Semi-solid die-casting method and system for ceramic particle premixing reinforced magnesium-based composite material
Through interface optimization and premixing processes, combined with gas stirring, ultrasonic stirring and temperature crushing technology, the problems of uneven mixing of ceramic particles and magnesium-based alloys and weak interface bonding are solved, and the comprehensive performance and preparation efficiency of magnesium-based composite materials are improved.
Patent Information
- Application Number
- CN202510890800.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-30
- Publication Date
- 2025-08-29
- Estimated Expiration
- 2045-06-30
AI Technical Summary
In the prior art, when preparing ceramic particles-enhanced magnesium-based composite materials, the density difference and intrinsic wetting of the nanoceramic particles and the matrix melt result in uneven mixing and weak interface bonding, resulting in poor comprehensive performance of the composite material.
The ceramic particles with an interface optimized interface are premixed with magnesium-based alloy, and the oxide layer or aluminum coating is formed by heating and preoxidation. Combined with a synchronous coupling process of gas stirring and ultrasonic stirring, prefabricated composite particles at high-quality metallurgical bonding interface are prepared, and the temperature crushing technology is used, and the semi-solid die-casting is finally carried out.
It significantly improves the uniformity and interface bonding strength of the composite material, improves the mechanical properties of the material, reduces the risk of energy consumption and oxidation inclusion, and achieves efficient composite material preparation.
Smart Images

Figure CN120555815A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation and application of nonferrous metal composite materials, and more specifically, relates to a semi-solid die-casting method and system for a magnesium-based composite material reinforced by premixing ceramic particles. Background Art
[0002] Compared with traditional forming methods, semi-solid metal forming technology has many unique advantages, such as near-net-shape forming, long mold life, low energy consumption, and heat treatability. It is hailed as one of the most promising metal material processing technologies of the 21st century. Depending on the process method, semi-solid forming technology is divided into two categories: rheoforming and thixoforming. Thixoforming technology is easy to control product quality and has been applied in industry, but this technology requires secondary heating of the semi-solid billet, resulting in a long process flow and high costs. Rheoforming directly processes semi-solid slurry into shape, with a short process flow and low costs. It has great development potential and is currently a hot topic of research.
[0003] The preparation technology of metal semi-solid slurry is the key technology of metal semi-solid rheological forming. The methods for preparing metal semi-solid slurry are mainly divided into stirring method and non-stirring method. The stirring method usually adopts mechanical stirring or electromagnetic stirring to violently stir the melt and break the dendrites to obtain a semi-solid slurry. Although this method can produce a semi-solid slurry, it often produces oxide inclusions, which makes the product prone to defects during the subsequent slurry forming. Non-stirring methods include near-liquidus casting, inclined plate casting, chemical refinement, etc. The semi-solid slurry produced by this method is of low quality and difficult to prepare on a large scale.
[0004] Traditional stirring semi-solid die casting uses screw stirring. The screw is used to shear the heated chip-like and granular alloy materials into a molten slurry containing solid phase components, which is then stored at the front end of the die-casting machine barrel. During the injection process, the entire screw is pushed forward by the cylinder to squeeze the molten metal into the mold for molding.
[0005] When preparing particle-reinforced magnesium-based composites using the traditional stirring semi-solid die-casting process, the reinforcement phase particles and alloy matrix phase particles are fed separately or simultaneously through a hopper and heated to form a semi-solid slurry. However, due to the large density difference between the ceramic reinforcement particles and the magnesium-based alloy, the intrinsic wettability between the two is poor. This results in uneven mixing and weak interfacial interaction when preparing particle-reinforced magnesium-based composites using the traditional stirring semi-solid die-casting process, ultimately leading to poor and unstable mechanical properties of the composite.
[0006] Although some existing technologies have improved the stirring process in the semi-solid slurry preparation process, such as CN101875105A discloses a bubble stirring semi-solid slurry preparation method and device, which adds mechanical vibration to the rotating graphite rod, proposes a process for preparing semi-solid slurry by a combined airflow stirring and mechanical vibration method, and designs and manufactures a set of semi-solid slurry preparation devices for this purpose. However, the mixing intensity generated by the airflow disturbance and the graphite rod mechanical vibration system in the above design scheme is insufficient, and there is a significant disadvantage in terms of material uniformity compared to traditional screw stirring, which is mainly reflected in the low mixing efficiency caused by insufficient shear force. It is also difficult to effectively solve the problem of uneven mixing and weak interface bonding between ceramic reinforcement particles and magnesium alloy in direct co-feed semi-solid die casting during the smelting process of semi-solid metal slurry due to density difference and poor intrinsic wettability. Summary of the Invention
[0007] In view of the defects of the prior art, the purpose of the present invention is to provide a semi-solid die-casting method for magnesium-based composite materials reinforced with ceramic particles based on prefabricated composite particles and interface synergistic reinforcement, aiming to solve the technical problems in the existing semi-solid die-casting preparation process of magnesium-based composite materials, such as uneven mixing and weak interface bonding caused by the density difference and poor intrinsic wettability between nano-ceramic particles and matrix melt, which in turn leads to poor overall performance of the prepared composite materials.
[0008] To achieve the above objectives, in a first aspect, the present invention provides a semi-solid die-casting method for a magnesium-based composite material reinforced with premixed ceramic particles, comprising the following steps: (1) Obtaining ceramic particles with optimized interfaces; the ceramic particles with optimized interfaces are aluminum-coated ceramic particles, or ceramic particles having an oxide layer on the surface; wherein the ceramic particles having an oxide layer on the surface are oxide ceramic particles, or are prepared by the following method: pre-oxidizing non-oxide ceramic particles by heating to form an oxide layer on the surface, thereby obtaining ceramic particles having an oxide layer on the surface; (2) heating the magnesium-based alloy particles and the interface-optimized ceramic particles together to melt the magnesium-based alloy and obtain a mixed melt; introducing an inert gas into the mixed melt and stirring the mixed melt to obtain a uniformly mixed melt; and when the interface-optimized ceramic particles are aluminum-coated ceramic particles, the magnesium-based alloy contains metallic aluminum; (3) cooling the uniformly mixed melt to obtain a solid master alloy, and crushing the solid master alloy to obtain prefabricated composite particles; (4) The prefabricated composite particles are die-casted using a semi-solid die-casting process to obtain a ceramic particle-reinforced magnesium-based composite material.
