Preparation method of lamellar hydrotalcite-like material and catalyst and application of lamellar hydrotalcite-like material and catalyst in propane dehydrogenation
By controlling the ratio of trivalent cations and PEG intercalation modification to prepare thin-layered hydrotalcite-like materials, the problems of poor mechanical strength and carbon deposition of hydrotalcite-like materials in propane dehydrogenation catalysts in the existing technology are solved, and high dispersion of Pt/Sn and high propylene selectivity are achieved, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202510729312.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-03
- Publication Date
- 2025-09-09
AI Technical Summary
Existing hydrotalcite-like materials in propane dehydrogenation catalysts have problems such as poor mechanical strength, migration and aggregation of Pt nanoparticles, high carbon deposition rate, and pore blockage. It is difficult to balance structural stability and metal dispersion, and the preparation process is complicated, making it difficult to industrialize.
Thin-layered hydrotalcite-like materials are synthesized through a specific process, the proportion of trivalent cations is controlled, and PEG intercalation modification is used to form an expanded interlayer structure, load Pt and Sn, optimize the interlayer sites, and use specific anions to anchor active metals, expand the interlayer distance, and improve mass transfer efficiency.
A thin layered carrier material with high crystallinity and structural stability is achieved, Pt/Sn is highly dispersed, high-temperature sintering is suppressed, the activity and selectivity of the propane dehydrogenation reaction are improved, and it is easy to industrialize.
Smart Images

Figure BDA0005431442560000051 
Figure BDA0005431442560000052 
Figure BDA0005431442560000061
Abstract
Description
Technical Field
[0001] The invention relates to a thin layer of hydrotalcite-like material, a preparation method of a catalyst and application thereof in propane dehydrogenation, and belongs to the field of propane dehydrogenation catalyst preparation. Background Art
[0002] As an important basic chemical raw material, propylene plays an irreplaceable role in the production of products such as polypropylene, acrylonitrile, and propylene oxide. As global demand for propylene continues to grow, the propane dehydrogenation (PDH) process has become a key technology for increasing propylene production due to its advantages such as abundant raw materials and simple process. Currently, the industry primarily uses two types of catalyst systems: Pt-based and Cr-based. Cr-based catalysts are limited in application due to environmental toxicity concerns. While Pt-based catalysts have excellent environmental performance, they still face key issues such as sintering of active components and deactivation due to carbon deposition.
[0003] Hydrotalcite (HT)-like materials are a kind of materials composed of divalent / trivalent metal cations (such as Mg 2+ 、Al 3+ ) and interlayer anions (such as CO3 2- ) is a layered compound assembled by electrostatic interaction, which has the characteristics of metal atomic-level dispersion, interlayer anion exchangeability, and adjustable structural topology, and is considered to be an ideal catalyst carrier.
[0004] Conventional HT materials, after high-temperature calcination, can form composite metal oxides with high specific surface areas, which can be used to support Pt-based PDH catalysts, demonstrating good propylene selectivity. However, these catalysts still have significant drawbacks: Firstly, the mechanical strength of HT calcined materials is poor, making the particles easily pulverized, leading to migration and aggregation of the supported Pt nanoparticles; secondly, the high rate of carbon deposition during the reaction can easily block the pores and reduce mass transfer efficiency.
[0005] Patent CN110538652A discloses a HT with a multi-level porous structure, which has the characteristics of high specific surface area, stable structure, and thinner layers. Although the conventional intercalation modification method used in this study can increase the interlayer spacing (d003 increased from 0.76nm to 1.2nm), it is difficult to effectively suppress the collapse of the layers at high temperatures.
[0006] Patent CN115228458A discloses a preparation method and application of a ZnMgAl hydrotalcite-based composite oxide catalyst for propane dehydrogenation. The catalyst has the advantages of low cost, simple preparation, and non-toxicity, but its propylene selectivity (about 85%) is still lower than industrial requirements.
