Enamel, photovoltaic glass and photovoltaic modules
By using a glaze composed of flux, ink oil, and pigments in a specific ratio, the problem of black glaze glass falling off in photovoltaic modules has been solved, thereby improving the stability and power generation efficiency of photovoltaic modules and making it suitable for high-end building integration.
Patent Information
- Application Number
- CN202510685537.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-05-26
AI Technical Summary
Existing black-glazed glass is prone to falling off when used in photovoltaic modules, resulting in poor stability and difficulty in matching traditional architectural styles.
A glaze composed of flux, ink oil and pigment in a specific ratio is used to prepare photovoltaic glass through ball milling and roller coating processes, ensuring that the glaze adheres firmly to the photovoltaic module.
The glaze is not easily detached from photovoltaic modules, exhibiting excellent stability and good power generation efficiency, making it suitable for building integration in high-end residential and commercial projects.
Smart Images

Figure BDA0005421342740000061 
Figure BDA0005421342740000062 
Figure BDA0005421342740000071
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic materials technology, and specifically relates to glazes, photovoltaic glass and photovoltaic modules. Background Technology
[0002] With the increasing popularity of Building Integrated Photovoltaics (BIPV), markets in Europe, America, and Japan are placing higher demands on the architectural integration of rooftop photovoltaic modules. Traditional buildings in these regions often use black roof tiles, and the traditional silver-framed, white-based photovoltaic modules are difficult to match due to their jarring color. All-black photovoltaic modules, with their pure black appearance, achieve a unified architectural style, making them the preferred choice for high-end residential and commercial projects. Black-glazed glass is a key component of all-black photovoltaic modules, made by coating the glass surface with a black glaze. Currently, the glaze coating on black-glazed glass is prone to peeling off when used in photovoltaic modules, resulting in poor stability and hindering its market adoption. Summary of the Invention
[0003] This invention aims to at least solve one of the technical problems existing in the prior art. To this end, this invention proposes an glaze, photovoltaic glass, and photovoltaic modules. When the photovoltaic glass prepared by this glaze is used in photovoltaic modules, the glaze will not easily peel off, exhibiting excellent stability.
[0004] The above-mentioned technical objective of the present invention is achieved through the following technical solution:
[0005] A glaze includes a flux, an ink oil, and a pigment, wherein the flux comprises the following raw materials: SiO2, Na2O, B2O3, SrO2, and Bi2O3.
[0006] In some embodiments of the present invention, the glaze comprises the following raw materials in parts by weight: flux: 45-70 parts; ink oil: 10-25 parts; pigment: 5-20 parts.
[0007] In some embodiments of the present invention, the percentages of each raw material in the flux are as follows: SiO2: 45wt%-55wt%; Na2O: 13wt%-20wt%; B2O3: 10wt%-20wt%; SrO2: 13.5wt%-14wt%; Bi2O3: 3wt%-3.5wt%.
[0008] In some embodiments of the present invention, the flux contains 13.8 wt% SrO2 and 3.2 wt% Bi2O3.
[0009] In some embodiments of the present invention, the ink oil includes a solvent, a resin, and a dispersant.
[0010] In some embodiments of the present invention, the percentages of each raw material in the ink oil are as follows: solvent: 40wt%-70wt%; resin: 2wt%-15wt%; dispersant: 15wt%-40wt%.
[0011] In some embodiments of the present invention, the solvent is water.
[0012] In some embodiments of the present invention, the dispersant is isopropanol.
[0013] In some embodiments of the present invention, the resin is one of epoxy resin, alkyd resin, PVB resin and polyurethane resin.
[0014] In some embodiments of the present invention, the resin is a polyurethane resin and the content of polyurethane resin in the ink oil is 4.5 wt%.
[0015] In some embodiments of the present invention, the ink conditioning oil is prepared by mixing the solvent and dispersant and stirring until they are evenly mixed, then adding the resin and stirring until the resin is completely dissolved, thus obtaining the ink conditioning oil.
[0016] In some embodiments of the present invention, the percentages of each raw material in the pigment are as follows: titanium dioxide: 5 wt%; copper powder: 55 wt%; chromium powder: 40 wt%.
[0017] The method for preparing the glaze as described above includes the following steps: mixing flux, ink oil and pigment and then grinding them.