[0009] Preferably, when preparing ceramic particles having an oxide layer on the surface in step (1), the non-oxide ceramic particles are first heated and pre-oxidized at a temperature above 800° C. to form an oxide layer on the surface.
[0010] Further preferably, the pre-oxidation temperature in step (1) is 800-950° C., and the pre-oxidation time is 1-3 h.
[0011] Preferably, in step (2), the magnesium-based alloy particles and the ceramic particles with optimized interfaces in step (1) are heated together at a temperature of 650-700° C. to melt the magnesium-based alloy and obtain a mixed melt.
[0012] Preferably, the stirring in step (2) is gas stirring and / or ultrasonic stirring.
[0013] Preferably, the cooling rate of step (3) is 1-50°C / s, and the cooling is performed to a temperature of 100-200°C, and then crushing is performed.
[0014] Preferably, the particle size of the prefabricated composite particles in step (3) is 2-20 mm.
[0015] Preferably, the solid phase ratio of the semi-solid slurry prepared in the semi-solid die-casting process of step (4) is controlled at 5-40%.
[0016] According to another aspect of the present invention, there is provided a ceramic particle reinforced magnesium-based composite material obtained by the preparation method.
[0017] According to another aspect of the present invention, there is provided a system for preparing the ceramic particle reinforced magnesium-based composite material, comprising a premixing device and a semi-solid die-casting device; The premixing device is used to achieve heating premixing, cooling and crushing of magnesium-based alloy particles and interface-optimized ceramic particles, and includes a heating premixing unit, a cooling unit and a crushing unit. The heating premixing unit includes a heating furnace, a paddle container placed in the heating furnace, a graphite ultrasonic probe inserted below the liquid level of the paddle container, a temperature sensor and a temperature controller; the graphite ultrasonic probe is hollow and has a through-hole design, and is used to introduce inert gas into the paddle container to perform gas stirring and / or ultrasonic stirring on the melt in the paddle container, thereby obtaining a uniformly mixed melt; the temperature sensor is used to detect the temperature in the heating furnace, and the temperature controller is used to control the temperature of the heating furnace; the cooling unit is connected to the paddle container, and is used to cool the uniformly mixed melt to obtain a solid intermediate alloy; the crushing unit is connected to the cooling unit, and is used to crush the solid intermediate alloy to obtain prefabricated composite particles; The semi-solid die-casting device is used to die-cast the prefabricated composite particles using a semi-solid die-casting process, thereby producing a ceramic particle-reinforced magnesium-based composite material.
[0018] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art: (1) The semi-solid die-casting method for magnesium-based alloy composite materials proposed in the present invention adds a step for preparing prefabricated composite particles before the feed port of the semi-solid hydraulic casting slurry machine. The prefabricated composite particles are obtained by premixing interface-optimized ceramic particles with magnesium-based alloy particles by heating, melting, and cooling and crushing. The interface-optimized ceramic particles are ceramic particles with an oxide layer on the surface or aluminum-coated ceramic particles. The ceramic particles are subjected to interface optimization treatment and further premixed with magnesium-based alloys through a specific premixing process. The two are coordinated to prepare prefabricated composite particles, which solves in advance the technical problems of density difference, poor wettability, and weak interface bonding between magnesium-based alloy particles and reinforcement phase particles in the traditional semi-solid die-casting process, and forms a high-quality metallurgical bonding interface under controllable conditions. The prefabricated composite particles are used as feed for the semi-solid die-casting process, which completely changes the raw material basis of semi-solid die-casting, ensures the uniformity and excellent interface of the final composite material product, and thus significantly improves the mechanical properties of the composite material.
[0019] (2) When the present invention uses ceramic particles with an oxide layer on the surface as ceramic particles for interface optimization, a dense oxide layer that is more easily and effectively wetted by the magnesium-based alloy is first formed on the surface of the ceramic particles through pre-oxidation. The formation of the oxide layer can also prevent excessive reaction between the ceramic particles and the molten magnesium alloy. The present invention reduces the agglomeration phenomenon in the subsequent slurrying process through pre-formed interface bonding, laying a good foundation for obtaining a semi-solid slurry with uniform structure. This improvement not only retains the process advantages of traditional semi-solid die casting, but also improves the comprehensive performance of the composite material by uniformly distributing the reinforcing phase.
[0020] (3) The present invention innovatively adopts a synchronous coupling process of gas stirring and ultrasonic stirring in the preparation process of the intermediate alloy of ceramic particles and magnesium alloy. Compared with the coupling method of gas stirring and mechanical stirring in the prior art, this process has significant advantages: first, the two stirring methods based on different physical mechanisms have better compatibility. The macro flow field generated by gas stirring and the high-frequency micro flow field formed by ultrasonic stirring have less mutual interference, which is conducive to maintaining a stable mixing environment of the melt; second, the two processes have a significant positive synergistic effect - the ultrasonic cavitation effect achieves micro stirring by generating micron-sized bubbles and their collapse process, while the inert gas continuously introduced by gas stirring not only forms macro convection, but also provides sufficient gas source supply for ultrasonic cavitation. The synergistic effect of the two strengthens the bubble growth-collapse dynamics process, and the final mixing effect shows a synergistic enhancement characteristic of 1+1>2, making the components more evenly mixed.
[0021] (4) Compared with the limitations of conventional graphite head mechanical stirring, the present invention adopts a combined stirring method of gas stirring and ultrasonic stirring in the premixing process for preparing the master alloy, which not only improves the mixing efficiency but also avoids the melt contamination problem that may be caused by mechanical stirring, providing a reliable process guarantee for the preparation of high-performance magnesium-based composite materials. The present invention can further reduce the speed of mechanical stirring during semi-solid die casting by premixing in advance, thereby reducing pollution.
