Steel part and machining method thereof

Through gradient temperature vacuum quenching, double tempering and tempering treatment, combined with segmented nitriding to control temperature and nitrogen potential, the problem of uneven nitriding layer of steel parts after turning is solved, the hardness and depth of the nitriding layer are improved, and efficient and low-cost processing effects are achieved. It is suitable for key components of medium and low-speed marine diesel engines.

CN120719244APending Publication Date: 2025-09-30CHONGQING HONGJIANG MACHINERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510952002.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-10
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

When steel parts after traditional turning are directly gas nitrided, the hardness of the nitrided layer is uneven and the depth is insufficient, which affects product performance, reduces production efficiency, and increases costs.

Method used

Adopt gradient temperature vacuum quenching, double tempering and quenching and tempering treatment, combined with staged nitriding to control temperature and nitrogen potential, use tetrachloroethylene and ammonia to treat the surface, and high-purity nitrogen slightly positive pressure cooling to ensure the uniformity and depth of the nitriding layer.

Benefits of technology

The uniformity of hardness and depth of the nitriding layer is achieved, production efficiency is improved, processing costs are reduced, and the performance requirements of key components of marine medium and low-speed diesel engines are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120719244A_ABST
    Figure CN120719244A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material machining, in particular to a steel part and a machining method thereof.The method comprises the steps that rough machining, vacuum quenching, tempering treatment, thermal refining, turning finish machining and nitriding treatment are sequentially conducted on a blank; the vacuum quenching adopts a gradient heating mode, and nitrogen is adopted for quenching; the nitriding treatment comprises the following steps that S1, the temperature of the part obtained after finish machining is increased to 350 + / -5 DEG C, meanwhile, tetrachloroethylene liquid and ammonia gas are introduced, and heat preservation is conducted for preset time; s2, the temperature is set to be 520 + / -5 DEG C, meanwhile, ammonia gas is introduced, the nitrogen potential factor is set to be 10, and heat preservation is conducted for 1-2 h; s3, the temperature is set to be 540 + / -5 DEG C, the nitrogen potential factor is set to be 0.8-1.0, and heat preservation is conducted for 20 + / -1 h; s4, the nitrogen potential factor is set to be 0.5-0.6, and heat preservation is conducted for 40 + / -1 h; and S5, cooling to room temperature to obtain a finished product. The problem that the effect is not ideal due to the fact that gas nitriding is directly carried out after turning of the steel part can be solved, and then turning replaces grinding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material processing, in particular to a steel part and a processing method thereof. Background Art

[0002] In the field of medium- and low-speed marine diesel engines, key components such as valve housings and needle valve bodies are often machined from 4Cr5MoSiV1. Because the working surfaces of these components must possess excellent wear resistance, gas nitriding has become the mainstream surface strengthening treatment. Long-term practice has shown that traditional processes require rough grinding of the working surfaces prior to nitriding, requiring a three-station grinder. This not only results in high processing costs but also significantly limits production efficiency. Therefore, the need for turning to replace grinding is becoming increasingly urgent.

[0003] However, production data shows that when gas nitriding is directly performed on workpieces after turning, the process has significant defects, namely, the hardness of the nitriding layer is unevenly distributed and overall low, and the uniformity of the depth of the nitriding layer is difficult to guarantee, which seriously affects the performance of the product. Summary of the Invention

[0004] The purpose of the present invention is to provide a steel part and a processing method thereof, which can solve the problem that the gas nitriding effect is not ideal when the steel part is directly subjected to turning processing, thereby realizing turning processing instead of grinding processing, improving processing efficiency, reducing processing costs, and meeting the performance requirements of the steel part.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for processing steel parts, comprising: sequentially performing rough processing, vacuum quenching, tempering, quenching and tempering, turning finishing, and nitriding on a blank; The vacuum quenching adopts a gradient temperature rising method and uses nitrogen for quenching; The nitriding treatment comprises the following steps: S1, heat the machined parts to 350±5℃, introduce tetrachloroethylene liquid and ammonia gas at the same time, and keep the temperature for the preset time; S2, set the temperature to 520±5℃, introduce ammonia gas, set the nitrogen potential factor to 10, and keep warm for 1-2 hours; S3, set the temperature to 540±5℃, the nitrogen potential factor to 0.8-1.0, and keep warm for 20±1h; S4, set the nitrogen potential factor to 0.5-0.6 and keep warm for 40 ± 1 h; S5, cooling to room temperature to obtain a finished product.