[0018] In some embodiments of the present invention, the grinding refers to ball milling in a ball mill jar at a speed of 300-500 r / min for 6-10 h, with samples taken every 2 h to obtain a black glaze.
[0019] A photovoltaic glass is prepared by coating a glass surface with an enamel as described above.
[0020] In some embodiments of the present invention, the photovoltaic glass is prepared by: uniformly coating the glaze onto the surface of the original glass using a roller coater, then placing the glazed original glass in a drying oven at 150-200℃ for curing for 10-20 minutes, and after the solvent has completely evaporated, placing it in a muffle furnace at 600-750℃ for tempering for 3-10 minutes to obtain the photovoltaic glass.
[0021] A photovoltaic module, comprising the photovoltaic glass described above.
[0022] The beneficial effects of this invention are:
[0023] The photovoltaic glass prepared by the glaze of this invention will not easily fall off when used in photovoltaic modules, and at the same time has good power generation efficiency, thus taking into account both excellent stability and power generation efficiency, which is conducive to its promotion in the market. Detailed Implementation
[0024] The present invention will be further described below with reference to specific embodiments.
[0025] Example 1:
[0026] A glaze comprises the following raw materials in parts by weight: flux: 45 parts; ink oil: 10 parts; pigment: 5 parts; the raw materials in the flux and their percentages in the flux are: SiO2: 53.5 wt%; Na2O: 20 wt%; B2O3: 10 wt%; SrO2: 13.5 wt%; Bi2O3: 3 wt%; the raw materials in the ink oil and their percentages in the ink oil are: water: 70 wt%; epoxy resin: 15 wt%; isopropanol: 15 wt%; the preparation method of the ink oil is: mix water and isopropanol and stir evenly, then add epoxy resin and stir until the epoxy resin is completely dissolved to obtain the ink oil; the raw materials in the pigment and their percentages in the pigment are: titanium dioxide: 5 wt%; copper powder: 55 wt%; chromium powder: 40 wt%.
[0027] The method for preparing the glaze as described above includes the following steps: mixing flux, ink oil and pigment, and then ball milling them in a ball mill jar at a speed of 300 r / min for 10 h, taking samples every 2 h to obtain a black glaze.
[0028] A photovoltaic glass is prepared by: uniformly coating the glaze as described above onto the surface of the original glass using a roller coater, then placing the glazed original glass in a 150°C drying oven for 20 minutes to cure, and after the solvent has completely evaporated, placing it in a 600°C muffle furnace for 10 minutes to temper, thus obtaining the photovoltaic glass.
[0029] A photovoltaic module, comprising the photovoltaic glass described above.
[0030] Example 2:
[0031] A glaze comprises the following raw materials in parts by weight: flux: 70 parts; ink oil: 25 parts; pigment: 20 parts; the raw materials in the flux and their percentages in the flux are: SiO2: 45wt%; Na2O: 17.5wt%; B2O3: 20wt%; SrO2: 14wt%; Bi2O3: 3.5wt%; the raw materials in the ink oil and their percentages in the ink oil are: water: 55wt%; alkyd resin: 5wt%; isopropanol: 40wt%; the preparation method of the ink oil is: mix water and isopropanol and stir evenly, then add alkyd resin and stir until the alkyd resin is completely dissolved to obtain the ink oil; the raw materials in the pigment and their percentages in the pigment are: titanium dioxide: 5wt%; copper powder: 55wt%; chromium powder: 40wt%.
[0032] The method for preparing the glaze as described above includes the following steps: mixing flux, ink oil and pigment, and then ball milling them in a ball mill jar at a speed of 500 r / min for 6 hours, taking samples every 2 hours to obtain a black glaze.
[0033] A photovoltaic glass is prepared by: uniformly coating the glaze as described above onto the surface of the original glass using a roller coater, then placing the glazed original glass in a 200°C drying oven for 10 minutes to cure, and after the solvent has completely evaporated, placing it in a 750°C muffle furnace for 3 minutes to temper, thus obtaining the photovoltaic glass.
[0034] A photovoltaic module, comprising the photovoltaic glass described above.