[0007] Patent CN115155613A discloses a method for preparing a hydrotalcite-like material and catalyst with a flower-shaped hierarchical pore structure. The material produced by this method features a large specific surface area, a stable structure, and thin lamellae. Due to its complex internal pores, it exhibits high stability and a lamella thickness of approximately 10 nm, resulting in high activity and longevity in propane dehydrogenation processes. However, the preparation process requires precise control of multiple process parameters, making industrialization challenging.
[0008] Existing technologies often prepare HT materials through simple intercalation modification, but this approach often struggles to balance structural stability and metal dispersion. Strategies for regulating the molar ratio X of trivalent cations and employing specific molecular weight polyethylene glycol for co-intercalation are rarely reported. Summary of the Invention
[0009] To address the shortcomings of the prior art, the present invention provides a thin layered hydrotalcite-like material, a catalyst preparation method, and its application in propane dehydrogenation. The material is synthesized through a specific process and has an optimized interlayer structure and metal dispersion properties. The process comprises the following steps:
[0010] (1) adding a certain amount of a first metal salt into a dissolving tank and dissolving it in water, then mixing the first metal salt solution with the second metal salt solution in a certain proportion to prepare a mixed solution, which is recorded as solution A;
[0011] (2) In a water bath, solution A and an alkaline solution containing carbonate and auxiliary anions are simultaneously added to a reactor for co-precipitation, and the hydrolysis conditions are adjusted;
[0012] (3) adding at least one of PEG-200, PEG-400, PEG-600, or PEG-1000 at the initial stage of the precipitation reaction;
[0013] (4) The reactor was crystallized in a water bath. After the crystallization was completed, the material was washed with water until the pH was 7-8 to remove Na + and SO4 2- Finally, a thin layer of hydrotalcite-like material is obtained through slurrying, spray drying, and multi-step calcination (500℃-600℃).
[0014] The metal ion M of the first metal salt in step (1) 2+ Mg 2 +、Zn 2+ 、Ni 2+ 、Cu 2+ 、Co 2+ 、Mn 2+ or Fe 2+ One or more of the metal ions M of the second metal salt 3+ Al 3+ 、Fe3+ or Cr 3+ One or more of , and X=M 3+ / (M 2+ +M 3+ )=0.2-0.34.
[0015] The hydrolysis conditions in step (2) include pH 8-10, temperature 40-60° C., and reaction time 4-8 hours.
[0016] The amount of PEG added in step (3) is 3%-8% of the mass of the hydrotalcite-like precursor, the crystallization temperature is 60-80° C., and the crystallization time is 8-12 hours.
[0017] The anions of the thin layered hydrotalcite-like material in step (4) include H2PO4 - 、ClO3 - 、[Ru(BPS)4]4 - , at least one of terephthalate.
[0018] The invention provides a propane dehydrogenation catalyst, which uses the thin layered hydrotalcite-like material as a carrier and loads 0.1-1wt% of Pt and 0.5-3wt% of Sn, wherein the Pt / Sn exists in a highly dispersed form at interlayer defect sites and has an average particle size of 1-5nm.
[0019] Preferably, the catalyst is used in the propane dehydrogenation reaction at a reaction temperature of 550-650°C and a space velocity of 1000-3000 h -1 When the propane conversion rate is ≥40%, the propylene selectivity is ≥90%.
[0020] The present invention is beneficial in that:
[0021] (1) By precisely controlling the ratio of trivalent cations and PEG intercalation modification, a thin layered carrier material with high crystallinity and structural stability was obtained;
[0022] (2) PEG replaces interlayer water to form an expanded thin layer structure. The unique interlayer structure provides an ideal dispersion site for active metals, facilitates Pt / Sn dispersion, and effectively inhibits sintering at high temperatures.
