particle size of the lithium-containing glass powder in step (1) is less than 100 mesh.
[0053] The present invention further preferably has a particle size of the lithium-containing glass powder within the above range, which has a better calcination and aging effect.
[0054] It is worth noting that the lithium-containing glass powder provided by the present invention can be obtained by grinding glass sheets into powder using a grinder. The specific grinding process is not limited, as long as the lithium-containing glass powder with the above-mentioned particle size range can be obtained.
[0055] It is worth noting that, in the process of water leaching of lithium according to the present invention, no additional acid is required, and only the acid added in the early roasting and aging can be used, so the acid consumption is low. The pH of the system during water leaching of lithium is higher than that of traditional acid leaching, generally 1.5 to 3, for example, it can be 1.5, 1.6, 1.8, 1.9, 2.0, 2.2, 2.3, 2.5, 2.8 or 3.0, etc.
[0056] In some specific embodiments, the lithium content in the lithium-containing glass powder is 1.5 to 5.2 wt%, for example, it can be 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt% or 5.2 wt%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0057] The study found that the lithium content in lithium-containing glass powder is within the above range. Compared with the lithium content of 0.1% to 3% in lithium-containing ore, the lithium content is relatively high and has a better extractable value.
[0058] In certain specific embodiments, the lithium in the lithium-containing glass powder exists in the form of ions and / or lithium aluminum silicon crystalline oxides.
[0059] In certain specific embodiments, the lithium-containing glass powder in step (1) further includes aluminum, silicon and sodium.
[0060] Specifically, the sodium aluminum silicate in the lithium-containing glass powder of the present invention exists in the form of crystalline or amorphous oxide silicate.
[0061] In some specific embodiments, the aluminum content in the lithium-containing glass powder is 2.0 to 15.0 wt%, for example, it can be 2.0 wt%, 2.5 wt%, 3.4 wt%, 4.2 wt%, 5 wt%, 5.9 wt%, 6.7 wt%, 7.5 wt%, 8.4 wt%, 9.2 wt%, 10 wt%, 11 wt%, 12 wt%, 14 wt% or 15 wt%, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0062] In some specific embodiments, the silicon content in the lithium-containing glass powder is 10 to 30 wt%, for example, it can be 10 wt%, 15 wt%, 20 wt%, 25 wt% or 30 wt%, etc., but is not limited to the listed values. Other values not listed within this range are also applicable.
[0063] In some specific embodiments, the sodium content in the lithium-containing glass powder is 2 to 10 wt%, for example, it can be 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%, etc., but is not limited to the listed values, and other values not listed within this range are also applicable.
[0064] In certain specific embodiments, the sulfuric acid in step (1) is concentrated sulfuric acid.
[0065] The key to activating the lithium-containing material by roasting and aging in the present invention is the use of concentrated sulfuric acid, which has dehydrating, strong oxidizing and strong acidity. When mixed with the solid lithium-containing material, it can convert the lithium in the lithium-containing material into soluble lithium sulfate, thereby providing a basis for subsequent water leaching.
[0066] In some specific embodiments, the concentration of sulfuric acid is 60-98 wt%, for example, it can be 60 wt%, 65 wt%, 69 wt%, 73 wt%, 77 wt%, 82 wt%, 86 wt%, 90 wt%, 94 wt% or 98 wt%, etc., but is not limited to the listed values, and other values not listed within this range are also applicable.
[0067] It is worth noting that the present invention first requires a sulfuric acid concentration of 60% or above to convert lithium into a water-soluble form under high temperature conditions. The specific sulfuric acid concentration above this is determined by the acid requirement determined by the lithium content of the raw material. If the raw material lithium content is low, the acid requirement is small, and a lower concentration of acid is needed to introduce additional water to mix the mixture. Conversely, if the raw material lithium content is high, the acid requirement is large, and the volume ratio of ultra-high concentrated sulfuric acid to minerals meets the mixing requirement. In this case, a higher concentration of concentrated acid is needed to mix the mixture to avoid the use of dilute acid to introduce excessive water, which will cause the mixed materials to stratify, and thus prevent the sulfate ions from effectively contacting the minerals.
[0068] In some embodiments, the sulfate salt comprises sodium sulfate and / or potassium sulfate.
[0069] In some specific embodiments, the mass ratio of sodium sulfate to potassium sulfate in the sulfate is 0.8 to 1:1, for example, it can be 0.8:1, 0.83:1, 0.85:1, 0.87:1, 0.89:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1 or 1:1, but is not limited to the listed values. Other values not listed within this range are also applicable, preferably 1:1.