[0006] Furthermore, the vacuum quenching specifically includes: in a vacuum state, keeping the rough-machined parts at a temperature of 650±10°C for 50 to 60 minutes, then heating them to 850±5°C and keeping them for 50 to 60 minutes, and finally heating them to 1000±5°C and keeping them for 90 to 120 minutes, and then quenching them with nitrogen at a pressure of 15 to 18 bar, and cooling them to below 60°C before taking them out of the furnace.

[0007] Furthermore, the tempering treatment includes: transferring the parts into a tempering furnace for a first tempering treatment within a preset time after vacuum quenching, and performing a second tempering treatment after air cooling to room temperature.

[0008] Furthermore, the temperature of the first tempering treatment is set to 550±5°C, and the holding time is set to 120-150 minutes; The temperature of the second tempering treatment is set to 595±5°C, and the holding time is set to 120-150 minutes.

[0009] Furthermore, the S1 specifically includes: Heat the finished parts to 350±5℃, and simultaneously introduce AL / min of tetrachloroethylene liquid and 5~10L / min of ammonia gas, keep warm for 3~5 minutes, then simultaneously introduce BL / min of tetrachloroethylene liquid and 5~10L / min of ammonia gas, and keep warm for 3~5 minutes; A=4.5×total surface area of ​​parts+20; B=4.5×total surface area of ​​parts+30.

[0010] Furthermore, the S4 specifically includes: introducing high-purity nitrogen to maintain a slightly positive pressure in the furnace, cooling the furnace for 2 hours, then air-cooling to below 120° C., taking the furnace out of the furnace and air-cooling to room temperature to obtain the finished product.

[0011] Furthermore, the nitrogen purity is ≥99.99%; The micro-positive pressure is 50-500 Pa, that is, the pressure inside the furnace is 50-500 Pa higher than the external atmospheric pressure.

[0012] Furthermore, before the nitriding treatment is performed, high-purity nitrogen is introduced into the nitriding furnace to exhaust the air in the nitriding furnace.

[0013] In a second aspect, the present invention discloses a steel part, which is manufactured using the above-mentioned steel part processing method.

[0014] The present invention has the following unexpected beneficial effects: 1. The present invention's steel parts processing method pre-treats rough-machined parts through vacuum quenching, tempering, and quenching and tempering, improving material hardness and microstructure uniformity. This allows for a more consistent surface roughness during finishing by turning, avoiding the high cost and low efficiency of grinding. Furthermore, the matrix structure after vacuum quenching, tempering, and quenching and tempering provides a foundation for uniform growth of the nitride layer, addressing the shortcomings of conventional direct nitriding after turning.

[0015] 2. The processing method of steel parts described in the present invention fundamentally solves the problem of unstable nitriding quality after turning instead of grinding through a combined design of pretreatment optimization of the matrix and segmented nitriding precise temperature and potential control. While improving the wear resistance and dimensional stability of the parts, it significantly reduces production costs and improves production efficiency. It has practical application value in the manufacture of key components of marine medium and low-speed diesel engines. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the specific implementation of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the implementation or prior art description. Obviously, the drawings described below are only some embodiments of the present invention.

[0017] Figure 1 A schematic flow chart of a method for processing steel parts according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0018] The following describes the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art will readily appreciate the other advantages and benefits of the present invention from the disclosure herein. The present invention may also be implemented or applied through various other specific embodiments, and the various details in this specification may be modified or altered based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are intended only to illustrate the present invention and are not intended to limit the scope of protection of the present invention.

[0019] In one embodiment, the present invention provides a method for processing steel parts. Figure 1 As shown, the method includes: performing rough machining, vacuum quenching, tempering, quenching and tempering, turning finishing and nitriding on the blank in sequence.

[0020] The vacuum quenching adopts a gradient temperature rising method and uses nitrogen for quenching.

[0021] In this embodiment, gradient vacuum quenching (nitrogen quenching) reduces internal stress in the material, avoiding the oxidation and deformation problems associated with traditional quenching. Tempering and quenching further refine the grain size and homogenize the microstructure, providing a stable matrix for subsequent nitriding and fundamentally improving the bond strength between the nitride layer and the substrate. Conventional processes currently rely solely on rough grinding without systematic heat treatment to optimize the substrate, resulting in insufficient bonding between the nitride layer and the substrate. This solution, however, enhances the toughness of the substrate through multiple heat treatment steps, significantly improving the load-bearing capacity of the nitride layer.