[0023] (3) On the one hand, specific anions can further anchor Pt / Sn and enhance catalytic activity; on the other hand, large-volume anions (such as terephthalate) can expand the interlayer spacing, which is beneficial to improving mass transfer efficiency;
[0024] (4) The preparation process is simple, and it has the advantages of thin layer structure and metal localization dispersion. It shows excellent activity and selectivity in propane dehydrogenation reaction and is easy to industrialize. DETAILED DESCRIPTION
[0025] The following is a detailed description of the implementation of the present invention. It should be noted that this embodiment is not intended to limit the present invention, and the raw materials in the embodiments and comparative examples are all from the company's tank farm or warehouse.
[0026] The analysis and evaluation are completed by our company's laboratory personnel.
[0027] Example 1:
[0028] Preparation of thin-layered hydrotalcite-like materials
[0029] (1) Add 50g of magnesium nitrate to a dissolving tank, add 300mL of water to dissolve it, and mix it with a solution containing 20g of aluminum nitrate to prepare a mixed solution A. At this time, X = Al 3+ / (Mg 2+ +Al 3+ )=0.25;
[0030] (2) Solution A and an alkaline sodium hydroxide solution containing sodium carbonate and terephthalate were added to a reaction kettle at the same time and in parallel at a water bath temperature of 60°C for co-precipitation. The pH of the reaction system was adjusted to 10, and the reaction time was 6 hours.
[0031] (3) PEG-400 was added at a level of 5% by weight of the hydrotalcite precursor in the later stage of the synthesis;
[0032] (4) The reactor was crystallized in a water bath at 75°C for 10 hours. After the crystallization was completed, the material was washed with water until the pH was 7-8 to remove Na + and SO4 2- Finally, a thin layer of hydrotalcite-like material was obtained through a multi-step process of slurrying, spray drying, and calcination at 550°C.
[0033] Preparation of propane dehydrogenation catalyst
[0034] The prepared thin-layered hydrotalcite-like material was used as a carrier, and 0.5 wt% Pt and 1.5 wt% Sn were loaded by impregnation, so that the Pt / Sn existed in a highly dispersed form at the interlayer defect sites, with an average particle size of 3 nm. This catalyst was designated Cat-1.
[0035] Propane dehydrogenation reaction
[0036] At a reaction temperature of 600°C and a space velocity of 2000 h -1 Under the above conditions, propane dehydrogenation reaction was carried out, with a propane conversion rate of 44.11% and a propylene selectivity of 93.62%.
[0037] Example 2:
[0038] Preparation of thin-layered hydrotalcite-like materials
[0039] (1) Add 40g zinc nitrate and 10g nickel nitrate to a dissolving tank, add 350mL water to dissolve, and mix with a solution containing 25g ferric nitrate to prepare a mixed solution A. At this time, X = Fe 3+ / (Zn 2+ +Ni 2+ +Fe 3+ )=0.3;
[0040] (2) In a water bath at 50°C, solution A and solution containing potassium carbonate, H2PO4 - The potassium hydroxide alkaline solution was simultaneously added to the reactor for co-precipitation, the pH of the reaction system was adjusted to 9, and the reaction time was 8 hours;
[0041] (3) 3% PEG-200 and 2% PEG-600 of the hydrotalcite precursor mass were added in the later stage of the synthesis;
[0042] (4) The reactor was crystallized in a water bath at 80° C. for 9 hours, and the subsequent treatment was the same as in Example 1 to obtain a thin layer of hydrotalcite-like material.
[0043] Preparation of propane dehydrogenation catalyst
[0044] The prepared thin layered hydrotalcite-like material was used as a carrier, and 0.3 wt% Pt and 2 wt% Sn were loaded by impregnation method, with an average Pt / Sn particle size of 2 nm. This catalyst was designated as Cat-2.
[0045] Propane dehydrogenation reaction
[0046] At a reaction temperature of 580°C and a space velocity of 1500 h -1 Under the above conditions, propane dehydrogenation reaction was carried out, with a propane conversion rate of 40.37% and a propylene selectivity of 92.07%.
