Method for manufacturing wiring board
By alternately stacking conductor layers and insulating layers on a supporting substrate and using direct imaging exposure technology to form fine wiring, the problem of low yield in the wiring substrate manufacturing process is solved, and efficient manufacturing of wiring substrates with multi-layer structures is achieved.
Patent Information
- Application Number
- CN202510224379.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-21
- Filing Date
- 2025-02-27
- Publication Date
- 2025-09-23
AI Technical Summary
In the prior art, relatively fine wiring substrates have a low yield rate during the manufacturing process, especially when the first wiring substrate and the second wiring substrate are bonded together, making it difficult to effectively improve the manufacturing efficiency.
Direct imaging exposure technology is used to alternately stack conductive layers and insulating layers on a supporting substrate to form a first build-up portion with fine wiring. The second and third build-up portions are then stacked in an opposing manner, utilizing a multi-layer structure to improve wiring density and connection reliability.
The invention realizes efficient manufacturing of a wiring substrate including multiple conductor layers with different wiring densities, improves the yield and manufacturing efficiency, and reduces the increase in working hours in the manufacturing process.
Smart Images

Figure CN120692779A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a wiring substrate. Background Art
[0002] Patent Document 1 discloses a method for manufacturing a wiring substrate comprising a first wiring substrate and a second wiring substrate. The first wiring substrate is formed by laminating an insulating resin and a wiring layer on a support substrate. The second wiring substrate is manufactured separately from the first wiring substrate. After the first and second wiring substrates are bonded, the support substrate is peeled off.
[0003] Patent Document 1: Japanese Patent Application Laid-Open No. 2020-4926
[0004] In the wiring board manufacturing method disclosed in Patent Document 1, a first wiring board and a second wiring board, each containing relatively fine wiring layers, must be joined via terminals protruding from their respective surfaces, and an insulating resin is filled between the first and second wiring boards. This is believed to reduce the yield rate during wiring board manufacturing. Summary of the Invention
[0005] A method for manufacturing a wiring substrate according to the present invention includes the following steps: preparing two first support substrates having a first surface and a second surface opposite the first surface and having one or more product areas; forming first build-up sections each including the first conductor layer and the first insulation layer by alternately stacking a first conductor layer and a first insulation layer within the one or more product areas on the first surface of each of the first support substrates; and forming second build-up sections by alternately stacking a second conductor layer and a second insulation layer on the side of each first build-up section opposite the first support substrate, with the second surfaces of the two first support substrates facing each other in the thickness direction of the first support substrates. The step of stacking the first conductor layers includes forming a first resist layer having a first resist pattern to form a conductor pattern according to the first resist pattern, and the step of forming the first resist layer having the first resist pattern includes exposing the first resist layer by direct imaging exposure, wherein the first and second conductor layers are formed such that the minimum width and minimum spacing of wiring in the first conductor layer are smaller than the minimum width and minimum spacing of wiring in the second conductor layer, respectively.
[0006] According to the embodiment of the present invention, a wiring substrate including a plurality of conductor layers having different wiring densities can be manufactured efficiently with good yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1This is a cross-sectional view showing an example of a wiring board manufactured by a manufacturing method according to an embodiment of the present invention.
[0008] Figure 2A This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0009] Figure 2B This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0010] Figure 2C This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0011] Figure 2D This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0012] Figure 2E This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0013] Figure 2F This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0014] Figure 2G This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0015] Figure 2H This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0016] Figure 2I This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0017] Figure 2J This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0018] Figure 2K This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0019] Figure 2L This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0020] Figure 2M This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0021] Figure 2N This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0022] Figure 2O This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0023] Figure 2P This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0024] Figure 2Q This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0025] Figure 2R This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0026] Figure 2S This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0027] Figure 2T This is a diagram showing an example of a method for manufacturing a wiring board according to an embodiment of the present invention.
[0028] Description of labels
[0029] 1: Wiring substrate; 10: First build-up portion; 20: Second build-up portion; 30: Third build-up portion; 11: Insulating layer (first insulating layer); 12: Conductor layer (first insulating layer); 21: Insulating layer (second insulating layer); 22: Conductor layer (second conductor layer); 13, 23, 33: Via conductors; 121, 221: Metal film layer; 122, 222: Plated film layer; 12p, 32p: Conductor pads; FW: Wiring (fine wiring); SP1: First supporting substrate; SP1a: First surface of the first supporting substrate; SP1b: Second surface of the first supporting substrate; SP2: Second supporting substrate; RL1: Resist layer (first resist layer); RL2: Resist layer (second resist layer). DETAILED DESCRIPTION
[0030] A wiring board manufactured by a method for manufacturing a wiring board according to an embodiment will be described with reference to the drawings. Figure 1 1 is a cross-sectional view showing a wiring substrate 1 as an example of a wiring substrate manufactured by a manufacturing method according to an embodiment. The wiring substrate 1 is merely an example of a wiring substrate to be manufactured. The laminated structure of the wiring substrate to be manufactured and the number of conductor layers and insulating layers are not limited to Figure 1 The laminated structure of the wiring substrate 1 and the number of conductor layers and insulating layers included in the wiring substrate 1 are shown. In addition, the referenced drawings are not intended to show the exact ratio of each component, but are depicted in a manner that facilitates understanding of the characteristics of the present invention.