[0035] Example 3:
[0036] A glaze comprises the following raw materials in the following percentages: flux: 66 parts; ink oil: 20 parts; pigment: 14 parts; the flux comprises the following raw materials: SiO2, Na2O, B2O3, SrO2 and Bi2O3; the ink oil comprises the following raw materials: water, resin and isopropanol; the ink oil is prepared by mixing water and isopropanol and stirring evenly, then adding resin and stirring until the resin is completely dissolved to obtain the ink oil; the raw materials in the pigment and their percentages in the pigment are: titanium dioxide: 5 wt%; copper powder: 55 wt%; chromium powder: 40 wt%.
[0037] The method for preparing the glaze as described above includes the following steps: mixing flux, ink oil and pigment, and then ball milling them in a ball mill jar at a speed of 400 r / min for 8 hours, taking samples every 2 hours to obtain a black glaze.
[0038] A photovoltaic glass is prepared by: uniformly coating the glaze as described above onto the surface of the original glass using a roller coater, then placing the glazed original glass in a 180°C drying oven for 15 minutes to cure, and after the solvent has completely evaporated, placing it in a 700°C muffle furnace for 5 minutes to temper, thus obtaining the photovoltaic glass.
[0039] A photovoltaic module, comprising the photovoltaic glass described above.
[0040] (1) First, the contents of Bi2O3 and SrO2 are set to control the impact resistance and weather resistance of the black enamel photovoltaic glass. With other components and process parameters unchanged, the weight percentage of the specific components of the flux is controlled as shown in Table 1 below:
[0041] Table 1.
[0042] serial number <![CDATA[SiO2]]> <![CDATA[Na2O]]> <![CDATA[B2O3]]> <![CDATA[Bi2O3]]> <![CDATA[SrO2]]> H001 52% 16% 15% 1.2% 15.8% H002 52% 16% 15% 2.2% 14.8% H003 52% 16% 15% 3.2% 13.8% H004 52% 16% 15% 4.2% 12.8%
[0043] The specific performance analysis is as follows, based on the control of Bi2O3 and SrO2 content:
[0044] 1) Adhesion: Take three points on the coating and use a crisscross tool with a 1mm interval to make a 10mm*10mm intersecting vertical grid. The scratches should reach the surface of the original glass. After removing the scratches, use tape to stick the scratched coating surface and quickly pull it up in a 90° direction. Repeat this 5 times and observe the changes and defects on the surface of the glaze coating grid.
[0045] 2) Hardness: A 5H hardness Chinese pencil was used to test the surface of the photovoltaic glass. After the scratches were erased with a soft eraser, the surface was visually inspected for scratches after the coating test.
[0046] 3) Acid resistance: Four different types of photovoltaic glass were placed in 0.1M HCl solution and soaked for 1h, 3h, 5h, 7h and 10h. After soaking, they were taken out, rinsed with distilled water, and dried at 100℃. The reflectance of the four different types of photovoltaic glass was then measured (using a Konica Minolta CM-26dG / 26d / 25d spectrophotometer) to study the stability of photovoltaic glass in acid solution.
[0047] 4) Alkali resistance: Four different types of photovoltaic glass were placed in 0.1M NaOH solution and soaked for 1h, 3h, 5h, 7h and 10h. After soaking, they were taken out, rinsed with distilled water, dried at 100℃ and the reflectivity of the four different types of photovoltaic glass was measured to study the stability of photovoltaic glass in alkaline solution.
[0048] 5) Salt resistance: Four different types of photovoltaic glass were placed in 0.1M NaCl solution and soaked for 1h, 3h, 5h, 7h and 1h. After soaking, they were taken out, rinsed with distilled water, dried at 100℃ and the reflectivity of the four different types of photovoltaic glass was measured to study the stability of photovoltaic glass in salt solution.
[0049] 6) Water resistance: Four different types of photovoltaic glass were placed in 80℃ hot water for 1h, 3h, 5h, 7h and 10h, then removed, rinsed with distilled water, dried at 100℃ and the reflectivity of the four different types of photovoltaic glass was tested to study the stability of photovoltaic glass in hot water.
[0050] 7) Moisture resistance: Four different photovoltaic glass samples were placed in a constant temperature and humidity chamber at 65℃ and 95% humidity for 168 hours. After being removed and cooled at room temperature for 30 minutes, the reflectance of the four different photovoltaic glass samples was measured.