[0047] Example 3:
[0048] Preparation of thin-layered hydrotalcite-like materials
[0049] (1) Add 30g of copper nitrate and 20g of cobalt nitrate to a dissolving tank, add 400mL of water to dissolve, and mix with a solution containing 18g of chromium nitrate to prepare a mixed solution A. At this time, X = Cr 3+ / (Cu 2+ +Co 2+ +Cr 3+ )=0.28;
[0050] (2) Solution A and an alkaline ammonia solution containing sodium bicarbonate and terephthalate were added to a reactor at a water bath temperature of 60°C for co-precipitation. The pH was adjusted to 10 and the reaction time was 5 hours.
[0051] (3) PEG-1000 was added at 8% by weight of the hydrotalcite precursor in the late stage of synthesis;
[0052] (4) The reactor was crystallized in a water bath at 80° C. for 8 hours, and a thin layer of hydrotalcite-like material was obtained through subsequent treatment.
[0053] Preparation of propane dehydrogenation catalyst
[0054] The prepared thin layered hydrotalcite-like material was used as a carrier, and 0.8 wt% Pt and 2.5 wt% Sn were loaded by impregnation method, with an average Pt / Sn particle size of 4 nm. This catalyst was designated as Cat-3.
[0055] Propane dehydrogenation reaction
[0056] At a reaction temperature of 620°C and a space velocity of 2500 h -1 Under the above conditions, propane dehydrogenation reaction was carried out, with a propane conversion rate of 42.99% and a propylene selectivity of 92.9%.
[0057] Comparative Example 1:
[0058] Preparation of hydrotalcite-like materials
[0059] (1) Add 50g of magnesium nitrate to a dissolving tank, add 300mL of water to dissolve it, and mix it with a solution containing 20g of aluminum nitrate to prepare a mixed solution A. At this time, X = Al 3+ / (Mg 2+ +Al 3+ )=0.25;
[0060] (2) Solution A and an alkaline sodium hydroxide solution containing sodium carbonate were added to the reactor simultaneously and co-precipitated at a water bath temperature of 60°C. The pH of the reaction system was adjusted to 10, and the reaction time was 6 hours.
[0061] (3) PEG was not added in the late stage of synthesis;
[0062] (4) The reactor was crystallized in a water bath at 75°C for 10 hours. After the crystallization was completed, the material was washed with water until the pH was 7-8 to remove Na + and SO4 2- Finally, the hydrotalcite-like material was obtained through a multi-step process of slurrying, spray drying, and calcination at 550°C.
[0063] Preparation of propane dehydrogenation catalyst
[0064] This material was used as a carrier to load 0.5 wt% of Pt and 1.5 wt% of Sn by impregnation. This catalyst was designated DB-1.
[0065] Propane dehydrogenation reaction
[0066] At a reaction temperature of 600°C and a space velocity of 2000 h -1 Under the above conditions, propane dehydrogenation reaction was carried out, with a propane conversion rate of 34.64% and a propylene selectivity of 89.47%.
[0067] Comparative Example 2:
[0068] Preparation of hydrotalcite-like materials
[0069] (1) Add 40g zinc nitrate and 10g nickel nitrate to a dissolving tank, add 350mL water to dissolve, and mix with a solution containing 25g ferric nitrate to prepare a mixed solution A. At this time, X = Fe 3+ / (Zn 2+ +Ni 2+ +Fe 3+ )=0.4;
[0070] (2) Solution A and an alkaline potassium hydroxide solution containing potassium carbonate were added to the reactor simultaneously and co-precipitated at a water bath temperature of 50°C. The pH of the reaction system was adjusted to 9, and the reaction time was 8 hours.
[0071] (3) 3% PEG-200 and 2% PEG-600 of the hydrotalcite precursor mass were added at the initial stage of the precipitation reaction;
[0072] (4) The reactor was crystallized in a water bath at 80°C for 9 hours. After the crystallization was completed, the material was washed with water until the pH was 7-8 to remove Na + and SO4 2- Finally, the hydrotalcite-like material was obtained through a multi-step process of slurrying, spray drying, and calcination at 550°C.