[0031] The wiring substrate 1 has a laminated structure including a first buildup portion 10 and a second buildup portion 20 each consisting of a plurality of conductor layers and insulating layers alternately laminated. Figure 1 As shown, the wiring substrate 1 may further include a third build-up portion 30 composed of an insulating layer and a conductive layer stacked on the insulating layer on the side of the second build-up portion 20 opposite to the first build-up portion 10. The wiring substrate 1 has two surfaces perpendicular to its thickness direction (a first surface 1F and a second surface 1B on the side opposite to the first surface 1F). Figure 1 As shown, the surface of first build-up section 10 (first surface 10F) constitutes first surface 1F. When wiring substrate 1 includes third build-up section 30, second surface 1B can be constituted by the surface of third build-up section 30 (second surface 30B). Alternatively, when third build-up section 30 is not formed and the wiring substrate is composed of first build-up section 10 and second build-up section 20, second surface 1B can be constituted by the surface of second build-up section 20 (second surface 20B). Wiring substrate 1 is formed as a coreless wiring substrate that does not include a core layer.
[0032] The first build-up portion 10 includes relatively fine wiring and can have a relatively high density of circuit wiring. Figure 1 In the example shown, the first build-up portion 10 has insulating layers (first insulating layers) 11 and conductive layers (first conductive layers) 12 alternately stacked. The conductive layers 12 facing each other with the first insulating layer 11 interposed therebetween are connected to each other by via conductors (first via conductors) 13. The first conductive layer 12 is patterned to have a predetermined conductive pattern. The first surface 10F of the first build-up portion 10 is composed of the surface (upper surface) of the first conductive layer 12 and the surface (upper surface) of the first insulating layer 11 exposed from the pattern of the conductive layer 12. In the example shown in the figure, the conductive layer 12 constituting the first surface 10F is formed into a pattern having a plurality of conductive pads 12p.
[0033] In addition, Figure 1 In the description of wiring substrate 1 shown, first surface 10F of first build-up portion 10, that is, the side of first surface 1F of wiring substrate 1, is referred to as "upper" or "upper side," and the side of second surface 1B of wiring substrate 1 is referred to as "lower" or "lower side." Furthermore, in various components, the surface of wiring substrate 1 facing first surface 1F is also referred to as the "upper surface," and the surface of wiring substrate 1 facing second surface 1B is also referred to as the "lower surface."
[0034] The conductor pad 12p is the uppermost surface of the first buildup portion 10, i.e., the outermost surface of the wiring substrate 1, and constitutes the component mounting surface of the wiring substrate 1 to which external electronic components can be connected. The component mounting surface of the wiring substrate 1 may also have multiple component mounting areas. For example, Figure 1As shown in the example of , two component mounting areas (EA1, EA2) may be formed corresponding to the areas where the electronic components E1, E2 are to be mounted.
[0035] In the illustrated example, when external electronic components are mounted on wiring substrate 1, the exposed upper surfaces of conductor pads 12p can be electrically and mechanically connected to the external electronic components via conductive bonding materials (not shown) such as solder, for example, between the upper surfaces of the external electronic components. In this case, a plating layer (not shown), such as a nickel layer and a tin layer, may be pre-formed on the upper surfaces of conductor pads 12p.
[0036] When multiple component mounting areas are formed, a conductor pattern capable of electrically connecting conductor pads 12p located in adjacent component mounting areas may be formed in conductor layer 12 within first build-up portion 10. During use, multiple electronic components mounted on wiring substrate 1 are electrically connected to each other via first build-up portion 10 via short paths. Examples of electronic components E1 and E2 that can be mounted on wiring substrate 1 include active components such as semiconductor integrated circuit devices and transistors.
[0037] exist Figure 1 In the example shown in FIG1 , second surface 10B of first build-up section 10, which is opposite to first surface 10F, is composed of the surface (lower surface) of insulating layer 11 and the surface (lower surface and side surfaces) of conductive layer 12. First build-up section 10 is stacked so that second surface 10B faces first surface 20F of second build-up section 20, which is opposite to second surface 20B.
[0038] The insulating layer 11 of the first laminated portion 10 can be formed using insulating resins such as epoxy resin and phenolic resin. The insulating layer 11 can include any one of fluororesin, liquid crystal polymer (LCP), polytetrafluoroethylene (PTFE), polyester resin (PE), and modified polyimide resin (MPI). The conductors constituting the conductor layer 12 and the via conductor 13 may be copper, nickel, etc., and copper is preferably used. Figure 1 , for ease of viewing, the conductor layer 12 and the via conductor 13 are shown as a single layer, but the conductor layer 12 and the via conductor 13 may have a multilayer structure. For example, the conductor layer 12 and the via conductor 13 may have a two-layer structure including a metal film layer (preferably a sputtered film layer or a chemically plated film layer) and a plated film layer (preferably an electroplated film layer).
[0039] The via conductor 13 that penetrates the insulating layer 11 in the thickness direction is formed by filling the through hole 11a that penetrates the insulating layer 11 with a conductor. Figure 1In the example, the via conductor 13 is formed integrally with the conductor layer 12 provided on the lower side thereof. Therefore, the via conductor 13 and the conductor layer 12 can be formed by the same metal film layer and the plated film layer. The conductor layer 12 is formed on the surface of the lower side of the insulating layer 11. The through hole 11a is formed, for example, so that the aspect ratio of the via conductor 13 (the height from the upper surface of the lower conductor layer 12 connected to the via conductor 13 to the lower surface of the upper conductor layer 12 / the diameter of the via conductor 13 on the upper surface of the lower conductor layer 12) is approximately 0.5 or more and approximately 1.0 or less. In addition, the via diameter of the via conductor 13 (the diameter of the via conductor 13 on the upper surface of the lower conductor layer 12 connected to the via conductor 13) is approximately 10 μm. In addition, although the term "diameter" is used, the planar shape of the via conductor 13 is not necessarily limited to a circle. "Diameter" refers to the distance between the two longest points on the outer periphery of the horizontal cross section of the via conductor 13.