[0070] The present invention further preferably adds sodium sulfate and potassium sulfate in combination, as the two have a synergistic effect during the roasting and aging process, and can enhance the destructive effect on the crystal structure of the glass phase.
[0071] In some specific embodiments, the mass ratio of the sulfate to the lithium-containing glass powder is 0.5 to 0.7:1, for example, it can be 0.5:1, 0.53:1, 0.55:1, 0.57:1, 0.59:1, 0.62:1, 0.64:1, 0.66:1, 0.68:1 or 0.7:1, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0072] The present invention further preferably sets the mass ratio of sulfate to lithium-containing glass powder within the above range, so that the efficiency of lithium leaching by water after calcination and aging is higher.
[0073] In certain specific embodiments, the molar ratio of the acid in the acid solution in step (1) to the acid theoretically required to form lithium sulfate with the lithium in the lithium-containing glass powder is 1 to 1.2:1, for example, it can be 1.0:1, 1.03:1, 1.05:1, 1.07:1, 1.09:1, 1.12:1, 1.14:1, 1.16:1, 1.18:1 or 1.2:1, etc., but is not limited to the listed values, and other values not listed within this range are also applicable.
[0074] The preferred amount of concentrated sulfuric acid used in the present invention is 1 to 1.2 times the theoretical amount, which can ensure sufficient conversion of lithium while simultaneously avoiding waste of acid solution and can also increase the lithium extraction rate of subsequent water leaching.
[0075] In some specific embodiments, the calcination and aging temperature in step (1) is 550-650°C, for example, it can be 550°C, 562°C, 573°C, 584°C, 595°C, 606°C, 617°C, 628°C, 639°C or 650°C, but is not limited to the listed values. Other values not listed within this range are also applicable.
[0076] In the present invention, the calcination and aging temperature is preferably controlled within the above range, which can further increase the lithium extraction rate and reduce the leaching of impurities.
[0077] In some specific embodiments, the holding time for roasting and aging is 1.5 to 3 hours, for example, it can be 1.5 hours, 1.7 hours, 1.9 hours, 2 hours, 2.2 hours, 2.4 hours, 2.5 hours, 2.7 hours, 2.9 hours or 3 hours, but is not limited to the listed values. Other values not listed within this range are also applicable.
[0078] In some specific embodiments, the heating rate of the roasting and aging is 1 to 10°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values. Other values not listed within this range are also applicable.
[0079] In certain specific embodiments, after the roasting and aging in step (1), the method further comprises: crushing and grinding the roasted and aging material to obtain a aging powder.
[0080] The present invention preferably crushes and grinds the roasted and aged material, which is more conducive to the subsequent water leaching lithium rate.
[0081] It is worth noting that those skilled in the art know that the roasted and aged material should be cooled before crushing and grinding. The present invention has no special requirements for the cooling, and the cooling can be carried out by methods well known to those skilled in the art, such as natural cooling to room temperature.
[0082] In some embodiments, the grinding produces a cured powder having a particle size of less than 100 mesh.
[0083] In certain specific embodiments, the step of water leaching lithium in step (2) comprises: mixing the aged powder and water, heating, stirring, leaching, and solid-liquid separation.
[0084] In certain specific embodiments, the water leaching of lithium in step (2) further comprises: washing the slag phase obtained by solid-liquid separation after the water leaching of lithium.
[0085] Preferably, the washing comprises at least two times.
[0086] In certain specific embodiments, during the water leaching of lithium in step (2), the solid-to-liquid ratio of the aging powder to water is 0.8 to 1.2:5, for example, it can be 0.8:5, 0.85:5, 0.89:5, 0.94:5, 0.98:5, 1.03:5, 1.07:5, 1.12:5, 1.16:5 or 1.2:5, etc., but is not limited to the listed values, and other values not listed within this range are also applicable.
[0087] The present invention preferably controls the solid-to-liquid ratio of water leaching of lithium within the above range, which has a better lithium extraction effect and can reduce water consumption.
[0088] In some specific embodiments, during the water leaching of lithium, the stirring leaching temperature is 60-70°C, for example, it can be 60°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0089] In some specific embodiments, during the water leaching of lithium, the stirring leaching time is 2 to 5 hours, for example, it can be 2 hours, 2.4 hours, 2.7 hours, 3 hours, 3.4 hours, 3.7 hours, 4 hours, 4.4 hours, 4.7 hours or 5 hours, but is not limited to the listed values. Other values not listed within this range are also applicable.