[0022] The machining method for steel parts disclosed herein pre-treats the rough-machined parts through vacuum quenching, tempering, and quenching and tempering. This improves material hardness and microstructure uniformity, enabling a more stable surface roughness during finishing by turning, while avoiding the high cost and low efficiency of grinding. Furthermore, the matrix structure after vacuum quenching, tempering, and quenching and tempering provides a foundation for uniform growth of the nitride layer, addressing the shortcomings of conventional nitriding methods that are performed directly after turning.

[0023] The nitriding treatment comprises the following steps: S1: The finished part is heated to 350±5°C while tetrachloroethylene liquid and ammonia gas are introduced and held for a preset time. This low-temperature preheating at 350±5°C slowly removes gases and impurities adsorbed on the part surface while initially activating the matrix, preparing it for nitrogen diffusion. Compared to traditional nitriding with a direct heating step, this step reduces stress concentration caused by sudden temperature changes and prevents part deformation.

[0024] The Cl element produced by the decomposition of tetrachloroethylene (C2Cl4) can react with surface oxides (such as Fe2O3) to form volatile chlorides (such as FeCl3), which purify the surface, expose fresh metal surfaces, and promote nitrogen adsorption. Furthermore, the Cl element acts as a "catalyst," lowering the nitriding temperature, shortening the nitriding time, and increasing the diffusion rate of nitrogen atoms. Ammonia (NH3) provides a nitrogen source, making it easier to decompose active nitrogen atoms on the cleaned surface.

[0025] In step S2, set the temperature to 520±5°C while introducing ammonia gas. The nitrogen potential factor is set to 10, and the temperature is maintained for 1-2 hours. 520±5°C is the ideal temperature range for nitriding, ensuring sufficient diffusion capacity for nitrogen atoms while preventing overheating and growth of the matrix. Setting the nitrogen potential factor (reflecting the concentration of nitrogen atoms in the atmosphere) to 10 quickly forms a nitrogen-rich layer on the part surface, increasing the initial hardness of the nitrided layer and providing support for subsequent deep nitriding. This also shortens the overall nitriding time and improves production efficiency.

[0026] In step S3, set the temperature to 540±5°C, the nitrogen potential factor to 0.8–1.0, and maintain the temperature for 20±1h. Raising the temperature to 540±5°C accelerates the diffusion of nitrogen atoms into the substrate, increasing the depth of the nitride layer. Lowering the nitrogen potential factor to 0.8–1.0 prevents excessive precipitation of brittle phases (such as Fe₄N) due to high surface nitrogen concentrations, thereby ensuring the toughness of the nitride layer. This step achieves the dual goals of deep diffusion and microstructure optimization through the combination of high temperature and low nitrogen potential.

[0027] In traditional processes, the depth of the nitriding layer is uneven, mostly due to the single control of nitrogen potential and temperature. However, this step allows nitrogen atoms to diffuse evenly in the substrate through precise temperature control and nitrogen potential adjustment, avoiding local over-nitriding or under-nitriding.

[0028] S4: Set the nitrogen potential factor to 0.5-0.6 and hold the temperature for 40±1h. This step further reduces the nitrogen potential to 0.5-0.6, slowing the penetration rate of surface nitrogen atoms and promoting the diffusion of internal nitrogen atoms to the surface, forming an ideal nitride layer structure with "high surface hardness + internal gradient transition." Long-term heat preservation (40±1h) allows the alloy nitrides (such as CrN and MoN) in the nitride layer to precipitate and refine uniformly, significantly improving hardness uniformity. Refined alloy nitrides are key to wear resistance. This step can improve the overall hardness of the nitride layer and make the hardness gradient along the depth direction smoother, avoiding the formation of localized softening zones.

[0029] S5, cooling to room temperature to obtain the finished product. Cooling can reduce the thermal stress between the nitride layer and the substrate, avoid cracking or peeling, and ensure the dimensional stability of the finished product.