[0040] Conductive layer 12 of wiring substrate 1 can include fine wiring FW as high-density wiring with relatively small wiring width and wiring distance (wiring spacing). Fine wiring FW can have the smallest wiring width and wiring distance among wirings constituting wiring substrate 1.
[0041] In the illustrated example, four of the plurality of conductor layers 12 included in first build-up unit 10 include fine wiring FW as high-density wiring. Any number of conductor layers 12 in first build-up unit 10 may include fine wiring FW. The number of conductor layers 12 including fine wiring FW in first build-up unit 10 is not limited.
[0042] Fine wiring FW included in first build-up section 10 has a smaller wiring width and wiring spacing (inter-wiring distance) than the wiring included in conductor layer (second conductor layer) 22 within second build-up section 20, described later. Specifically, for example, the minimum wiring width of fine wiring FW is 2 μm or less, and the minimum wiring spacing is 2 μm or less. Including fine wiring FW in first build-up section 10 can sometimes provide wiring with more appropriate characteristics corresponding to the electrical signals that can be transmitted by the wiring within first build-up section 10. From a similar perspective, the aspect ratio of fine wiring FW that can be included in first conductor layer 12 is, for example, 2.0 to 4.0.
[0043] When the conductor layer 12 is formed to include fine wiring FW as described above, it is sometimes preferable to also form via conductors 13 at fine pitches, connecting the opposing conductor layers 12 across the insulating layer 11. Small-diameter through-holes 11a for the via conductors 13 can be formed in the insulating layer 11. Therefore, the insulating layer 11 may contain inorganic fillers such as fine particles composed of silicon dioxide (SiO2), aluminum oxide, or mullite. However, in order to facilitate the formation of small-diameter through-holes 11a, it is sometimes preferable to exclude inorganic fillers from the insulating layer 11.
[0044] In first build-up section 10, which includes conductive layer 12 containing fine wiring FW, insulating layer 11 has a thickness of, for example, approximately 7.5 μm to 10 μm. In this case, insulating layer 11 preferably does not include a core material (reinforcement material) such as glass fiber or aramid fiber. Conductive layer 12 has a thickness of 7 μm or less.
[0045] like Figure 1 As shown, the first build-up part 10 is stacked on the second build-up part 20. That is, the second surface 10B of the first build-up part 10 is opposite to the first surface 20F of the second build-up part 20. The second build-up part 20 has insulating layers (second insulating layers) 21 and conductive layers (second conductive layers) 22 stacked alternately, similarly to the first build-up part 10. Via conductors 23 are formed in the insulating layers 21 to penetrate through the insulating layers 21 and connect the conductive layers that are opposite to each other across the insulating layers 21. Each conductive layer 22 is patterned to have a predetermined conductive pattern. As shown in FIG. Figure 1 As shown, similar to the first build-up section 10 , the second build-up section 20 does not include a core layer.
[0046] like Figure 1 As shown, second surface 20B of second build-up section 20, which is comprised of the lower surface of insulating layer 21 and the lower surface and side surfaces of conductive layer 22 of the lowest layer of second build-up section 20, faces first surface 30F of third build-up section 30. Third build-up section 30 includes insulating layer 211 and conductive layer 212 formed on its lower surface. Insulating layer 211 covers the lowermost conductive layer 22 of second build-up section 20 and the lower surface of the lowermost insulating layer 21 of second build-up section 20 not covered by conductive layer 22. Via conductor 33 is formed in insulating layer 211, penetrating insulating layer 211 and connecting conductive layer 212 to conductive layer 22 of second build-up section 20.
[0047] The insulating layer 21 constituting the second laminate portion 20 can be formed using the same insulating resin as the insulating layer 11. The insulating layer 21 may also include a core material (reinforcement material) composed of glass fiber or aramid fiber. The insulating layer 211 of the third laminate portion 30 includes a core material 21b composed of glass fiber. The insulating layers 21 and 211 may also include an inorganic filler (not shown) composed of microparticles such as silica (SiO2), alumina, or mullite. The conductor layer 22 of the second laminate portion 20 and the conductor layer 212 of the third laminate portion 30, as well as the via conductors 23 and 33, can be formed using any metal such as copper or nickel, similar to the conductor layer 12 and the via conductor 13.
[0048] As described above, the wiring width and wiring spacing of the wiring included in the conductor layer 22 of the second build-up portion 20 and the conductor layer 212 of the third build-up portion 30 are larger than the wiring width and wiring spacing of the wiring included in the conductor layer 12 of the first build-up portion 10. The thickness of the conductor layer 22 is formed to be thicker than the thickness of the conductor layer 12, for example, 10 μm or more. The conductor layer 22 of the second build-up portion 20 does not include a wiring pattern that can arrange wiring at the same fine pitch as the fine wiring FW of the first build-up portion 10. For example, the minimum wiring width of the wiring included in the conductor layer 22 is approximately 4 μm, and the minimum wiring spacing is approximately 6 μm. The via diameter of the via conductor 23 (the diameter of the via conductor 23 on the upper surface of the lower conductor layer 22 to which the via conductor 23 is connected) is approximately 50 μm.
[0049] The insulating layer 211 and conductive layer 212 of the third build-up section 30 are both thicker than the insulating layer 21 and conductive layer 22 in the second build-up section 20. For example, the thickness of the insulating layer 211 is between 100 μm and 200 μm. Furthermore, the thickness of the conductive layer 212 is approximately 20 μm. The diameter of the via-hole conductor 33 formed in the insulating layer 211 (the diameter of the via-hole conductor 33 on the upper surface of the conductive layer 212) is approximately 100 μm.