[0022] (5) The present invention innovatively adopts an incompletely cooled warm crushing process in the intermediate alloy premix preparation process. When the intermediate alloy is cooled to a suitable temperature with a certain amount of residual heat in the cooling chamber, it can be transferred to the crushing process, instead of having to cool to room temperature before crushing in the traditional process. This warm crushing method fully utilizes the plastic deformation ability of the material at higher temperatures, which not only significantly reduces the crushing energy consumption, but also more effectively controls the size and morphology of the intermediate alloy particles (metals become softer at high temperatures and are more likely to undergo plastic deformation rather than brittle fracture, while at room temperature, metals may be more brittle and easily break into smaller particles. The size of warm crushing will be larger than the size of room temperature crushing. The relative area of large-sized intermediate alloy particles in contact with air is smaller, which can reduce oxidation and avoid particle cracks, etc.). At the same time, the appropriate residual temperature helps to reduce the internal stress generated during the crushing process, avoid defects such as microcracks in the particles, and provide intermediate alloy raw materials with uniform size and stable quality for the subsequent pulping process, thereby improving the efficiency and controllability of the process as a whole.
[0023] (6) The present invention breaks through the traditional semi-solid die-casting process. First, prefabricated composite particles are prepared and then pre-mixed with magnesium-based alloys. The prefabricated composite particles with high-quality metallurgical bonding interfaces formed after pre-mixing are fed as raw materials into a semi-solid die-casting device for semi-solid die-casting production. Compared with the traditional process without pre-mixing, semi-solid die-casting after pre-mixing can shorten the mixing time of the semi-solid slurry and reduce the risk of oxidation inclusions caused by air exposure, and can also further improve the mechanical properties of the composite material finally obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of a device for premixing ceramic particles and magnesium alloy for preparing a raw material for an intermediate alloy according to some embodiments of the present invention; Figure 2 1 is a schematic structural diagram of a semi-solid die-casting machine with an integrated injection part and a slurry making part involved in some embodiments of the present invention; Figure 3 These are the mechanical property test results of the cast magnesium alloy materials prepared in different embodiments and comparative examples of the present invention; Figure 4The flowchart is a semi-solid die-casting method of a magnesium-based composite material reinforced with premixed ceramic particles in some embodiments of the present invention.
[0025] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein: 1-Heating furnace; 2-Paddle container; 3-Graphite ultrasonic probe; 4-Ultrasonic stirring and gas stirring controller; 5-Temperature sensor; 6-Temperature controller; 7-Valve; 8-Cooler; 9-Crushing motor; 10-Crusher; 11-Hydraulic injection unit; 12-Screw rotation unit; 13-Screw; 14-Feeding hopper; 15-Heater; 16-Nozzle. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0027] The present invention provides a method for preparing a magnesium-based composite material reinforced by premixing ceramic particles through semi-solid die casting, comprising the following steps: (1) Obtaining ceramic particles with optimized interfaces; the ceramic particles with optimized interfaces are aluminum-coated ceramic particles, or ceramic particles having an oxide layer on the surface; wherein the ceramic particles having an oxide layer on the surface are oxide ceramic particles, or are prepared by the following method: pre-oxidizing non-oxide ceramic particles by heating to form an oxide layer on the surface, thereby obtaining ceramic particles having an oxide layer on the surface. That is, pre-oxidizing non-oxide ceramic particles by heating to form an oxide layer on the surface, thereby obtaining ceramic particles having an oxide layer on the surface; when the ceramic particles are oxide ceramic particles, their surface already has an oxide layer, and the above-mentioned heating and oxidation step is omitted; (2) Heating the magnesium-based alloy particles and the ceramic particles with optimized surface interfaces in step (1) together to melt the magnesium-based alloy and obtain a mixed melt; introducing an inert gas into the mixed melt and stirring the mixed melt to obtain a uniformly mixed melt; and in order to avoid the introduction of impurity elements, when the ceramic particles with optimized interfaces are aluminum-coated ceramic particles, the magnesium-based alloy contains metallic aluminum; when the ceramic particles with optimized interfaces are ceramic particles with an oxide layer on the surface, this limitation does not apply.
[0028] (3) cooling the uniformly mixed melt to obtain a solid master alloy, and crushing the solid master alloy to obtain prefabricated composite particles; (4) The prefabricated composite particles described in step (3) are die-casted using a semi-solid die-casting process to obtain a ceramic particle-reinforced magnesium-based composite material.
[0029] The ceramic particles used as the reinforcement phase in the present invention can be any of the commonly used ceramic particle types in the prior art. In some embodiments, the ceramic particles are one or more of micron- or nanometer-sized Al2O3 ceramic particles, SiC ceramic particles, B2C ceramic particles, Si3C4 ceramic particles, and TiB2 ceramic particles. The interface-optimized ceramic particles comprise 0.1-40% of the weight of the magnesium-based alloy. The magnesium-based alloy described in the present invention can be any of a variety of magnesium-based alloys, including but not limited to AZ series magnesium alloys and AM series magnesium alloys.
[0030] In some embodiments, when preparing ceramic particles having an oxide layer on the surface in step (1), the non-oxide ceramic particles are first heated at above 900° C. for pre-oxidation to form an oxide layer on the surface.
[0031] In a preferred embodiment, in step (1), the non-oxide ceramic particles are first heated and pre-oxidized at 800°C-950°C to form an oxide layer on their surface. The pre-oxidation time in step (1) is 1-3 hours.