[0051] 8) Thermal cycling resistance: Four different types of photovoltaic glass were placed in a constant temperature chamber. The temperature was set to 80±1℃ and kept at that temperature for 3 hours. Then the temperature was set to 40±1℃ and kept at that temperature for 3 hours. Then the temperature was raised to 80±1℃ and this cycle was repeated. The time for temperature rise or fall was 2 hours. A total of 20 cycles were tested, and the reflectivity of the four different types of photovoltaic glass was measured.
[0052] 9) UV resistance: Four different types of photovoltaic glass were irradiated with 8 UV150W lamps at 60℃ for 5 hours and then condensed at 50℃ for 5 hours as one cycle. A total of 10 cycles were conducted. The reflectivity of the four different types of photovoltaic glass was measured and the results were observed as shown in Table 2.
[0053] Table 2.
[0054]
[0055] As can be seen from the specific test results in Table 2, the glaze coating on H003 (i.e., when the contents of Bi2O3 and SrO2 are 3.2% and 13.8% respectively) will not peel off, demonstrating excellent stability.
[0056] (2) The type of resin in the ink coating affects the quality of the ink coating, which in turn has a significant impact on the power generation efficiency and impact resistance of photovoltaic modules. If the resin decomposes during drying, the ink coating will not adhere well enough and will peel off. If the resin does not decompose after the glass matrix softens, the ink coating will turn black, produce pinholes, and reduce the adhesion of the coating after sintering. Therefore, it is necessary to select an ink resin with a suitable decomposition temperature. While keeping the Bi2O3 and SrO2 contents constant at 3.2% and 13.8% respectively, the effects of four different resins on the power generation efficiency and impact resistance of photovoltaic modules were investigated. The test results are shown in Table 3.
[0057] Table 3.
[0058]
[0059]
[0060] As can be seen from the specific test results in Table 3, polyurethane resin has the greatest impact on the power generation efficiency and impact resistance of photovoltaic modules.
[0061] (3) Next, it is necessary to find a suitable polyurethane resin content. Therefore, five ink oils were designed. The polyurethane resin content in the ink oils is shown in Table 4. The influence of different polyurethane resin contents on the power generation efficiency and impact resistance of photovoltaic modules was investigated.
[0062] Table 4.
[0063]
[0064] As can be seen from the test results in Table 4, when the polyurethane resin content in the ink is 4.5 wt%, its impact resistance and power generation efficiency can reach the optimal level.
[0065] In summary, when the contents of Bi2O3 and SrO2 in the flux are 3.2% and 13.8% respectively, and the polyurethane resin in the ink is a synthetic raw material with a content of 4.5 wt%, the photovoltaic module can have the best power generation efficiency and stability.
[0066] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A glaze, characterized by: The mixture includes flux, ink oil, and pigments; the ink oil includes solvent, resin, and dispersant, wherein the resin is polyurethane resin and the content of polyurethane resin in the ink oil is 4.5 wt%; the percentage of each raw material in the flux is as follows: SiO2: 45 wt%-55 wt%; Na2O: 13 wt%-20 wt%; B2O3: 10 wt%-20 wt%; SrO2: 13.5 wt%-14 wt%; Bi2O3: 3 wt%-3.5 wt%.
2. A glaze according to claim 1, characterised in that: The glaze comprises the following raw materials in parts by weight: flux: 45-70 parts; ink oil: 10-25 parts; pigment: 5-20 parts.
3. A glaze according to claim 1, characterised in that: The percentages of solvent and dispersant in the ink oil are as follows: solvent: 40wt%-70wt%; dispersant: 15wt%-40wt%.
4. A glaze according to claim 1, characterised in that: The preparation method of the ink conditioning oil is as follows: after mixing the solvent and dispersant and stirring evenly, the resin is added and stirred until the resin is completely dissolved, and the ink conditioning oil is obtained.
5. The method for preparing the glaze according to any one of claims 1-4, characterized in that: Includes the following steps: It is obtained by mixing flux, ink oil and pigment and then grinding.
6. A photovoltaic glass, characterized in that: The photovoltaic glass is prepared by coating the glass surface with the glaze described in any one of claims 1-4.
7. A photovoltaic module, characterized in that: Includes the photovoltaic glass as described in claim 6.
Citation Information
Patent Citations
Glass powder for photovoltaic ink and preparation method thereof
CN114249538A
Photovoltaic black glaze as well as preparation method and application thereof
CN119977333A
Glass frit for formation of barrier wall, back glass substrate for plasma display panel and plasma display panel
JP2003020251A