[0050] Similar to conductor layer 12 and via conductor 13, conductor layers 22, 212 and via conductors 23, 33 may also have a multilayer structure, for example, a two-layer structure including a metal film layer and a plated film layer. Second build-up section 20 and third build-up section 30 do not include fine wiring patterns like fine wiring FW of first build-up section 10. In this case, the metal film layer in the two-layer structure of conductor layer 22 and via conductor 23, and conductor layer 212 and via conductor 33 may be a chemically plated film layer formed of a chemically plated film, particularly a chemically plated copper film layer, and the plated film layer may be an electroplated film layer formed of an electroplated film, particularly an electroplated copper film layer.
[0051] exist Figure 1In the example shown in FIG. 1 , wiring substrate 1 further includes a solder resist layer 31 formed on the surfaces of insulating layer 211 and conductive layer 212. Solder resist layer 31 is formed using, for example, a photosensitive polyimide resin or epoxy resin. Openings 31 a are formed in solder resist layer 31, and conductive pads 32 p of conductive layer 212 of third build-up portion 30 are exposed through openings 31 a.
[0052] When the wiring substrate 1 itself is mounted on an external element such as an external wiring substrate (e.g., a motherboard of any electrical device), the second surface 1B of the wiring substrate 1, which is opposite to the component mounting surface of the wiring substrate 1, can be a connection surface for connection to the external element. The conductor pad 32p can be connected to any substrate, electrical component, or mechanical component. In addition, the wiring substrate 1 can have a rectangular shape with each side measuring 80 mm or more and 240 mm or less when viewed from above. In addition, "viewed from above" means observing the object with a line of sight parallel to the thickness direction of the wiring substrate 1.
[0053] Next, refer to Figures 2A to 2T , to manufacture Figure 1 The manufacturing method of the wiring substrate of the embodiment is described by taking the case of the wiring substrate 1 shown in FIG. In addition, each structural element formed in the manufacturing method described below can be used in the embodiment as long as there is no special description. Figure 1 The first build-up portion 10 is formed from the materials exemplified as the materials of the corresponding structural elements in the description of the wiring substrate 1. Furthermore, in the subsequent description of the method for manufacturing the wiring substrate 1, the side closer to the core material GS1 constituting the first support substrate SP1 is referred to as "lower" or "lower side," and the side farther from the first support substrate SP1 is referred to as "upper" or "upper side." The first build-up portion 10 is formed on the first support substrate SP1. Therefore, the surface of each element constituting the wiring substrate 1 that faces the first support substrate SP1 is referred to as the "lower surface," and the surface that faces the side opposite to the first support substrate SP1 is also referred to as the "upper surface."
[0054] The manufacturing method of the wiring substrate of the embodiment includes the following steps: manufacturing a first build-up portion 10 on the first surface SP1a of the two main surfaces (surfaces perpendicular to the thickness direction) of the first support substrate SP1, namely the first surface SP1a and the second surface SP1b; making the two manufactured first support substrates SP1 (1a, refer to Figure 2J ) The second surfaces SP1b of the respective support substrates SP1 are opposed to each other in the thickness direction of the first support substrate SP1; and the second build-up sections 20 are stacked on the first build-up sections 10. In the manufacturing method of the wiring substrate 1 described above, the third build-up section 30 is further stacked on the second build-up section 20 (see Figure 1 The two first support substrates SP1 (1a, see Figure 2J) can also be separated by the second support substrate SP2 (refer to Figure 2L ) The first supporting substrates SP1 are bonded to the second supporting substrate SP2 so that the second surfaces SP1b of the first supporting substrates SP1 face each other in the thickness direction thereof.
[0055] First, if Figure 2A As shown, a first support substrate SP1 is prepared. In the method for manufacturing a wiring substrate of the embodiment, the first support substrate SP1 used has at least one of its two surfaces perpendicular to its thickness direction, that is, the surface on which the first build-up portion 10 is formed ( Figure 2A The first surface SP1a in the first supporting substrate SP1 has good flatness. The surface of the first surface SP1a of the first supporting substrate SP1 has a flatness of, for example, ±2.5 μm or less. In addition, “flatness” here refers to an indicator that can numerically display the smoothness (uniformity) of a plane, in accordance with or in accordance with JIS B0621-1984. Therefore, a flatness of ±2.5 μm or less means that the concavity or convexity in the thickness direction of the first supporting substrate SP1 relative to the imaginary plane serving as a reference is less than 2.5 μm on each single surface. The first supporting substrate SP1 includes, for example, a core material GS1 as a glass substrate, a first metal film layer ML1 stacked on the surface of at least one surface of the core material GS1 (the surface on the first surface SP1a side of the first supporting substrate SP1), and a second metal film layer ML2 stacked on the metal film layer ML1 via an adhesive layer AL1. The first metal film layer ML1 and the second metal film layer ML2 are, for example, metal film layers formed by chemical plating or sputtering. The first metal film layer ML1 and the second metal film layer ML2 are each depicted as a single layer in the figure, but may also include a plurality of layers. For example, the first metal film layer ML1 and the second metal film layer ML2 can each have a double-layer structure consisting of a titanium layer and a copper layer. The adhesive layer AL1 can include, for example, an azobenzene-based polymer adhesive that can be attached or detached by light irradiation. In addition to a glass substrate, the first supporting substrate SP1 can also include any of a silicon substrate, a metal substrate, and a ceramic substrate as the core material GS1.