[0090] As a preferred technical solution of the present invention, see Figure 1 , the method comprises the following steps:
[0091] (1) mixing the lithium-containing glass powder and concentrated sulfuric acid having a concentration of 60 to 98 wt % in a molar ratio of 1 to 1.2:1 between the acid in the acid solution and the lithium in the lithium-containing glass powder to form lithium sulfate, heating the mixture to 550 to 650° C. at a rate of 1 to 10° C. / min and maintaining the temperature for 1.5 to 3 hours for calcination and aging, crushing and grinding the calcined and aging material to obtain an aging powder having a particle size of less than 100 mesh;
[0092] (2) mixing water and the matured powder in step (1) to form a slurry at a solid-liquid ratio of 0.8 to 1.2:5, and stirring and leaching at 60 to 70° C. for 2 to 5 hours, followed by solid-liquid separation. The slag phase obtained by the solid-liquid separation is washed with water at least twice, and the liquid phase after washing and the solid-liquid separation is a lithium-rich solution.
[0093] The present invention has no particular limitation on the solid-liquid separation in the above process. Any device and method for solid-liquid separation known to those skilled in the art can be used, and can also be adjusted according to the actual process. For example, it can be filtration, centrifugation or sedimentation separation, or a combination of different methods.
[0094] The present invention has no particular limitation on the grinding in the above process. Any device and method known to those skilled in the art for grinding may be used, and may be adjusted according to the actual process. For example, it may be ball milling, crushing, etc., or a combination of different methods.
[0095] Example 1
[0096] This embodiment provides a method for extracting lithium from lithium-containing glass, the method comprising the following steps:
[0097] (1) The production waste provided by a certain company, the lithium content of the glass flake raw material is 5.0wt%, the aluminum content is 3.5wt%, the silicon content is 28.0wt%, and the sodium content is 8.5wt%. The glass flake is ground into powder using a grinder, and the particle size is less than 100 mesh.
[0098] According to the molar ratio of the acid in the acid solution and the lithium in the lithium-containing glass powder to form the acid theoretically required for lithium sulfate being 1.1:1, the lithium-containing glass powder, industrial concentrated sulfuric acid with a concentration of 98wt%, sodium sulfate and potassium sulfate (the mass ratio of sulfate to lithium-containing glass powder is 0.6:1, and the mass ratio of sodium sulfate to potassium sulfate is 1:1) are mixed, stirred and cooled, and then placed in a muffle furnace and heated to 600°C at 5°C / min for 2h to perform roasting and aging. After the roasted and aging material is cooled, it is crushed and ground to below 100 mesh;
[0099] (2) Mix water and the matured powder at a solid-liquid ratio of 1:5 to form a slurry, and stir and leach at 65°C for 3 hours. Filter with a vacuum filter, and wash the resulting residue with water at a solid-liquid ratio of 1:5 at 65°C for three times, each time for 30 minutes. The washed liquid and the filtered liquid phase are lithium-rich solutions.
[0100] Example 2
[0101] This embodiment provides a method for extracting lithium from lithium-containing glass, the method comprising the following steps:
[0102] (1) The production waste provided by a certain company, the lithium content of the glass sheet raw material is 1.5wt%, the aluminum content is 15wt%, the silicon content is 24wt%, and the sodium content is 2.3wt%. The glass sheet raw material is aluminum-rich and low-lithium raw material. The glass sheet is ground to below 100 mesh using a grinder.
[0103] According to the molar ratio of the acid in the acid solution and the acid theoretically required to form lithium sulfate in the lithium-containing glass powder being 1.2:1, the lithium-containing glass powder, 98wt% industrial concentrated sulfuric acid, sodium sulfate and potassium sulfate (the mass ratio of sulfate to lithium-containing glass powder is 0.7:1, and the mass ratio of sodium sulfate to potassium sulfate is 0.8:1) are mixed, stirred and cooled, and then placed in a muffle furnace and heated to 650°C at 1°C / min for 1.5h to perform roasting and aging. After cooling the roasted and aging material, the material is crushed and ground to below 100 mesh;
[0104] (2) Mix water and the matured powder to form a slurry at a solid-liquid ratio of 2:5, and stir and leach at 70°C for 2 hours. Filter with a vacuum filter, and wash the resulting residue with water at a solid-liquid ratio of 2:5 at 70°C for three times, each time for 25 minutes. The washed liquid and the filtered liquid phase are lithium-rich solutions.
