Anti-fouling and anti-seepage hollow injection molding barrel and preparation process thereof

The preparation of chitosan composite coating solves the problem of balancing antifouling and anti-seepage performance with transparency of polypropylene injection-molded barrels, achieving high transparency and good antifouling and anti-seepage effects.

CN120665467AInactive Publication Date: 2025-09-19JIANGXI FUTENG PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511093763.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-06
Publication Date
2025-09-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polypropylene injection-molded barrels have difficulty in achieving both anti-fouling and anti-seepage properties and transparency, and existing coating modifications lead to performance degradation.

Method used

Chitosan composite coatings, including double-bonded chitosan, composite modified chitosan and silicone oil modified chitosan, are used to improve compatibility and impermeability while maintaining high transparency by controlling the proportion of each component and the degree of cross-linking.

Benefits of technology

The prepared anti-fouling and anti-seepage hollow injection-molded barrel has good anti-fouling and anti-seepage performance while maintaining high transparency, thus solving the problem of performance degradation in the prior art.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of anti-fouling and anti-seepage coatings, and discloses an anti-fouling and anti-seepage hollow injection molding barrel and a preparation process thereof. The preparation process comprises the following steps: S1, adding styrene, acrylic acid, fluorine-containing acrylate, divinyl benzene, bicyclo [2.2. 2] octyl-5-ene-2, 3-dicarboxylic anhydride, a chitosan composition, potassium persulfate and an emulsifier into water, and uniformly stirring to obtain an antifouling and anti-seepage coating; s2, the surface of the polypropylene hollow injection molding barrel is coated with the antifouling and anti-seepage coating, heat preservation is conducted for 6-7 h at the temperature of 75-80 DEG C, drying is conducted, and the antifouling and anti-seepage hollow injection molding barrel is obtained; the chitosan composition is a composition of double-bond chitosan, composite modified chitosan and silicone oil modified chitosan; the mass ratio of the double-bond chitosan to the composite modified chitosan to the silicone oil modified chitosan is (3-4): 1: (6-8).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-fouling and anti-seepage coatings, and discloses an anti-fouling and anti-seepage hollow injection molding barrel and a preparation process thereof. Background Art

[0002] Plastic barrels, known for their rust-resistant and lightweight properties, are widely used in industrial production and daily life. Injection-molded barrels made from polypropylene resin offer relatively high hardness, low specific gravity, high tensile strength, excellent resistance to stress cracking, and chemical resistance. Their high transparency also meets the specific needs of a variety of applications.

[0003] Injection-molded barrels made of polypropylene resin have room for improvement in terms of anti-fouling and anti-seepage performance. Due to the poor compatibility of polypropylene with various polar polymers or additives, modifying them with these substances inevitably leads to a decrease in the performance of the polypropylene itself. Therefore, existing technologies often improve the performance of the barrels by applying coatings to the barrel surface, but these coatings also have the problem of achieving both anti-fouling and anti-seepage performance and transparency. Therefore, the development of a highly transparent, anti-fouling and anti-seepage hollow injection-molded barrel and its preparation process are of great significance. Summary of the Invention

[0004] The object of the present invention is to provide a anti-fouling and anti-seepage hollow injection molding barrel and a preparation process thereof, so as to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a preparation process of an anti-fouling and anti-seepage hollow injection molding barrel, comprising the following steps:

[0006] S1: Add styrene, acrylic acid, divinylbenzene, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, chitosan composition, emulsifier, fluorinated acrylate, and potassium persulfate to water and mix well to obtain an antifouling and anti-seepage coating;

[0007] S2: applying an antifouling and anti-seepage coating to the surface of a polypropylene hollow injection-molded barrel to a thickness of 10 to 100 μm, maintaining the coating at 75 to 80° C. for 6 to 7 hours, and drying to obtain an antifouling and anti-seepage hollow injection-molded barrel;

[0008] In the chitosan composition, the mass ratio of double-bonded chitosan, composite modified chitosan and silicone oil modified chitosan is (3-4):1:(6-8).

[0009] More optimally, the antifouling and anti-seepage coating comprises the following raw materials, calculated by mass: 40 to 50 parts of styrene, 20 to 30 parts of acrylic acid, 1 to 2 parts of divinylbenzene, 1 to 2 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 3 to 6 parts of chitosan composition, 1 to 2 parts of emulsifier, 1 to 2 parts of fluorine-containing acrylate, 0.1 to 0.2 parts of potassium persulfate, and 50 to 80 parts of water;

[0010] More optimally, the preparation of the double-bonded chitosan comprises the following steps: by weight: taking succinic anhydride and maleic anhydride, adding them to dimethyl sulfoxide and stirring evenly, adding chitosan, stirring and reacting at 55-60° C. for 1-2 hours, and removing the solvent to obtain double-bonded chitosan;

[0011] The double-bonded chitosan comprises the following raw materials, calculated by mass: 0.1-0.2 parts of succinic anhydride, 0.3-0.5 parts of maleic anhydride, and 1-2 parts of chitosan.