[0056] In addition, the following Figure 2A as well as Figure 2B to Figure 2T In the figure, an example of forming a single wiring substrate on the first supporting substrate SP1 is illustrated to explain the method of manufacturing a wiring substrate. However, multiple wiring substrates can be formed on the first supporting substrate SP1. Specifically, the surface of the first supporting substrate SP1 has one or more continuous product areas, and a stacked body (laminated portion) containing a wiring substrate in each product area is formed on the surface of the first supporting substrate SP1. When the first supporting substrate SP1 has multiple product areas, the wiring substrates are manufactured by dividing the formed stacked body into sections for each product area.
[0057] Then, if Figure 2BAs shown, a conductor layer 12 having a plurality of conductor pads 12p is formed on the first surface SP1a of the first support substrate SP1. In forming the conductor layer 12 in contact with the first support substrate SP1, a plating resist is formed on the metal film layer ML2, for example, and openings corresponding to the formation areas of the pattern of the conductor pads 12p are formed in the plating resist by, for example, photolithography. Next, a plated film layer is formed in the openings by electroplating using the metal film layer ML2 as a seed layer. After the plated film layer is formed, the plating resist is removed to form a Figure 2B The status shown.
[0058] Then, if Figure 2C As shown, an insulating layer 11 is stacked to cover the upper surface and side surfaces of the conductor layer 12 and the first surface SP1a of the first support substrate SP1 exposed from the conductor pattern of the conductor layer 12. As the insulating layer 11, insulating resins such as epoxy resin and phenolic resin can be used. Fluororesin, liquid crystal polymer (LCP), polyvinyl fluoride resin (PTFE), polyester resin (PE), and modified polyimide resin (MPI) can also be used. The insulating layer 11 is formed by hot pressing these resins formed into a film. Next, the via conductor 13 (see Figure 1 ) is formed at the formation position by irradiating with, for example, a carbon dioxide laser, an excimer laser, or the like to form a through hole 11a.
[0059] Although not shown in the figure, the formation of the through hole 11a based on the irradiation of a laser such as a carbon dioxide laser can be carried out by protecting the upper surface of the insulating layer 11 with a protective film such as a polyethylene terephthalate (PET) film while irradiating the laser. A through hole 11a is formed that penetrates the protective film and the insulating layer 11. In addition, after the through hole 11a is formed, a desmearing process can be performed to prevent the decrease in the adhesion during the formation of the conductor layer 12 caused by the processing modifier generated at the bottom of the through hole 11, an increase in the resistance component, etc. The desmearing process is preferably a dry desmearing process using plasma gas. The desmearing process can also be performed while protecting the surface of the insulating layer 11 while a protective film such as a polyethylene terephthalate (PET) film is formed on the surface of the insulating layer 11.
[0060] Then, if Figure 2D As shown, a metal film layer 121 is formed on the inner wall of the through hole 11a and on the surface of the insulating layer 11 by chemical plating or sputtering. Preferably, the metal film layer 121 can be a sputtered film formed by sputtering. In addition, when a protective film is provided on the surface of the insulating layer 11 during the formation of the through hole 11a and / or the desmear treatment, the protective film can be stripped and removed before the formation of the metal film layer 121.
[0061] Then, if Figure 2EAs shown, a dry film resist containing, for example, a photosensitive epoxy resin is adhered to the metal film layer 121, and the resist layer RL1 is formed in contact with the upper surface of the metal film layer 121. Next, the resist layer RL1 is exposed. In the manufacturing method of the wiring substrate of the embodiment, it is preferred to implement direct imaging exposure in the process of exposing the resist layer RL1. In the direct imaging exposure, no photomask is used, and the resist layer RL1 is directly irradiated with irradiation light L. As the light source of the irradiation light L, for example, a semiconductor laser or an ultra-high pressure mercury lamp with a wavelength of 350nm to 410nm can be used. According to the conductor pattern of the first conductor layer 12 to be formed on the insulating layer 11 (refer to Figure 2H ) corresponding to the drawing pattern, scanning the irradiation light L. In addition, the exposure amount can be determined by the illuminance of the exposure light source and the scanning speed of the irradiation light L.
[0062] Then, if Figure 2F As shown, a conductor pattern corresponding to the first conductor layer 12 to be formed on the insulating layer 11 is formed on the first resist layer RL1 (see FIG. Figure 2H Specifically, after the exposure step of the resist layer RL1 is completed, the resist layer RL1 is developed using a developer consisting of an aqueous sodium carbonate solution, for example, which may contain a surfactant, a defoaming agent, and a small amount of an organic solvent for promoting development, to form an opening RL1o. The conductor pattern of the first conductor layer 12 to be formed on the insulating layer 11 includes the wiring FW (see Figure 2H ), the opening RL1o corresponding to the wiring FW can be formed so that the minimum width of the opening is 2 μm or less, and the minimum spacing between the openings is 2 μm or less. Furthermore, in the description of the wiring substrate manufacturing method, the resist layer exposed by direct imaging exposure in forming the conductive layer 12 of the first build-up portion 10 is also referred to as the first resist layer RL1, and the resist pattern formed on the first resist layer RL1 is also referred to as the first resist pattern.
[0063] Next, if Figure 2G As shown, by electroplating the metal film layer 121 as a power supply layer, a plated film layer 122 is formed in the opening RL1o of the first resist layer RL1. The interior of the through hole 11a is completely filled with the plated film 122, forming a via conductor 13.