[0032] In step (1), the heating furnace is first raised to 900°C or above, and ceramic particles that need to be heated and pre-oxidized are added, such as SiC ceramic particles, B4C ceramic particles, Si3N4 ceramic particles, etc. (Since Al2O3 ceramic particles are oxides themselves, this step can be omitted). The purpose of pre-oxidation is to form a dense oxide layer on the surface of the ceramic particles. For example, after pre-oxidation, a dense SiO2 layer is formed on the surface of SiC particles and Si3N4 particles, and a dense B2O3 layer is formed on the surface of B4C ceramic particles after pre-oxidation, so as to reduce the excessive reaction between ceramic particles and molten magnesium alloy in the premixing process and the subsequent semi-solid die-casting process. The reaction of ceramic particle pre-oxidation is as follows:
[0033]
[0034]
[0035] Oxides such as SiO2 layers act as diffusion barriers, preventing direct contact between Mg and SiC and inhibiting the formation of harmful phases such as Mg2Si. Furthermore, the surface of untreated SiC is magnesiphobic, making it difficult for liquid magnesium to effectively wet the particles, resulting in interfacial porosity and weak bonding. SiO2, on the other hand, has chemical properties closer to oxide ceramics (such as Al2O3) and exhibits better wettability with magnesium melt than SiC, promoting close adhesion at the interface and reducing porosity. After 1-3 hours of pre-oxidation, the heating furnace is cooled to the melting temperature of the magnesium-based alloy and the magnesium-based alloy is added for melting.
[0036] In other embodiments, the interface-optimized ceramic particles are aluminum-coated ceramic particles. The aluminum-coated ceramic particles can be prepared by molten aluminum impregnation, physical vapor deposition, mechanical ball milling coating or thermal spraying; the aluminum-coated ceramic particles can have an aluminum coating thickness of 0.1-100 μm. The molten aluminum impregnation method is to prepare aluminum-coated ceramic particles, that is, immerse the ceramic particles in molten aluminum liquid and use capillary action or external force to achieve coating. The physical vapor deposition method is to evaporate or sputter aluminum onto the ceramic surface in a vacuum environment. The mechanical ball milling coating method is to press aluminum powder onto the ceramic surface by cold welding during high-energy ball milling. For example, in some embodiments, mechanical ball milling is used to prepare the coating. Ceramic particles and aluminum powder are mixed in a ball mill at a mass ratio of 1.5-2:1 in a jar, with a ball-to-material ratio of 10:1-20:1. The milling is performed at a rotational speed of 200-500 rpm for 2-5 hours. The milling is performed in an inert atmosphere (such as Ar) to prevent oxidation. Aluminum-coated ceramic particles can also be prepared using thermal spraying, where aluminum wire or powder is melted and then sprayed at high speed onto a stream of ceramic particles.
[0037] In a preferred embodiment, the thickness of the aluminum coating on the surface of the aluminum-coated ceramic particles is controlled to be between 0.5 and 50 μm to achieve optimal wetting and interfacial bonding. When the aluminum-coated ceramic particles are premixed with a Mg-Al alloy (such as AZ91), the compatibility of the Al coating with the Al content of the matrix and the formation of a continuous solid solution between the coating and the matrix avoid heterogeneous interfaces, thereby improving the wettability of the ceramic particles and facilitating their diffusion.
[0038] In some embodiments, in step (2), the magnesium-based alloy particles and the ceramic particles with optimized interfaces in step (1) are heated together at a temperature of 650-700°C to melt the magnesium-based alloy and obtain a mixed melt. This ensures the fluidity of the melt during the premixing process while preventing overheating that may lead to severe oxidation of the magnesium, dissolution or reaction of the ceramic, or excessive energy consumption.
[0039] In some embodiments, the stirring in step (2) is gas stirring and / or ultrasonic stirring. More preferably, gas and ultrasonic stirring are used simultaneously.
[0040] In some embodiments, the cooling rate of step (3) is 1-50°C / s, and the cooling is performed to a temperature of 100-200°C, followed by crushing. The particle size of the granular master alloy raw material in step (3) is 2-20 mm.
[0041] When crushing the solid master alloy, the present invention selects an appropriate crusher based on the size of the solid master alloy and the required crushing force. By appropriately setting the crusher parameters, the large alloy material is crushed into uniform small pieces. The crusher motor power can be selected between 15 kW and 110 kW, and the resulting metal granules have a diameter or side length of 2 to 20 mm.
[0042] The present invention first optimizes the interface of ceramic particles, then heats and melts the interface-optimized ceramic particles with a magnesium-based alloy, premixes them, cools them, and then warm-crushes them to obtain granular intermediate alloy raw materials, referred to as prefabricated composite particles. The prefabricated composite particles with high-quality metallurgical bonding interfaces are then used as raw materials for semi-solid die-casting, and die-casting is performed using existing semi-solid die-casting processes and apparatus to produce ceramic particle-reinforced magnesium-based composite materials. In some embodiments, the solid phase fraction of the semi-solid slurry prepared during the semi-solid die-casting process in step (4) is controlled to be 5-40%.
[0043] Because the present invention premixes interface-optimized ceramic particles and magnesium-based alloys to form an intermediate alloy, the two are already well mixed and dispersed during the premixing process. Therefore, the mixing time of the slurry during the semi-solid die-casting process can be appropriately shortened, and a good reinforcing phase dispersion effect can also be achieved. In a preferred embodiment, the stirring time of the semi-solid slurry during the semi-solid die-casting process in step (4) of the present invention is 5-8 minutes.
[0044] The present invention also provides a preparation system for a ceramic particle reinforced magnesium-based composite material, comprising a premixing device and a semi-solid die-casting device; the premixing device is used to achieve heating premixing, cooling and crushing of magnesium-based alloy particles and ceramic particles with optimized interfaces, such as Figure 1 As shown, it includes a heating premixing unit, a cooling unit and a crushing unit, wherein the heating premixing unit includes a heating furnace 1, a paddle container 2 placed in the heating furnace 1, a graphite ultrasonic probe 3 inserted below the liquid level of the paddle container 2, a temperature sensor 5 and a temperature controller 6; the graphite ultrasonic probe 3 is hollow and has a through-hole design, and is used to introduce inert gas into the paddle container 2 to perform gas stirring and / or ultrasonic stirring on the melt in the paddle container 2, thereby obtaining a uniformly mixed melt; the temperature sensor 5 is used to detect the temperature in the heating furnace 1, and the temperature controller 6 is used to control the temperature of the heating furnace 1; the cooling unit is connected to the paddle container 2, and is used to cool the uniformly mixed melt to obtain a solid intermediate alloy; the crushing unit is connected to the cooling unit, and is used to crush the solid intermediate alloy to obtain a granular intermediate alloy raw material, that is, prefabricated composite particles; the semi-solid die-casting device is used to die-cast the prefabricated composite particles using a semi-solid die-casting process, thereby obtaining a ceramic particle-reinforced magnesium-based composite material In some embodiments, such as Figure 2As shown, the semi-solid die-casting device includes a hydraulic injection unit 11, a screw rotation unit 12, a screw 13, a hopper 14, a heater 15 and a nozzle 16; during operation, the prefabricated composite particles prepared by the magnesium-based alloy and ceramic particle premixing device are fed through the hopper 14, and after feeding, the prefabricated composite particles undergo semi-solid melting under the heating action of the heater 15, and at the same time, the screw rotation unit 12 drives the screw 13 to rotate at a set speed (preferably in the range of 100-150 rpm) to stir the molten material to prepare a semi-solid metal slurry; under the action of the hydraulic injection unit 11, the semi-solid metal slurry pushes the entire screw 13 forward to spray the semi-solid metal slurry from the nozzle 16 into the mold for molding.