[0012] More optimally, the preparation of the composite modified chitosan includes the following steps: Step 1: adding bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, polyethylene glycol monooleate and lutidine to dimethyl sulfoxide, heating to 65-70° C. and stirring evenly, keeping the temperature to react for 2-3 hours, and removing the solvent to obtain modified polyethylene glycol monooleate;

[0013] Step 2: Take modified polyethylene glycol monooleate and chitosan, add them to dimethyl sulfoxide and stir evenly, add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide at 20-25°C, stir for 1-2h, heat to 80-90°C, stir for 18-24h, remove the solvent, and obtain composite modified chitosan.

[0014] More optimally, the modified polyethylene glycol monooleate comprises the following raw materials, calculated by weight: 15 to 20 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 30 to 35 parts of polyethylene glycol monooleate, and 2 to 3 parts of lutidine;

[0015] The composite modified chitosan comprises the following raw materials, calculated by mass: 1-2 parts of modified polyethylene glycol monooleate, 3-5 parts of chitosan, 0.5-1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and 0.5-1 part of N-hydroxysuccinimide.

[0016] More optimally, the preparation of the silicone oil-modified chitosan includes the following steps: taking double-bonded chitosan, adding it to an acetic acid aqueous solution and stirring evenly to obtain a chitosan solution; stirring epoxy silicone oil and isopropyl alcohol evenly, adding them to the chitosan solution, heating to 55-65°C, stirring and reacting for 4-6 hours, and removing the solvent to obtain silicone oil-modified chitosan.

[0017] More optimally, the silicone oil-modified chitosan comprises the following raw materials, calculated by mass: 1-2 parts of double-bonded chitosan, 100-200 parts of acetic acid aqueous solution, 0.1-0.2 parts of epoxy silicone oil, and 2-5 parts of isopropyl alcohol.

[0018] More optimally, the preparation of the polypropylene hollow injection molding barrel includes the following steps: taking polypropylene resin, placing it in the barrel of an injection molding machine, heating and melting it, injecting it into a mold, and shaping it to obtain a polypropylene hollow injection molding barrel.

[0019] Compared with the prior art, the present invention achieves the following beneficial effects: a chitosan composition is added to the antifouling and anti-seepage coating; chitosan itself has good film-forming properties, and the amino groups impart excellent oil resistance to it; however, since the amino groups are hydrophilic groups, the overall hydrophobicity is relatively poor; therefore, the chitosan composition of the present invention is a composition of double-bonded chitosan, composite modified chitosan, and silicone oil-modified chitosan in a certain mass ratio; after the chitosan is double-bonded, groups that can participate in cross-linking reactions are introduced to improve the overall compatibility; the double-bonding process of this step needs to be controlled to ensure that some amino groups are still present, otherwise the oil resistance will decrease, resulting in a decrease in the overall antifouling performance; Silicone oil modified chitosan introduces a hydrophobic silicone oil structure to improve the poor hydrophobicity of chitosan; polyethylene glycol monooleate is introduced into the composite modified chitosan, and the presence of polyethylene glycol monooleate allows it to serve as a compatibilizer between double-bonded hydrophilic chitosan and silicone oil modified hydrophobic chitosan, thereby improving the overall affinity; the addition ratio of each raw material in the chitosan composition needs to be controlled to balance the hydrophobicity and oleophobicity to achieve a good anti-fouling effect; at the same time, the introduction of the chitosan composition can increase the cross-linking points of the coating, and the increase in the degree of cross-linking can increase the impermeability, but the amount added needs to be controlled, as excessive cross-linking will lead to a decrease in transparency. In summary, the polypropylene injection barrel prepared by this scheme has high transparency and good anti-fouling and anti-permeation capabilities. DETAILED DESCRIPTION