[0064] Next, after removing the first resist layer RL1 using an alkaline stripping solution, the portion of the metal film layer 121 not covered by the plated film layer 122 is removed by etching. Figure 2HAs shown, a conductor layer 12 having a two-layer structure composed of a metal film layer 121 and a plated film layer 122 is formed, which has fine wiring FW. The conductor layer 12 is formed to have a thickness of, for example, 7 μm or less, a minimum wiring width of the wiring FW of 2 μm or less, a minimum wiring spacing of 2 μm or less, and an aspect ratio of, for example, 2.0 to 4.0.
[0065] Then, if Figure 2I As shown, a desired number of insulating layers 11 and conductive layers 12 and via-hole conductors 13 penetrating the insulating layers are formed on the conductive layer 12 and the insulating layer 11 by the same method as the above-mentioned method of forming the insulating layer 11, the conductive layer 12 and the via-hole conductors 13.
[0066] Then, if Figure 2J As shown, the insulating layer 11 and the conductive layer 12, the topmost layers of the insulating layer 11 and the conductive layer 12 of the first build-up portion 10, are formed on the upper side of the conductive layer 12. A first support substrate SP1 (1a) is manufactured in which the first build-up portion 10 is formed on the first surface SP1a of the first support substrate SP1. By forming the first build-up portion 10 on the first surface SP1a of the first support substrate SP1 having good flatness, the conductive layer 12 in the first build-up portion 10 can have high flatness. It is also considered that problems such as positional deviation and insufficient adhesion are less likely to occur when forming the via conductor 13 connected to the conductive layer 12. A first build-up portion 10 with high connection reliability can be formed. This is considered to be particularly advantageous when the conductive layer 12 in the first build-up portion 10 includes fine wiring FW.
[0067] As described above, in the manufacturing method of the wiring substrate of the embodiment, it is preferred to use direct imaging exposure in the formation of the resist pattern of the first resist layer RL1. As a result, it is believed that the yield rate in the manufacture of the wiring substrate can be improved. Specifically, in the exposure method using a photomask, exposure is performed in units of photomasks, so the adjustment of the depth of focus is also performed only in units of photomasks. On the other hand, in direct imaging exposure, it is not necessary to use a photomask, so the depth of focus can be adjusted in units of exposure beams. Therefore, it is believed that by implementing direct imaging exposure in the formation of the conductor layer 12 that can include relatively fine wiring FW, the resolution of the resist pattern is excellent compared to the case where exposure using a photomask is implemented.
[0068] In the manufacturing method of the wiring substrate, the product areas on the surface of the first supporting substrate SP1 each have a rectangular shape with each side having a size of 80 mm or more and 240 mm or less when viewed from above. Therefore, the laminate (laminated portion) formed within the range of one or more product areas of the first supporting substrate SP1 has a rectangular shape with each side having a size of 80 mm or more when viewed from above. In this way, in the case of manufacturing a laminate of a relatively large size, in the exposure using a photomask whose range that can be exposed in one exposure is limited, it is necessary to repeatedly perform exposure in different ranges, and sometimes the working hours in the exposure process increase. In contrast, in direct imaging exposure, the entire range of the wiring substrate is scanned by the irradiation light in one exposure, so that the increase in the working hours in the exposure process can be suppressed, and therefore, the manufacturing yield of the wiring substrate can sometimes be improved.
[0069] As shown in the figure, the uppermost conductive layer 12 does not include wiring FW. In this case, the conductive layer 12 can be formed by a method including forming a resist pattern by exposing the resist layer using a photomask. Alternatively, the uppermost conductive layer 12 not including wiring FW can be formed by the same method as that used to form the insulating layer 11 and the conductive layer 12 on the insulating layer 11 (including a method of direct image exposure of the resist layer).
[0070] Furthermore, in the method for manufacturing a wiring substrate according to the embodiment, any of the plurality of conductive layers 12 constituting first build-up portion 10 may be formed by a method including direct imaging exposure of a resist layer. Thus, for example, in the illustrated example, the lowermost conductive layer 12 (the conductive layer 12 in contact with first support substrate SP1) in first build-up portion 10 that does not include wiring FW may be formed by a method including forming a resist pattern by exposing the resist layer using a photomask, or may be formed by a method including direct imaging exposure.
[0071] Then, if Figure 2K As shown, the second build-up portion 20 is stacked on the uppermost insulating layer 11 and the conductive layer 12 in the first build-up portion 10 (see FIG. Figure 2R ). The insulating layer 21a is formed of the same insulating resin as that constituting the insulating layer 11. A film 21b formed of a resin such as polyethylene terephthalate is laminated on the insulating layer 21a and is releasably bonded to the insulating layer 21a.
[0072] In the method for manufacturing the wiring board of the embodiment, the first support substrate SP1 (1a) on which the first buildup portion 10 having the insulating layer 21a and the film 21b is laminated is then attached to the second support substrate SP2. Figure 2LAs shown, the first support substrate SP1 (1a) laminated with the first laminated portion 10 is pasted on both sides of the two main surfaces (surfaces perpendicular to the thickness direction) of the second support substrate SP2. The second support substrate SP2, for example, includes a glass substrate, i.e., a core material GS2, which is the same as the core material GS1 of the first support substrate SP1. Alternatively, the second support substrate SP2 may also use a CCL (Copper Clad Laminate), a double-sided copper-clad laminate comprising an insulating layer and copper foil hot-pressed on both sides thereof. The main surface of the second support substrate SP2 is bonded to the second surface SP1b of the first support substrate SP1. For example, the bonding can be performed via an adhesive layer AL2 composed of any adhesive such as an epoxy-based or acrylic-based resin. However, the two first support substrates SP1 (1a) laminated with the first laminated portion 10 may be placed opposite each other by bonding the respective second surfaces SP1b to each other using the same adhesive without passing through the second support substrate SP2.