[0030] As a preferred embodiment of the present invention, the vacuum quenching process specifically involves holding the rough-machined part at 650±10°C for 50-60 minutes under vacuum. At this temperature (650±10°C), carbides (such as Cr and Mo carbides) in the blank begin to slowly dissolve, and internal stresses in the material are initially released. This temperature is below the austenitization temperature, preventing structural inhomogeneity caused by premature austenitization and establishing uniform matrix conditions for subsequent heating.

[0031] Then raise the temperature to 850±5°C and hold for 50-60 minutes. At 850±5°C, which is close to the austenitizing temperature, carbides dissolve further and more evenly, while austenite grains begin to slowly form. This holding time (50-60 minutes) ensures that carbon and alloying elements diffuse fully into the matrix, reducing component segregation and avoiding local hardness differences after quenching.

[0032] Finally, the temperature is raised to 1000±5°C and held for 90–120 minutes. 1000±5°C reaches the complete austenitization temperature, at which point carbides are almost completely dissolved and the austenite composition is homogenized. Holding for 90–120 minutes ensures a moderate grain size, avoids overheating that can lead to coarsening, and lays the foundation for obtaining a fine martensite structure during subsequent quenching. This gradient heating method avoids the thermal stress concentration caused by rapid heating in traditional quenching processes, reduces the risk of billet deformation and cracking, and improves workpiece dimensional stability during subsequent finishing (such as turning instead of grinding), thereby reducing scrap rates.

[0033] The steel is then quenched with nitrogen at a pressure of 15-18 bar and cooled to below 60°C before being removed from the furnace. The cooling rate of nitrogen, which is between that of oil quenching and air quenching, ensures that the supercooled austenite of 4Cr5MoSiV1 steel quickly passes through the "nose" region, preventing pearlite or bainite transformation, while also reducing quenching internal stresses by controlling the cooling rate. Cooling to below 60°C before removal from the furnace ensures that the martensitic transformation is fully completed, resulting in a high-hardness martensitic matrix. This provides a strong support for the nitrided layer and prevents surface spalling caused by insufficient matrix strength after nitriding.

[0034] After vacuum quenching, tempering and quenching and tempering can eliminate quenching stress and obtain a tempered sorbite structure, which not only ensures matrix strength but also provides good cutting performance for finishing. In this case, turning instead of grinding can reduce tool wear and improve processing efficiency.

[0035] In this preferred embodiment, a gradient temperature increase is combined with a high-pressure nitrogen quenching process to uniformly distribute the alloy elements in the matrix. These elements have a strong affinity with nitrogen and can promote the uniform precipitation of nitrides during nitriding, thereby improving the hardness and depth uniformity of the nitrided layer.

[0036] As a preferred embodiment of the present invention, the tempering treatment includes: transferring the parts into a tempering furnace for a first tempering treatment within a preset time after vacuum quenching, and performing a second tempering treatment after air cooling to room temperature.

[0037] In this preferred embodiment, the first tempering treatment rapidly eliminates quenching stresses. Following vacuum quenching, the material is immediately transferred to the tempering furnace, illustratively for a preset time of 30 minutes. This prevents the retained austenite from stabilizing due to aging over time, which could hinder subsequent stress release. During this period, the martensite lattice distortion has not yet "frozen," allowing carbon atoms to diffuse easily during tempering, effectively eliminating quenching stresses. Air cooling to room temperature prevents carbide aggregation caused by slow cooling and maintains matrix toughness.

[0038] The second tempering treatment deeply stabilizes the microstructure and stresses. The second tempering temperature, higher than the first, further decomposes the retained austenite and uniformly precipitates fine carbides, strengthening the matrix. This stage eliminates residual stress and significantly reduces deformation caused by stress release during nitriding.

[0039] Traditional single tempering results in high residual stress. The localized stress release during nitriding causes inconsistent nitrogen diffusion rates, with faster diffusion in areas of concentrated stress and slower diffusion in areas of low stress, resulting in variations in the depth of the nitride layer. Double tempering in this preferred embodiment achieves uniform stress distribution in the substrate, improving the consistency of nitrogen diffusion rates and ensuring uniform depth of the nitride layer.

[0040] If retained austenite is not fully decomposed, it will transform into bainite during nitriding, accompanied by volume expansion, causing microcracks in the nitrided layer. Double tempering minimizes retained austenite, avoiding these defects and enabling the surface roughness Ra of the nitrided layer to be controlled below 0.8μm, meeting the wear resistance requirements of the working surface.