[0020] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0021] It should be noted that the purchasers of all raw materials involved in the present invention are not subject to any special restrictions, and illustratively include: ethanol (CAS: 64-17-5); polypropylene resin (7633U high-transmittance polypropylene); polydimethylsiloxane (A214840, Zhengzhou Alpha Chemical Co., Ltd.); fluorinated silicone oil (F-102 fluorosilicone oil, Aluda New Materials); maleic anhydride (CAS: 108-31-6); chitosan (S11064, Yuanye); bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride (CAS: 6708-37-8); polyethylene glycol monooleate ( CAS: 9004-96-0); Lutidine (CAS: 108-47-4); 1-(3-Dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (S39167, Yuanye); N-hydroxysuccinimide (CAS: 6066-82-6); Epoxy silicone oil (A00227, Jiyesheng); Styrene (CAS: 100-42-5); Divinylbenzene (CAS: 1321-74-0); Emulsifier (sodium lauryl sulfate, CAS: 151-21-3); Fluorinated acrylate (heptafluorobutyl acrylate, CAS: 424-64-6);

[0022] Unless otherwise specified, the following are parts by mass and mass ratios;

[0023] The raw material of polypropylene hollow injection molding barrel is polypropylene resin (7633U high-transparency polypropylene). The polypropylene resin is placed in the barrel of the injection molding machine, heated and melted, and then injected into the mold to make it.

[0024] Example 1: S1: Take 0.1 parts of succinic anhydride and 0.4 parts of maleic anhydride, add 100 parts of dimethyl sulfoxide, stir evenly, add 1.5 parts of chitosan, stir and react at 60°C for 2 hours, remove the solvent to obtain double-bonded chitosan;

[0025] S2: Add 18 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 35 parts of polyethylene glycol monooleate and 2 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0026] S3: Take 1 part of modified polyethylene glycol monooleate and 4 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0027] S4: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0028] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 4:1:7 to obtain a chitosan composition: 45 parts of styrene, 25 parts of acrylic acid, 1 part of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 5 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0029] Example 2: S1: Take 0.2 parts of succinic anhydride and 0.3 parts of maleic anhydride, add 100 parts of dimethyl sulfoxide, stir evenly, add 1 part of chitosan, stir and react at 60°C for 2 hours, remove the solvent to obtain double-bonded chitosan;

[0030] S2: Add 15 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 30 parts of polyethylene glycol monooleate and 2 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0031] S3: Take 1 part of modified polyethylene glycol monooleate and 3 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0032] S4: Take 1 part of double-bonded chitosan, add it to 100 parts of 2wt% acetic acid aqueous solution, stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add it to the chitosan solution, heat it to 60°C, stir and react for 6 hours, remove the solvent to obtain silicone oil-modified chitosan;

[0033] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 3:1:7 to obtain a chitosan composition: 40 parts of styrene, 30 parts of acrylic acid, 1 part of divinylbenzene, 2 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 6 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0034] Example 3: S1: Take 0.2 parts of succinic anhydride and 0.5 parts of maleic anhydride, add 200 parts of dimethyl sulfoxide, stir evenly, add 2 parts of chitosan, stir and react at 60°C for 2 hours, remove the solvent to obtain double-bonded chitosan;

[0035] S2: Add 20 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 35 parts of polyethylene glycol monooleate and 3 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0036] S3: Take 2 parts of modified polyethylene glycol monooleate and 5 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0037] S4: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0038] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 4:1:8 to obtain a chitosan composition: 40 parts of styrene, 30 parts of acrylic acid, 2 parts of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 3 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0039] Comparative Example 1 (changing the raw material ratio in the chitosan composition, the remaining method steps are consistent with Example 1): S1: Take 0.2 parts of succinic anhydride and 0.4 parts of maleic anhydride, add 150 parts of dimethyl sulfoxide, stir evenly, add 1.5 parts of chitosan, stir at 60°C for 2 hours, remove the solvent, and obtain double-bonded chitosan;

[0040] S2: Add 18 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 35 parts of polyethylene glycol monooleate and 2 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0041] S3: Take 1 part of modified polyethylene glycol monooleate and 4 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0042] S4: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0043] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 1:1:7 to obtain a chitosan composition: 45 parts of styrene, 25 parts of acrylic acid, 1 part of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 5 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0044] Comparative Example 2 (changing the raw material ratio in the chitosan composition, the remaining method steps are consistent with Example 1): S1: Take 0.1 parts of succinic anhydride and 0.4 parts of maleic anhydride, add 150 parts of dimethyl sulfoxide, stir evenly, add 1.5 parts of chitosan, stir at 60°C for 2 hours, remove the solvent, and obtain double-bonded chitosan;