[0105] Example 3
[0106] This embodiment provides a method for extracting lithium from lithium-containing glass, the method comprising the following steps:
[0107] (1) The production waste provided by a certain company, the lithium content of the glass sheet raw material is 2.8wt%, the aluminum content is 3.0wt%, the silicon content is 6.5wt%, and the sodium content is 5.2wt%. The glass sheet is ground to below 100 mesh using a grinder.
[0108] According to the molar ratio of the acid in the acid solution and the lithium in the lithium-containing glass powder to form the acid theoretically required for lithium sulfate being 1.0:1, the lithium-containing glass powder, industrial concentrated sulfuric acid with a concentration of 98wt%, sodium sulfate and potassium sulfate (the mass ratio of sulfate to lithium-containing glass powder is 0.5:1, and the mass ratio of sodium sulfate to potassium sulfate is 0.9:1) are mixed, stirred and cooled, and then placed in a muffle furnace and heated to 550°C at 10°C / min for 3h to perform roasting and aging, and the roasted and aging material is crushed and ground to below 100 mesh;
[0109] (2) Mix water and the matured powder to form a slurry at a solid-liquid ratio of 0.8:5, and stir and leach at 60°C for 5 hours. Filter with a vacuum filter, and wash the resulting residue with water at a solid-liquid ratio of 0.8:5 at 60°C for three times, each time for 35 minutes. The washed liquid and the filtered liquid phase are lithium-rich solutions.
[0110] Example 4
[0111] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that potassium sulfate is not added and the amount of potassium sulfate is replaced by sodium sulfate. The details will not be repeated here.
[0112] Example 5
[0113] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that sodium sulfate is not added and the amount of sodium sulfate is replaced by potassium sulfate, and thus will not be described in detail here.
[0114] Example 6
[0115] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that the mass ratio of sulfate to lithium-containing glass powder is 0.3:1, and thus will not be described in detail here.
[0116] Example 7
[0117] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that the mass ratio of sulfate to lithium-containing glass powder is 0.8:1, and thus will not be described in detail here.
[0118] Example 8
[0119] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that the calcination and aging temperature is 500° C., and thus will not be described in detail here.
[0120] Example 9
[0121] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1 except that the calcination and aging temperature is 700° C., and thus will not be described in detail here.
[0122] Example 10
[0123] This embodiment provides a method for extracting lithium from lithium-containing glass. The method is the same as that of Example 1, except that the 98 wt % concentrated sulfuric acid is replaced by a 55 wt % sulfuric acid solution, and thus will not be described in detail here.
[0124] Comparative Example 1
[0125] This comparative example provides a method for extracting lithium from lithium-containing glass. The method is the same as Example 1 except that concentrated sulfuric acid is replaced by hydrochloric acid with a concentration of 36 wt %. The details will not be repeated here.
[0126] Comparative Example 2
[0127] This comparative example provides a method for extracting lithium from lithium-containing glass. The method is the same as Example 1 except that concentrated sulfuric acid is replaced by a sodium hydroxide solution with a concentration of 48 wt %. The details will not be repeated here.
[0128] Comparative Example 3
[0129] This comparative example provides a method for extracting lithium from lithium-containing glass, which is carried out using Example 2 in CN118326174A.
[0130] Although the lithium in this comparative example has a good leaching rate, the aluminum concentration in the lithium-rich solution of Example 1 is only 0.2850 g / L. This is because aluminum sulfate decomposes into aluminum oxide that is difficult to leach during the aging and roasting process, thereby reducing the leaching concentration of aluminum during selective lithium extraction. The subsequent lithium-rich solution is used for aluminum removal, which can also reduce the lithium loss rate. In addition, Example 1 uses water leaching, and the leaching pH is high. The acid leaching used in Comparative Example 3 has a low pH of the leachate. In the subsequent deep impurity removal process, the pH needs to be adjusted to alkaline, and the alkali consumption is high. That is, the early acid consumption and the late alkali consumption of Example 1 are significantly reduced compared with Comparative Example 3.
[0131] Comparative Example 4
[0132] This comparative example provides a method for extracting lithium from lithium-containing glass. The method is the same as Example 1 except that sodium sulfate and potassium sulfate are not added, and the details are not repeated here.
[0133] Test method: ICP is used to test the lithium in lithium-containing glass powder, lithium-rich solution and slag phase, and the lithium leaching rate of the lithium-rich solution is calculated; at the same time, the concentration of impurities such as silicon, aluminum, and sodium in the lithium-rich solution is tested.