[0045] The present invention premixes magnesium-based alloy and ceramic particles to obtain prefabricated composite particles with high-quality metallurgical bonding interface, and then the prefabricated composite particles can be semi-solid die-casted using conventional semi-solid die-casting equipment in the prior art. For example, Figure 2 The semi-solid die-casting machine shown has an integrated injection and slurrying section. Other semi-solid die-casting devices may also be used, such as a semi-solid die-casting machine with separate injection and slurrying sections. In some embodiments, when semi-solid die-casting the master alloy particles, a composite stirring process combining mechanical stirring with electromagnetic stirring can be used in the slurrying process. The contactless nature of electromagnetic stirring can reduce the mechanical stirring speed of the screw while ensuring slurry uniformity.
[0046] The traditional semi-solid die-casting process feeds ceramic particles and magnesium-based alloy particles simultaneously from a hopper. Due to the large density difference between the ceramic particles and the molten / semi-solid magnesium alloy, stratification is very easy during the flow process. Furthermore, the ceramic particles and the magnesium alloy have poor intrinsic wettability, making it difficult for the particles to be effectively encapsulated and dispersed by the melt, and they are prone to agglomeration. Furthermore, when the two raw materials are directly mixed and die-casted, during the short residence time in the die-casting machine barrel or injection chamber, there is insufficient shear force or time to overcome the density difference and wettability barriers to achieve uniform mixing. The uneven mixing of ceramic particles and magnesium-based alloy directly leads to large ceramic particle distribution gradients, severe local agglomeration, and weak interfacial bonding in the composite material. This is not just a problem of mixing "uniformity," but also a problem of interface problems and stress concentration sources. Ultimately, key mechanical properties of the resulting composite material, such as strength, toughness, and fatigue performance, are significantly lower than theoretical expectations or cannot be consistently met.
[0047] The present invention discloses a semi-solid die-casting method for preparing ceramic particle-reinforced magnesium-based composite materials, belonging to the technical field of non-ferrous metal composite material processing. This method first obtains ceramic particles with optimized interfaces, then premixes the optimized ceramic particles with magnesium-based alloy particles to produce prefabricated composite particles with a high-quality metallurgical bonding interface. Finally, these premixed composite particles are used as raw materials in a semi-solid die-casting process for die-casting to produce the composite material. During the premixing process, the heating temperature is specifically controlled to ensure the fluidity of the melt while preventing overheating that could lead to severe magnesium oxidation, ceramic dissolution or reaction, or excessive energy consumption. (This temperature control target differs from the temperature control target used in conventional direct die-casting, where temperature control is primarily aimed at forming a semi-solid slurry.) Combined with specific stirring and cooling and crushing processes during the premixing process, these steps work synergistically to produce a metallurgical bonding interface significantly superior to that achieved by conventional direct die-cast composite materials. This solves the problems of poor wettability between the ceramic particles and the magnesium matrix, uneven dispersion, and material contamination encountered in conventional semi-solid die-casting.
[0048] The core innovations of this invention include: 1) adding a premixing step for interface-optimized ceramic particles and magnesium alloy before feeding the pulping machine; 2) producing high-quality metallurgical interface prefabricated composite particles through a synchronous coupling process of gas agitation and ultrasonic agitation, significantly improving the uniformity of the reinforcing phase distribution; and 3) employing a warm crushing technique to crush the intermediate alloy before it is fully cooled, reducing energy consumption and preventing microcracks. Compared to existing technologies, this invention achieves efficient dispersion and interface bonding of ceramic particles through a multi-stage coordinated process, reducing melt oxidation and impurity introduction. This combines a short process flow, low energy consumption, and excellent finished product performance, making it suitable for large-scale production of high-performance magnesium-based composites.
[0049] Unlike existing die-casting processes, where ceramic particles and magnesium alloy particles briefly come into contact in the die-casting machine, forming a weak interface, the molten magnesium alloy in the present invention achieves full contact with the ceramic particles during the premixing stage under optimized wetting conditions (via surface oxidation or Al coating), resulting in favorable interfacial interactions and reactions. This results in a high-quality metallurgical bonding interface between the ceramic particles and the magnesium matrix within the premixed particles after cooling. The die-casting machine is no longer fed with a physical mixture, but rather prefabricated composite particles with a uniform internal structure and well-bonded interfaces. This fundamentally addresses the segregation problems and poor initial wettability caused by the density difference between the ceramic particles and the magnesium alloy. During the semi-solid remelting / stirring process, the prepared prefabricated composite particles eliminate segregation caused by the density difference, resulting in a homogeneous mixed solution after melting. In contrast, the original mixture without premixing undergoes delamination / precipitation after melting due to density mismatch, resulting in a two-phase separated slurry structure and requiring additional energy to break up agglomerates. Therefore, the preparation of prefabricated composite particles in the present invention significantly improves the fluidity of the melt during the semi-solid remelting / stirring process.
[0050] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given. However, the protection scope of the present invention is not limited to the following embodiments. The process parameters in the following embodiments that do not specify specific conditions are generally based on conventional conditions.
[0051] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to form one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed in the present invention.
[0052] The process parameters in the following examples where no specific conditions are specified are generally based on conventional conditions.