[0045] S2: Add 18 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 35 parts of polyethylene glycol monooleate and 2 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0046] S3: Take 1 part of modified polyethylene glycol monooleate and 4 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0047] S4: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0048] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 7:1:4 to obtain a chitosan composition: 45 parts of styrene, 25 parts of acrylic acid, 1 part of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 5 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept warm at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0049] Comparative Example 3 (increasing the amount of chitosan composition added, and the remaining steps are consistent with Example 1): S1: 0.1 parts of succinic anhydride and 0.4 parts of maleic anhydride were added to 150 parts of dimethyl sulfoxide, stirred evenly, and 1.5 parts of chitosan were added. The mixture was stirred at 60°C for 2 hours, and the solvent was removed to obtain double-bonded chitosan;

[0050] S2: Add 18 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 35 parts of polyethylene glycol monooleate and 2 parts of lutidine to 500 parts of dimethyl sulfoxide, heat to 70°C, stir evenly, keep warm and react for 3 hours, and remove the solvent to obtain modified polyethylene glycol monooleate;

[0051] S3: Take 1 part of modified polyethylene glycol monooleate and 4 parts of chitosan, add them to 300 parts of dimethyl sulfoxide and stir evenly, add 1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 parts of N-hydroxysuccinimide at 25°C, stir for 2 hours, heat to 90°C, stir for 20 hours, wash to remove impurities, remove the solvent, and obtain composite modified chitosan;

[0052] S4: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0053] S5: Double-bonded chitosan, composite modified chitosan, and silicone oil modified chitosan are mixed in a mass ratio of 4:1:7 to obtain a chitosan composition: 45 parts of styrene, 25 parts of acrylic acid, 1 part of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 8 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0054] Comparative Example 4 (no composite modified chitosan was added, and the remaining steps were the same as those in Example 1): S1: 0.1 parts of succinic anhydride and 0.4 parts of maleic anhydride were added to 150 parts of dimethyl sulfoxide, stirred evenly, and 1.5 parts of chitosan were added. The mixture was stirred at 60° C. for 2 h, and the solvent was removed to obtain double-bonded chitosan.

[0055] S2: Take 2 parts of double-bonded chitosan, add them to 100 parts of 2 wt% acetic acid aqueous solution, and stir evenly to obtain a chitosan solution; stir evenly 0.2 parts of epoxy silicone oil and 5 parts of isopropyl alcohol, add them to the chitosan solution, heat to 60°C, stir and react for 6 hours, and remove the solvent to obtain silicone oil-modified chitosan;

[0056] S3: Double-bonded chitosan and silicone oil-modified chitosan are mixed in a mass ratio of 4:7 to obtain a chitosan composition: 45 parts of styrene, 25 parts of acrylic acid, 1 part of divinylbenzene, 1 part of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 5 parts of chitosan composition, 1 part of emulsifier, 1 part of fluorine-containing acrylate, and 0.1 part of potassium persulfate are added to 60 parts of water and stirred evenly to obtain an antifouling and anti-seepage coating; the antifouling and anti-seepage coating is applied to the surface of a polypropylene hollow injection molding barrel with a coating thickness of 60 μm, kept at 80°C for 6 hours, and dried to obtain an antifouling and anti-seepage hollow injection molding barrel.

[0057] Performance test: Take polypropylene resin, select the same process as that for preparing polypropylene hollow injection molding barrel, place it in the barrel of an injection molding machine, heat and melt it, inject it into the mold, and then stretch and shape it to obtain a 100 μm polypropylene plate; apply the antifouling and anti-seepage coating prepared in Examples 1 to 3 and Comparative Examples 1 to 4 on the surface of the polypropylene plate to a coating thickness of 60 μm, keep it at 80°C for 6 hours, and dry it to obtain a sample; (1) test the light transmittance with reference to ASTM D1003; (2) test the water contact angle; (3) test the antifouling performance by wiping with absorbent cotton and measuring the number of times the scratch by an oil pen can be erased; see Table 1 for details;

[0058] Table 1:

[0059] Transmittance / % Water contact angle / ° Oil-resistant pen wipe Example 1 91.0 135 161 Example 2 90.4 131 156 Example 3 90.7 132 155 Comparative Example 1 84.6 112 144 Comparative Example 2 85.2 124 135 Comparative Example 3 83.3 108 120 Comparative Example 4 83.1 121 136

[0060] Conclusion: In comparative example 1, the raw material ratio in the chitosan composition is changed, with less double-bonded chitosan and more silicone oil-modified chitosan, the cross-linking degree and hydrophobicity and oleophobicity are changed, and the performance is significantly reduced; in comparative example 2, more double-bonded chitosan and less silicone oil-modified chitosan are used, and the oil resistance is reduced; in comparative example 3, the amount of chitosan composition added is increased, and the resulting coating is rough, resulting in a significant reduction in performance; in comparative example 4, no composite modified chitosan is added, and the performance is reduced due to the lack of a compatibilizer, which shows the importance of this substance; in summary, this scheme prepares a polypropylene injection barrel with high transparency, high waterproofness, anti-fouling and anti-penetration.