[0073] Preparation of propane dehydrogenation catalyst
[0074] This material was used as a carrier, and 0.3 wt% of Pt and 2 wt% of Sn were loaded by impregnation. This catalyst was designated DB-2.
[0075] Propane dehydrogenation reaction
[0076] At a reaction temperature of 580°C and a space velocity of 1500 h -1 Under the above conditions, propane dehydrogenation reaction was carried out, with a propane conversion rate of 31.85% and a propylene selectivity of 88.33%.
[0077] Catalyst performance evaluation:
[0078] A micro fixed-bed reactor was used for performance evaluation.
[0079] The properties of the propane gas used in the evaluation are as follows:
[0080] Table 1 Basic properties of propane gas used
[0081]
[0082] The evaluation results are as follows:
[0083]
[0084]
[0085] Judging from the evaluation data, the propane conversion rate and propylene selectivity are significantly improved compared with the comparison agent, indicating that the catalyst prepared by this patent has good application value. Of course, the present invention can also have many other embodiments, and technicians familiar with this field can make various corresponding modifications and adjustments based on the present invention, but these should all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a thin layer of hydrotalcite-like material and catalyst and its application in propane dehydrogenation, wherein the specific preparation steps are as follows: (1) adding a certain amount of a first metal salt into a dissolving tank and dissolving it in water, then mixing the first metal salt solution with the second metal salt solution in a certain proportion to prepare a mixed solution, which is recorded as solution A; (2) In a water bath, solution A and an alkaline solution containing carbonate and auxiliary anions are simultaneously added to a reactor for co-precipitation, and the hydrolysis conditions are adjusted; (3) adding at least one of PEG-200, PEG-400, PEG-600, or PEG-1000 at the initial stage of the precipitation reaction; (4) The reactor was crystallized in a water bath. After the crystallization was completed, the material was washed with water until the pH was 7-8 to remove Na + and SO4 2- Finally, a thin layer of hydrotalcite-like material is obtained through slurrying, spray drying, and multi-step calcination (500-600℃).
2. The preparation method according to claim 1, wherein: The metal ion M of the first metal salt in step (1) 2+ Mg 2+ 、Zn 2+ 、Ni 2+ 、Cu 2+ 、Co 2+ 、Mn 2+ or Fe 2+ One or more of the metal ions M of the second metal salt 3+ Al 3+ 、Fe 3+ or Cr 3+ One or more of , and X=M 3+ / (M 2+ +M 3+ )=0.2-0.
34.
3. The preparation method according to claim 1, wherein: The hydrolysis conditions in step (2) include pH 8-10, temperature 40-60° C., and reaction time 4-8 hours.
4. The preparation method according to claim 1, wherein: The amount of PEG added in step (3) is 3%-8% of the mass of the hydrotalcite-like precursor, the crystallization temperature is 60-80° C., and the crystallization time is 8-12 hours.
5. The preparation method according to claim 1, wherein: The anions of the thin layered hydrotalcite-like material in step (4) include H2PO4 - 、ClO3 - 、[Ru(BPS)4]4 - , at least one of terephthalate.
6. A propane dehydrogenation catalyst, characterized in that: The thin layered hydrotalcite-like material according to claim 5 is used as a carrier, loaded with 0.1-1 wt% Pt and 0.5-3 wt% Sn, and Pt / Sn exists in the interlayer defect sites in a highly dispersed form with an average particle size of 1-5 nm.
7. The catalyst according to claim 6, characterized in that: In the propane dehydrogenation reaction, the reaction temperature is 550-650℃ and the space velocity is 1000-3000h -1 , propane conversion rate ≥40%, propylene selectivity ≥90%.
Citation Information
Patent Citations
Preparation method for flaky hierarchical-pore-structure hydrotalcite-like material and catalyst, and application of catalyst in propane dehydrogenation
CN110538652A