[0053] Example 1 Surface-oxidized nano-scale SiC particles (10-200 nm in size) are used as reinforcing particles, and AZ91D is used as the magnesium-based alloy. Figure 1 Magnesium-based alloy and ceramic particle premixing device and Figure 2 The magnesium-based composite material of this embodiment was prepared using a semi-solid die-casting device, wherein the surface-oxidized SiC accounted for 10% of the total mass of the final magnesium-based composite material.
[0054] like Figure 1 As shown, the magnesium-based alloy and ceramic particle premixing device includes a heating premixing unit, a cooling unit and a crushing unit, wherein the heating premixing unit includes a heating furnace 1, a paddle container 2 placed in the heating furnace 1, a graphite ultrasonic probe 3 inserted below the liquid level of the paddle container 2, an ultrasonic stirring and gas stirring controller 4, a temperature sensor 5, a temperature controller 6 and a valve 7; the graphite ultrasonic probe 3 is hollow and has a through-hole design, and is used to introduce inert gas into the paddle container 2 to perform gas stirring and ultrasonic stirring on the liquid in the paddle container 2, and the ultrasonic stirring and gas stirring controller 4 is connected to the graphite ultrasonic probe 3; the temperature sensor 5 (i.e., a thermocouple) is inserted into the furnace from the side of the furnace body for testing the internal temperature of the heating furnace 1, and the temperature controller 6 is used to control the temperature of the heating furnace 1; the heating furnace 1 adopts a resistive heating furnace. The cooling unit is connected to the slurry container 2 via a valve 7. The valve 7 is used to pass the premixed melt in the slurry container 2 into a cooler 8 in the cooling unit. The crushing unit includes a crushing motor 9 and a crusher 10. The crushing motor 9 drives the crusher 10. The solid master alloy cooled in the cooler 8 is crushed by the crushing motor 9 and crusher 10 to obtain the granular master alloy raw material.
[0055] Figure 2 The semi-solid die-casting device shown includes a hydraulic injection unit 11, a screw rotation unit 12, a screw 13, a feeding hopper 14, a heater 15 and a nozzle 16; the granular master alloy raw material, i.e., the prefabricated composite particles, prepared by the magnesium-based alloy and ceramic particle premixing device is fed through the feeding hopper 14, and the granular master alloy raw material is melted under the heating action of the heater 15. At the same time, the screw rotation unit 12 drives the screw 13 to rotate to perform strong stirring to prepare a semi-solid metal slurry; under the action of the hydraulic injection unit 11, the semi-solid metal slurry pushes the entire screw 13 forward to spray the semi-solid metal slurry from the nozzle 16 into the mold for molding.
[0056] The preparation method flow chart is shown in Figure 4 , specifically: Step 1: Place slurry container 2 in the hearth of heating furnace 1 and heat it to a pre-oxidation temperature of 900°C. Add nano-sized SiC particles to the container for pre-oxidation for 2 hours. After pre-oxidation, set the furnace temperature to 680°C, the melting point of AZ91D. Add AZ91D magnesium-based alloy particles to slurry container 2.
[0057] Step 2: High-energy ultrasonic vibration and gas agitation are applied to the molten metal in direct contact within slurry container 2. A graphite ultrasonic probe is lowered 10 mm below the molten metal surface, and ultrasonic vibration is activated while simultaneously introducing high-purity argon gas for 30 minutes of bubble agitation. The ultrasonic frequency is adjusted to 20 kHz, and the ultrasonic vibration volume power is 30 W / cm³ (vibration volume power is the ratio of ultrasonic vibration power to the volume of the vibrated melt) to obtain a premixed melt.
[0058] Step 3: The premixed melt flows into a cooling chamber through a valve and is cooled into a solid master alloy; the temperature of the cooling chamber is adjusted so that the cooling rate of the melt is 1-50°C / s, and cooling is stopped when the alloy cools to 100°C-200°C.
[0059] Step 4: Put the obtained solid master alloy into a crusher to obtain small pieces of master alloy raw materials after crushing; the motor power of the crusher is selected to be 30KW, and the crushing is controlled to obtain granular metal pieces with a diameter or side length of 2-20mm.
[0060] Step 5: Put small pieces of master alloy raw materials, i.e. prefabricated composite particles, into Figure 2The semi-solid die casting machine shown performs semi-solid die casting in the hopper of the slurry machine feed port. Small pieces of granular master alloy raw material, or prefabricated composite particles, prepared by the premixing device are fed through a hopper 14. Heater 15 controls the melt temperature to a target value of 580±10°C, melting the granular master alloy raw material to its solidus-liquidus temperature range. Simultaneously, a screw rotation unit 12 drives screw 13 at a set speed of 120 rpm, applying intense shear stirring to the semi-molten alloy. Stirring is continued for 5.5±0.5 minutes, maintaining a solid fraction of 30%. After the semi-solid metal slurry is prepared, the hydraulic injection unit 11 is activated, applying a set propulsion pressure of 90 MPa ± 5 MPa. This drives the entire screw 13 forward rapidly as a plunger, ejecting the semi-solid metal slurry at high speed through the nozzle 16 and injecting it into the pre-closed die-casting mold cavity. The injection speed is controlled by adjusting the flow rate of the hydraulic system to ensure that the mold cavity is filled in a very short time (<0.5 seconds). A holding pressure of 35 MPa ± 2 MPa is applied for 3-10 seconds to compensate for solidification shrinkage and ensure the density of the casting. The slurry quickly fills the mold and solidifies under pressure, ultimately resulting in a near-net-shape magnesium-based composite die-casting.
[0061] Comparative Example 1 The other aspects are the same as in Example 1, except that ceramic particles are not introduced and the Figure 2 The semi-solid die casting device shown is used to prepare AZ91D material.
[0062] Comparative Example 2 The other aspects are the same as in Example 1, except that ceramic particles are introduced without premixing. Figure 2 The semi-solid die-casting device shown adds ceramic particles SiC particles and AZ91D magnesium-based alloy particles from the feeding hopper 14, and prepares ceramic particle-reinforced magnesium-based composite materials according to the same semi-solid die-casting method as Example 1, and the stirring time of the semi-solid metal slurry is 10±0.5min.