[0061] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art will be able to modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.

Claims

1. A process for preparing a pollution-proof and anti-seepage hollow injection-molded barrel, characterized by: The following steps are involved: S1: Add styrene, acrylic acid, divinylbenzene, fluorinated acrylate, emulsifier, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, chitosan composition, and potassium persulfate to water and stir evenly to obtain an antifouling and anti-seepage coating; S2: applying the antifouling and anti-seepage coating to the surface of a polypropylene hollow injection-molded barrel, keeping the barrel at 75-80° C. for 6-7 hours, and drying the barrel to obtain an antifouling and anti-seepage hollow injection-molded barrel; The chitosan composition consists of double-bonded chitosan, composite modified chitosan and silicone oil modified chitosan.

2. The process for preparing a anti-fouling and anti-seepage hollow injection molding barrel according to claim 1, characterized in that: The antifouling and anti-seepage coating comprises the following raw materials, calculated by mass: 40 to 50 parts of styrene, 20 to 30 parts of acrylic acid, 1 to 2 parts of divinylbenzene, 1 to 2 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 3 to 6 parts of chitosan composition, 0.1 to 0.2 parts of potassium persulfate, 50 to 80 parts of water, 1 to 2 parts of emulsifier, and 1 to 2 parts of fluorine-containing acrylate; In the chitosan composition, the mass ratio of double-bonded chitosan, composite modified chitosan and silicone oil modified chitosan is (3-4):1:(6-8).

3. The process for preparing a anti-fouling and anti-seepage hollow injection molding barrel according to claim 1, characterized in that: Preparation of the double-bonded chitosan The method comprises the following steps: taking succinic anhydride and maleic anhydride, adding them into dimethyl sulfoxide and stirring evenly, adding chitosan, stirring and reacting at 55-60 DEG C for 1-2 hours, and removing the solvent to obtain double-bonded chitosan.

4. The process for preparing a anti-fouling and anti-seepage hollow injection-molded barrel according to claim 3, characterized in that: The double-bonded chitosan comprises the following raw materials, calculated by mass: 0.1-0.2 parts of succinic anhydride, 0.3-0.5 parts of maleic anhydride, and 1-2 parts of chitosan.

5. The process for preparing a anti-fouling and anti-seepage hollow injection molded barrel according to claim 1, characterized in that: Preparation of the composite modified chitosan The method comprises the following steps: step 1: adding bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, polyethylene glycol monooleate and lutidine to dimethyl sulfoxide, heating to 65-70° C., stirring evenly, keeping the temperature to react for 2-3 hours, and removing the solvent to obtain modified polyethylene glycol monooleate; Step 2: Take modified polyethylene glycol monooleate and chitosan, add them to dimethyl sulfoxide and stir evenly, add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide at 20-25°C, stir for 1-2h, heat to 80-90°C, stir for 18-24h, remove the solvent, and obtain composite modified chitosan.

6. The process for preparing a anti-fouling and anti-seepage hollow injection-molded barrel according to claim 5, characterized in that: The modified polyethylene glycol monooleate comprises the following raw materials, calculated by mass: 15 to 20 parts of bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 30 to 35 parts of polyethylene glycol monooleate, and 2 to 3 parts of lutidine; The composite modified chitosan comprises the following raw materials, calculated by mass: 1-2 parts of modified polyethylene glycol monooleate, 3-5 parts of chitosan, 0.5-1 part of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and 0.5-1 part of N-hydroxysuccinimide.

7. The process for preparing a anti-fouling and anti-seepage hollow injection molded barrel according to claim 4, characterized in that: The preparation of the silicone oil modified chitosan comprises the following steps: Take double-bonded chitosan, add it to acetic acid aqueous solution and stir evenly to obtain chitosan solution; stir epoxy silicone oil and isopropyl alcohol evenly, add them to the chitosan solution, heat to 55-65°C, stir and react for 4-6 hours, remove the solvent to obtain silicone oil-modified chitosan.

8. The process for preparing a anti-fouling and anti-seepage hollow injection-molded barrel according to claim 7, characterized in that: The silicone oil modified chitosan comprises the following raw materials, calculated by mass: 1-2 parts of double-bonded chitosan, 0.1-0.2 parts of epoxy silicone oil, and 2-5 parts of isopropyl alcohol.

9. An anti-fouling and anti-seepage hollow injection-molded barrel prepared according to the process for preparing an anti-fouling and anti-seepage hollow injection-molded barrel according to any one of claims 1 to 8.