[0073] Next, the film 21b is peeled off from the insulating layer 21a on both main surfaces of the second supporting substrate SP2. Thereafter, the insulating layer 21a is thermally cured. As a result, Figure 2M As shown, the second laminated portion 20 (see Figure 2R ) is formed on the uppermost insulating layer 11 and the conductive layer 12 of the first buildup portion 10. Figure 2C as well as Figure 2D The through hole 21 a is formed by the same method as the formation of the through hole 11 a and the formation of the metal film layer 121 described above, and the metal film layer 221 is formed on the upper surface of the insulating layer 21 and the inner surface of the through hole 21 a.
[0074] In addition, Figure 2M And the following references Figure 2N to Figure 2R In the figure, the laminate formed on one surface of the second support substrate SP2 is shown, and the laminate that can be formed on the opposite surface is omitted. However, on the opposite surface of the second support substrate SP2, laminates of the same form and number are also formed simultaneously with the formation of the second and third build-up sections on the illustrated surface.
[0075] Next, if Figure 2N As shown, a resist layer RL2 is formed on the metal film layer 221. Next, the resist layer RL2 is exposed. During the exposure process of the resist layer RL2, exposure using a photomask M can be performed. Alternatively, direct imaging exposure can be performed during the exposure process of the resist layer RL2. In this case, compared to the direct imaging exposure performed during the exposure process of the resist layer RL1, direct imaging exposure can be performed, resulting in a larger beam spot diameter and a lower resolution of the formed resist pattern.
[0076] Then, if Figure 2O As shown, the above reference Figure 2F The resist layer RL2 is developed using a developer in the same manner as the development of the first resist layer RL1 described above, and a conductive pattern corresponding to the second conductive layer 22 is formed (see FIG. Figure 2Q ) corresponding to the resist pattern. Specifically, an opening RL2o is formed corresponding to the conductor pattern of the second conductor layer 22 to be formed. When the conductor pattern of the second conductor layer 22 to be formed on the insulating layer 21 includes wiring, the opening RL2o corresponding to the wiring can be formed so that the minimum opening width is approximately 4 μm and the minimum opening spacing is approximately 6 μm. In addition, the resist layer used to form the conductor layer 22 is also referred to as the second resist layer RL2, and the resist pattern formed in the second resist layer RL2 is also referred to as the second resist pattern.
[0077] Then, if Figure 2P As shown, by electroplating the metal film layer 221 as a power supply layer, a plated film layer 222 is formed in the opening RL2o of the second resist layer RL2. The interior of the through hole 21a is completely filled with the plated film 222, forming a via conductor 23.
[0078] Next, after removing the second resist layer RL2 using a stripping solution, the portion of the metal film layer 221 not covered by the plated film layer 222 is removed by etching. Figure 2Q As shown, a second conductor layer 22 having a two-layer structure consisting of a metal film layer 221 and a plated film layer 222 is formed. The second conductor layer 22 can be formed to have a thickness of, for example, 10 μm or greater. The second conductor layer 22 can be formed to have wiring with a minimum wiring width of approximately 4 μm and a minimum wiring spacing of approximately 6 μm.
[0079] Then, if Figure 2R As shown, by repeatedly performing the steps of forming the above-mentioned insulating layer 21, the conductive layer 22, and the via-hole conductor 23, the desired number of insulating layers 21 and conductive layers 22 and the via-hole conductor 23 penetrating each insulating layer 21 are formed. The second build-up portion 20 is formed on the first build-up portion 10. In the formation of the first build-up portion 10 and the second build-up portion 20, the minimum value of the wiring width of the wiring FW in the first conductive layer 12 is smaller than the minimum value of the wiring width of the wiring in the second conductive layer 22, and the minimum value of the wiring spacing of the wiring FW in the first conductive layer 12 is smaller than the minimum value of the wiring spacing of the wiring in the second conductive layer 22. In addition, in Figure 2R And the following Figure 2S as well as Figure 2T In the figure, the metal film layers 121, 221 and the plated film layers 122, 222 are not depicted. The conductor layers 12, 22 and Figure 1 Likewise depicted as a single layer.
[0080] As described above, in the method for manufacturing wiring substrate 1, second build-up section 20 having conductive layer 22 with a relatively gentle wiring pattern relative to first build-up section 10 is stacked on first build-up section 10, subsequent to stacking of first build-up section 10 onto first supporting substrate SP1. Therefore, compared to a manufacturing method in which first and second build-up sections 10, which are formed separately, are joined via a connecting member, manufacturing can be performed with fewer steps.
[0081] Then, if Figure 2S As shown, the insulating layer 211, the conductive layer 212, and the via conductor 33 penetrating the insulating layer 211 of the third buildup part 30 are formed on the top insulating layer 21 and the conductive layer 22 of the second buildup part 20 by the same method as the method for forming the insulating layer 21, the conductive layer 22, and the via conductor 23. As the insulating resin forming the insulating layer 211, a prepreg containing an insulating resin such as epoxy resin or BT resin impregnated in a reinforcing material (core material) 21b composed of glass fiber is used. That is, as Figure 2S As shown, on the two main surfaces of the second support substrate SP2, the first support substrate SP1 (1a) on which the first build-up portion 10 is stacked, the second build-up portion 20, and the third build-up portion 30 are formed in this order from the second support substrate SP2. Next, a solder resist layer 31 is formed by forming a photosensitive epoxy resin or polyimide resin layer on the surfaces of the insulating layer 211 and the conductive layer 212. Then, openings 31a are formed to define the conductive pads 32p using photolithography.