[0063] Comparative Example 3 The other steps are the same as those in Example 1, except that in step 1, the ceramic SiC particles are not pre-oxidized but directly pre-mixed with the magnesium alloy. Step 1 is specifically as follows: Step 1: Place the slurry container 2 in the hearth of the heating furnace 1, add nano-scale SiC particles into the slurry container, set the heating furnace temperature to 680°C, the melting temperature of AZ91D, and add AZ91D magnesium-based alloy metal particles into the slurry container 2.
[0064] Example 2 The other steps are the same as those in Example 1, except that the ceramic particles for interface optimization in this example are aluminum-coated SiC ceramic particles, and the aluminum-coated SiC accounts for 10% of the total mass of the final magnesium-based composite material. The other steps are the same as those in Example 1. Step 1 is specifically as follows: Step 1: Prepare aluminum-coated SiC ceramic particles using ball milling. Nano-SiC particles (10-200 nm) and aluminum powder are mixed in a ball mill at a mass ratio of 1.8:1, resulting in a ball-to-powder ratio of 15:1. Argon is introduced into the mill and dry milled at 400 rpm for 2.5 hours to produce aluminum-coated SiC ceramic particles with a particle size of 0.1-2.5 mm and an aluminum coating thickness of 30-50 μm. Place slurry container 2 in the hearth of heating furnace 1, add the prepared aluminum-coated SiC particles, and then set the furnace temperature to 680°C, the melting point of AZ91D. Add AZ91D magnesium-based alloy metal particles to slurry container 2.
[0065] The mechanical properties of the magnesium alloy materials prepared in Example 1, Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested. The test results are shown in Table 1.
[0066] Table 1 Mechanical properties test results of cast magnesium alloy materials prepared in different embodiments and comparative examples
[0067] As shown in Table 1 and Figure 3 As shown, the mechanical properties of the magnesium alloy material prepared in Comparative Example 2, which introduced ceramic particles as a reinforcement phase, were significantly improved compared to Comparative Example 1, which did not introduce ceramic particles. Comparative Example 3, based on Comparative Example 2, added a premixing step, but it was simply premixing without optimizing the interface of the ceramic particles. Compared to Comparative Example 2, the mechanical properties were improved, but the improvement was small (the tensile strength, yield strength, and elongation increased by 4.7%, 2.9%, and 5.6%, respectively). In Examples 1 and 2, the ceramic particles were first pre-oxidized and aluminum-coated, and then premixed to prepare prefabricated composite particles. These particles were used as feed for a semi-solid die-casting device. The mechanical properties of the composite materials prepared were significantly improved compared to the comparative examples. The tensile strength, yield strength, and elongation of Example 1 increased by 12.5%, 12.2%, and 38%, respectively, compared to Comparative Example 2; the tensile strength, yield strength, and elongation of Example 2 increased by 17.2%, 17.6%, and 52.8%, respectively, compared to Comparative Example 2.
[0068] Comparative Example 4 Other aspects are the same as those of Example 1, except that the graphite ultrasonic probe only turns on ultrasonic vibration, and the vibration frequency, power and time are the same as those of Example 1.
[0069] Comparative Example 5 Other aspects are the same as in Example 1, except that the graphite ultrasonic probe only starts gas stirring, and the stirring time is the same as in Example 1.
[0070] Table 2 Effects of different stirring methods on the mechanical properties of prepared magnesium-based composites
[0071] As can be seen from Table 2 (where "×" indicates that this stirring method was not used, and "√" indicates that the corresponding stirring method was used), the mechanical properties of the composite material obtained by using both ultrasonic stirring and gas stirring during premixing are significantly improved compared to using either stirring method alone. Possible reasons for this are that the macroscopic flow field generated by gas stirring and the high-frequency microflow field formed by ultrasonic stirring have less mutual interference, which is conducive to maintaining a stable mixing environment for the melt; the ultrasonic cavitation effect achieves microscopic stirring by generating micron-sized bubbles and their collapse process, while the continuous inert gas introduced by gas stirring not only forms macroscopic convection but also provides sufficient gas source supply for ultrasonic cavitation, resulting in a significant positive synergistic effect between the two stirring methods. The resulting mixing effect exhibits a synergistic enhancement characteristic of 1+1>2, making the components more evenly mixed, and the resulting composite material mechanical properties also exhibit a synergistic enhancement effect of 1+1>2.
[0072] Example 3 A magnesium-based composite material was prepared using micron-sized Al2O3 ceramic particles as reinforcing particles and AM60 as a magnesium-based alloy, wherein Al2O3 accounted for 12% of the total mass of the final magnesium-based composite material.
[0073] The specific preparation method is: Step 1: Place the slurry container in the furnace of the heating furnace and heat the slurry container to the preset AM60 melting temperature of 680° C. Add metal particles and micron-sized Al2O3 ceramic particles into the slurry container.
[0074] Step 2: Inside the slurry container, a graphite ultrasonic probe is used to apply high-energy ultrasonic vibration and gas agitation to the molten metal, directly contacting the molten metal. The graphite ultrasonic probe is lowered 10mm below the molten metal surface, and ultrasonic vibration is activated while high-purity argon gas is introduced for bubble agitation for 25-30 minutes. The ultrasonic frequency is adjusted to 20kHz, and the ultrasonic vibration volume power is 30W / cm³. The ultrasonic vibration volume power is the ratio of the ultrasonic vibration power to the volume of the vibrated melt.
[0075] Step 3: The mixed metal liquid flows into the cooling chamber through the valve and is cooled into a solid master alloy; the temperature of the cooling chamber is adjusted so that the cooling rate of the melt is 1-50°C / s, and the cooling is stopped when the alloy cools to 100°C-200°C.
[0076] Step 4: Put the obtained solid master alloy into a crusher to obtain small pieces of master alloy raw materials after crushing; the motor power of the crusher is selected to be 30KW, and the crushing is controlled to obtain granular metal pieces with a diameter or side length of 2-20mm.