[0134] The test results of the above embodiments and comparative examples are shown in Table 1.
[0135] Table 1
[0136]
[0137] From Table 1 we can see the following points:
[0138] (1) From Example 1 and Example 3, it can be seen that the method for extracting lithium from lithium-containing glass provided by the present invention has the advantages of combining sulfate + sulfuric acid mixed aging and roasting with water leaching of lithium, and can selectively extract lithium from waste glass, wherein the lithium leaching rate in the lithium-rich solution is above 90.11%, and the silicon concentration in the lithium-rich solution is within 0.0391 g / L, the aluminum concentration in the lithium-rich solution is within 0.2850 g / L, and the sodium concentration in the lithium-rich solution is within 21.89 g / L; and from Example 2, it can be seen that even for aluminum-rich and low-lithium glass sheet raw materials, the lithium leaching rate can still reach above 98.52%, and the aluminum concentration after leaching is only 15.6800 g / L. Compared with the aluminum content in the raw material, the leached aluminum concentration is relatively low, which has the effect of selective lithium extraction;
[0139] (2) From the perspective of Example 1 and Examples 4 to 5, it can be seen that in Example 1, a combined sulfate of sodium sulfate and potassium sulfate is used for aging and roasting. Compared with Examples 4 to 5, which respectively use only sodium sulfate and potassium sulfate, the lithium leaching rate of the lithium-rich solution in Example 1 is 93.2%, while Example 4 cannot effectively destroy the glass structure. Although Example 5 can destroy the glass structure, the contact during the reaction process is insufficient due to the high melting point of potassium sulfate, which will lead to a decrease in the lithium leaching rate during the water leaching process. Finally, the lithium leaching rates in the lithium-rich solutions of Examples 4 to 5 are only 2.20% and 88.65%, respectively. This shows that the present invention can significantly improve the lithium extraction rate of water leaching by preferably using a combined salt of potassium sulfate and sodium sulfate in conjunction with sulfuric acid for roasting and aging.
[0140] (3) From Example 1 and Examples 6 to 7, it can be seen that the mass ratio of sulfate to lithium-containing glass powder in Example 1 is 0.6:1. Compared with the mass ratios of sulfate to lithium-containing glass powder in Examples 6 to 7, which are only 0.3:1 and 0.8:1 respectively, the lithium leaching rate of the lithium-rich solution in Example 1 is 93.2%, while the sulfate ratio in Example 6 is reduced. Finally, the lithium leaching rate of the lithium-rich solution in Example 6 is 75.34%. When the amount of sulfate added in Example 7 is too high, the slag sample after roasting is dense and difficult to peel, and the cost of auxiliary materials increases, but it has no obvious effect on improving the leaching rate. This shows that the present invention can significantly improve the lithium extraction rate of water leaching while optimizing the state of the slag sample after roasting by preferably controlling the mass ratio of sulfate to lithium-containing glass powder within a reasonable range.
[0141] Similarly, the calcination temperature will also affect the degree of damage to the glass structure and the density of the slag sample after calcination. It can be seen from Example 1 and Examples 8 to 9 that the present invention preferably controls the calcination and aging temperature within a reasonable range, which can significantly improve the lithium extraction rate of water immersion while optimizing the state of the slag sample after calcination.
[0142] (4) Based on Example 1 and Example 10, it can be seen that the present invention preferably uses concentrated sulfuric acid with a concentration higher than 60 wt % to effectively destroy the glass structure during the roasting and aging process, thereby increasing the lithium leaching rate.
[0143] (3) From Example 1, Comparative Examples 1 to 2, and Comparative Example 4, it can be seen that hydrochloric acid is used in Comparative Example 1, and the hydrochloric acid roasting process is very volatile, and the degree of damage to the glass structure is limited, and it is difficult to leach lithium and aluminum after roasting and aging. Alkali roasting is used in Comparative Example 2, which can cause lithium, aluminum, and silicon to be leached simultaneously, but it is difficult to achieve effective selective lithium leaching, and subsequent filtration is difficult, resulting in large lithium losses. In Comparative Example 4, since sodium sulfate and potassium sulfate are not added, direct sulfuric acid aging and roasting cannot destroy its structure, so lithium, aluminum, and silicon are not leached or the leaching rate is extremely low. This shows that the present invention can significantly improve the lithium extraction rate by adopting a glass-sulfate-sulfuric acid mixed aging and roasting method and then extracting lithium by water leaching.