[0082] Then, if Figure 2T As shown in FIG. 1 , the first support substrate SP1 and the second support substrate SP2 can be removed from the adhesive layer AL1 together with the laminate including the first buildup portion 10. Figure 2T Although not shown in the figure, the removal of the first support substrate SP1 can be performed on the first support substrate SP1 on both sides of the second support substrate SP2. The lower surface of the second metal film layer ML2 under the conductor pad 12p is exposed. In the removal of the first support substrate SP1, for example, after the adhesive layer AL1 is irradiated with a laser to soften it, the second metal film layer ML2 of the first support substrate SP1 is peeled off. Then, the second metal film layer ML2 is removed by etching to expose the lower surface of the conductor pad 12p and the lower surface of the insulating layer 11. In addition, the stacked body that can include a plurality of wiring substrates can be divided into individual independent wiring substrates according to each product area. Completion Figure 1 The wiring substrate 1 is shown.
[0083] In the method for manufacturing a wiring substrate according to the embodiment, first, a high-quality first build-up section 10 with high flatness is formed on a first supporting substrate SP1. After the second surfaces SP1b of two first supporting substrates SP1 (1a) each having the first build-up section 10 stacked thereon are opposed to each other, the second build-up section 20 and the third build-up section 30 are stacked on each of the first build-up sections 10. It is believed that the manufacturing yield of the wiring substrate is improved, and high-quality wiring substrates 1 can be manufactured efficiently with a high yield.
[0084] The manufacturing method of the wiring substrate of the embodiment is not limited to the Figures 2A to 2T The conditions, sequence, etc. of the described method can be arbitrarily changed. Furthermore, certain steps may be omitted, and other steps may be added. For example, a solder resist layer having an opening exposing the conductor pad 12p may be formed on the conductor pad 12p and the insulating layer 11 exposed after the second metal film layer ML2 is removed by etching. Furthermore, a conductor bump connected to the conductor pad 12p may be formed within the opening of the solder resist layer. A plating layer including a nickel layer and a tin layer may also be formed on the surface of the conductor bump.
Claims
1. A method for manufacturing a wiring substrate, comprising the following steps: preparing two first support substrates having a first surface and a second surface opposite to the first surface and having one or more product areas; forming first build-up portions including the first conductive layer and the first insulating layer by alternately stacking first conductive layers and first insulating layers within the one or more product regions on the first surface of each first support substrate; as well as The second build-up portion is formed by placing the second surfaces of the two first support substrates opposite to each other in the thickness direction of the first support substrate and alternately stacking second conductive layers and second insulating layers on the side of each first build-up portion opposite to the first support substrate. in, The step of stacking the first conductor layer includes the steps of: forming a first resist layer having a first resist pattern and forming a conductor pattern according to the first resist pattern; The step of forming a first resist layer having the first resist pattern comprises the following steps: exposing the first resist layer by direct imaging exposure, The first and second conductor layers are formed so that the minimum wiring width and the minimum wiring interval of the wiring in the first conductor layer are smaller than the minimum wiring width and the minimum wiring interval of the wiring in the second conductor layer, respectively.
2. The method for manufacturing a wiring substrate according to claim 1, wherein: The step of making the second surfaces of the two first support substrates face each other includes the step of bonding the two first support substrates to the second support substrate via the second support substrate.
3. The method for manufacturing a wiring substrate according to claim 2, wherein: The method for manufacturing a wiring substrate further includes the step of removing the first support substrate together with the second support substrate after forming the second build-up portion.
4. The method for manufacturing a wiring substrate according to claim 1, wherein: The step of stacking the second conductor layer includes the steps of: forming a second resist layer having a second resist pattern and forming a conductor pattern according to the second resist pattern; The step of forming the second resist layer having the second resist pattern includes exposing the second resist layer using a photomask.
5. The method for manufacturing a wiring substrate according to claim 1, wherein: Each of the product areas has a rectangular shape with each side being not less than 80 mm and not more than 240 mm in a plan view.
6. The method for manufacturing a wiring substrate according to claim 1, wherein: The flatness of the first surface of the first support substrate is ±2.5 μm or less.
7. The method for manufacturing a wiring substrate according to claim 6, wherein: The first supporting substrate is selected from any substrate selected from a glass substrate, a silicon substrate, a metal substrate, and a ceramic substrate.
8. The method for manufacturing a wiring substrate according to claim 1, wherein: The step of stacking the first conductor layer includes the step of setting the minimum value of the width of the wiring included in the conductor pattern to be 2 μm or less and setting the minimum value of the spacing between the wirings to be 2 μm or less.
9. The method for manufacturing a wiring substrate according to claim 1, wherein: The thickness of the first conductor layer is formed to be less than 7 μm. The second conductive layer is formed to have a thickness of 10 μm or more.
10. The method for manufacturing a wiring substrate according to claim 1, wherein: The first conductive layer is formed to include wiring having an aspect ratio of 2.0 to 4.
0.
11. The method for manufacturing a wiring substrate according to claim 1, wherein: The method for manufacturing a wiring substrate further includes forming a third build-up section by alternately stacking a third insulating layer and a third conductive layer on a side of the second build-up section opposite to the first build-up section.
12. The method for manufacturing a wiring substrate according to claim 1, wherein: The step of forming the second buildup portion includes forming the second insulating layer on each of the first buildup portions on each of the first support substrates before the second faces are opposed to each other.
Citation Information
Patent Citations
Wiring board and manufacturing method thereof
JP2020004926A