[0077] Step 5: Add small pieces of master alloy raw materials into Figure 2 The semi-solid die casting machine shown performs semi-solid die casting in the hopper of the slurry machine feed port. Small pieces of granular master alloy raw material, prepared by the premixing device, are fed through a hopper 14. Heater 15 controls the melt temperature to a target value of 580 ± 10°C, melting the granular master alloy raw material to its solidus-liquidus temperature range. Simultaneously, a screw rotation unit 12 drives screw 13 at a set speed of 120 rpm, applying intense shear stirring to the semi-molten alloy. Stirring is continued for 5.5 ± 0.5 minutes, maintaining a solid fraction of 25%. After the semi-solid metal slurry is prepared, the hydraulic injection unit 11 is activated, applying a set propulsion pressure of 90 MPa ± 5 MPa. This drives the entire screw 13 forward rapidly as a plunger, ejecting the semi-solid metal slurry at high speed through the nozzle 16 and injecting it into the pre-closed die-casting mold cavity. The injection speed is controlled by adjusting the flow rate of the hydraulic system to ensure that the mold cavity is filled in a very short time (<0.5 seconds). A holding pressure of 35 MPa ± 2 MPa is applied for 3-10 seconds to compensate for solidification shrinkage and ensure the density of the casting. The slurry quickly fills the mold and solidifies under pressure, ultimately resulting in a near-net-shape magnesium-based composite die-casting.
[0078] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.
Claims
1. A semi-solid die-casting method for magnesium-based composite materials reinforced with premixed ceramic particles, characterized in that: The steps include: (1) Obtaining ceramic particles with optimized interfaces; the ceramic particles with optimized interfaces are aluminum-coated ceramic particles, or ceramic particles having an oxide layer on the surface; wherein the ceramic particles having an oxide layer on the surface are oxide ceramic particles, or are prepared by the following method: pre-oxidizing non-oxide ceramic particles by heating to form an oxide layer on the surface, thereby obtaining ceramic particles having an oxide layer on the surface; (2) heating the magnesium-based alloy particles and the interface-optimized ceramic particles together to melt the magnesium-based alloy and obtain a mixed melt; introducing an inert gas into the mixed melt and stirring the mixed melt to obtain a uniformly mixed melt; and when the interface-optimized ceramic particles are aluminum-coated ceramic particles, the magnesium-based alloy contains metallic aluminum; (3) cooling the uniformly mixed melt to obtain a solid master alloy, and crushing the solid master alloy to obtain prefabricated composite particles; (4) The prefabricated composite particles are die-casted using a semi-solid die-casting process to obtain a ceramic particle-reinforced magnesium-based composite material.
2. The method according to claim 1, wherein The ceramic particles in step (1) are one or more of micron-sized or nano-sized Al2O3 ceramic particles, SiC ceramic particles, B2C ceramic particles, Si3C4 ceramic particles and TiB2 ceramic particles; and / or, In step (2), the ceramic particles with optimized surface interface account for 0.1-40% of the mass of the magnesium-based alloy.
3. The method according to claim 1, wherein In step (1), when preparing ceramic particles having an oxide layer on the surface, the non-oxide ceramic particles are heated and pre-oxidized at a temperature above 800° C. to form an oxide layer on the surface.
4. The method according to claim 1, wherein The pre-oxidation temperature in step (1) is 800-950°C, and the pre-oxidation time is 1-3 h.
5. The method according to claim 1, wherein The aluminum-coated ceramic particles in step (1) are prepared by molten aluminum impregnation, physical vapor deposition, mechanical ball milling coating or thermal spraying; the aluminum-coated ceramic particles have an aluminum coating thickness of 0.1-100 μm.
6. The method according to claim 1, wherein Step (2) heating the magnesium-based alloy particles and the ceramic particles with optimized interfaces in step (1) at a temperature of 650-700° C. to melt the magnesium-based alloy and obtain a mixed molten body.
7. The method according to claim 1, wherein The stirring in step (2) is gas stirring and / or ultrasonic stirring.
8. The method according to claim 1, wherein The cooling rate of step (3) is 1-50°C / s, and the cooling is performed to a temperature of 100-200°C, and then crushing is performed; the particle size of the prefabricated composite particles in step (3) is 2-20 mm.
9. A ceramic particle reinforced magnesium-based composite material, characterized in that: The method is obtained by the method according to any one of claims 1 to 8.
10. A system for preparing a ceramic particle reinforced magnesium-based composite material according to claim 9, characterized in that: Including pre-mixing device and semi-solid die casting device; The premixing device is used to achieve heating premixing, cooling and crushing of magnesium-based alloy particles and interface-optimized ceramic particles, and includes a heating premixing unit, a cooling unit and a crushing unit. The heating premixing unit includes a heating furnace (1), a paddle container (2) placed in the heating furnace (1), a graphite ultrasonic probe (3) inserted below the liquid level of the paddle container (2), a temperature sensor (5) and a temperature controller (6); the graphite ultrasonic probe (3) is hollow and has a through-hole design, and is used to pass inert gas into the paddle container (2) to perform gas stirring and / or ultrasonic stirring on the melt in the paddle container (2), thereby obtaining a uniformly mixed melt; the temperature sensor (5) is used to detect the temperature in the heating furnace (1), and the temperature controller (6) is used to control the temperature of the heating furnace (1); the cooling unit is connected to the paddle container (2) and is used to cool the uniformly mixed melt to obtain a solid intermediate alloy; the crushing unit is connected to the cooling unit and is used to crush the solid intermediate alloy to obtain prefabricated composite particles; The semi-solid die-casting device is used to die-cast the prefabricated composite particles using a semi-solid die-casting process, thereby producing a ceramic particle-reinforced magnesium-based composite material.
Citation Information
Patent Citations
Preparation method of SiC particle reinforced magnesium-based composite material
CN115491568A
Preparation method of nano SiC particle reinforced magnesium-based composite material
CN116254435A
Ultrasonic wave and gas stirring combined dispersion box
CN215877570U
Cited By
Modular semi-solid forming method and system for particle-reinforced magnesium-based composite material
CN121373351A