[0144] The present invention uses the above-described embodiments to illustrate the detailed features of the present invention. However, the present invention is not limited to the above-described detailed features, which does not mean that the present invention must rely on the above-described detailed features to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent replacements for the selected technical features of the present invention, additions to auxiliary technical features, and selections of specific methods, etc., fall within the scope of protection and disclosure of the present invention.
Claims
1. A method for extracting lithium from lithium-containing glass, characterized in that: The method comprises the following steps: (1) mixing lithium-containing glass powder, sulfate and sulfuric acid, and calcining and aging to obtain an aging powder; (2) extracting lithium from the aging powder in step (1) by water to obtain a lithium-rich solution.
2. The method according to claim 1, characterized in that The particle size of the lithium-containing glass powder in step (1) is less than 100 mesh; Preferably, the lithium content in the lithium-containing glass powder is 1.5 to 5.2 wt%; Preferably, the lithium in the lithium-containing glass powder exists in the form of ions and / or lithium aluminum silicon crystalline oxide.
3. The method according to claim 1 or 2, characterized in that The lithium-containing glass powder in step (1) further comprises aluminum, silicon and sodium elements; Preferably, the aluminum content in the lithium-containing glass powder is 2.0 to 15.0 wt%; Preferably, the silicon content in the lithium-containing glass powder is 10 to 30 wt%; Preferably, the sodium content in the lithium-containing glass powder is 2-10 wt%.
4. The method according to any one of claims 1 to 3, characterized in that The sulfuric acid in step (1) is concentrated sulfuric acid; Preferably, the concentration of the sulfuric acid is 60 to 98 wt%; Preferably, the sulfate comprises sodium sulfate and / or potassium sulfate; Preferably, the mass ratio of sodium sulfate to potassium sulfate in the sulfate is 0.8 to 1:1; Preferably, the mass ratio of the sulfate to the lithium-containing glass powder is 0.5-0.7:
1.
5. The method according to any one of claims 1 to 4, characterized in that The molar ratio of the acid in the acid solution in step (1) to the acid theoretically required to form lithium sulfate with respect to the lithium in the lithium-containing glass powder is 1 to 1.2:
1.
6. The method according to any one of claims 1 to 5, characterized in that The calcination temperature in step (1) is 550-650°C; Preferably, the holding time of the roasting and aging is 1.5 to 3 hours; Preferably, the heating rate of the calcination and aging is 1-10°C / min.
7. The method according to any one of claims 1 to 6, characterized in that After the roasting and aging, step (1) further comprises: crushing and grinding the roasted and aging material to obtain a aging powder; Preferably, the grinding obtains a cured powder having a particle size of less than 100 mesh.
8. The method according to any one of claims 1 to 7, characterized in that The step of water leaching lithium in step (2) comprises: mixing the aged powder and water to form a slurry, heating the mixture, stirring and leaching, and solid-liquid separation; Preferably, the water leaching of lithium in step (2) further comprises: washing the slag phase obtained by solid-liquid separation after the water leaching of lithium; Preferably, the washing comprises at least two times.
9. The method according to any one of claims 1 to 8, characterized in that During the water leaching of lithium in step (2), the slurry solid-liquid ratio of the aged powder to water is 0.8 to 1.2:5; Preferably, during the water leaching of lithium, the stirring leaching temperature is 60-70°C; Preferably, during the water leaching of lithium, the stirring leaching time is 2 to 5 hours.
10. The method according to any one of claims 1 to 9, characterized in that The method comprises the following steps: (1) mixing the lithium-containing glass powder and concentrated sulfuric acid having a concentration of 60 to 98 wt % in a molar ratio of 1 to 1.2:1 between the acid in the acid solution and the lithium in the lithium-containing glass powder to form lithium sulfate, heating the mixture to 550 to 650° C. at a rate of 1 to 10° C. / min and maintaining the temperature for 1.5 to 3 hours for calcination and aging, crushing and grinding the calcined and aging material to obtain an aging powder having a particle size of less than 100 mesh; (2) mixing water and the matured powder in step (1) to form a slurry at a solid-liquid ratio of 0.8 to 1.2:5, and stirring and leaching at 60 to 70° C. for 2 to 5 hours, followed by solid-liquid separation. The slag phase obtained by the solid-liquid separation is washed with water at least twice, and the liquid phase after washing and the solid-liquid separation is a lithium-rich solution.