[0041] As a preferred embodiment of the present invention, the temperature of the first tempering treatment is set to 550±5°C, and the holding time is set to 120~150min; the temperature of the second tempering treatment is set to 595±5°C, and the holding time is set to 120~150min.

[0042] This preferred embodiment obtains tempered troostite with uniform distribution of fine-grained carbides through the dual-temperature strategy of "low-temperature decomposition + high-temperature stabilization" and precise holding time control, providing low-stress and easy-to-process matrix conditions for turning instead of grinding, and providing an ideal matrix for the nitriding layer. It is particularly suitable for the mass production of precision parts such as marine diesel engine valve housings and needle valve bodies, and meets the industrial needs of high efficiency and low cost.

[0043] As a preferred embodiment of the present invention, S1 specifically includes: heating the finished part to 350±5°C, simultaneously introducing AL / min of tetrachloroethylene liquid and 5-10L / min of ammonia gas, keeping warm for 3-5 minutes, and then simultaneously introducing BL / min of tetrachloroethylene liquid and 5-10L / min of ammonia gas, and keeping warm for 3-5 minutes; A=4.5×total surface area of ​​the part+20; B=4.5×total surface area of ​​the part+30.

[0044] This preferred embodiment introduces a low amount of tetrachloroethylene (value A) during the first pass, gently activating the surface and preventing excessive corrosion. A higher amount (value B) is then introduced during the second pass to further remove the residual oxide layer. Simultaneously, these two activations create a "rough-to-dense" surface microstructure, increasing the nitriding contact area and improving nitrogen atomic adsorption efficiency. By adjusting the Cl / N ratio in stages, surface decarburization or corrosion caused by a single high Cl concentration can be avoided, while ensuring that nitrogen atoms penetrate at an appropriate rate during the initial nitriding phase, preventing the formation of a loose layer on the surface.

[0045] It should be noted that the surface area is expressed in m 2 That is, to calculate in square meters, just take the numerical value.

[0046] As a preferred embodiment of the present invention, S4 specifically includes: introducing high-purity nitrogen to maintain a slightly positive pressure in the furnace, cooling the furnace for 2 hours, then air-cooling to below 120°C, taking the furnace out of the furnace and air-cooling to room temperature to obtain the finished product.

[0047] Slow cooling over a two-hour period can reduce the thermal stress between the nitride layer and the substrate, preventing brittle cracking of the nitride layer caused by rapid cooling, especially the propagation of microcracks in the compound layer. Slow cooling allows the supersaturated nitrogen atoms in the nitride layer to fully precipitate, forming a uniform nitride, avoiding nitrogen atom segregation caused by rapid cooling and improving the hardness uniformity of the nitride layer.

[0048] Air-cool to below 120℃ before taking out of the oven to avoid the water vapor in the air reacting with the surface of high-temperature parts to form rust, and to prevent new stress on the parts due to sudden changes in ambient temperature.

[0049] High-purity nitrogen is introduced into the furnace to maintain a slightly positive pressure, effectively isolating the outside air and preventing oxidation of the nitride layer surface during the cooling process, thereby maintaining surface finish and nitride layer integrity. Furthermore, the nitrogen atmosphere maintains the nitrogen potential within the furnace, preventing nitrogen atoms in the nitride layer from back-diffusion and precipitation due to the decrease in the ambient nitrogen potential during cooling, thereby ensuring the stability of the nitride layer depth and hardness.

[0050] As a preferred embodiment of the present invention, the nitrogen purity is ≥99.99%; the slightly positive pressure is 50-500 Pa, that is, the pressure in the furnace is 50-500 Pa higher than the external atmospheric pressure.

[0051] Slightly positive pressure creates an "air curtain" effect, preventing outside air (including oxygen and moisture) from entering the furnace. This is especially true during the cooling or unloading phases. If the furnace is under negative pressure, outside air can easily be sucked back into the furnace, leading to surface oxidation of parts. The slightly positive pressure design effectively avoids this problem, ensuring that parts remain protected by an inert atmosphere throughout the cooling process.

[0052] The slightly positive pressure environment also promotes more uniform nitrogen circulation within the furnace, enhancing the heat exchange efficiency between the gas and the part surface, thereby improving the uniformity of the temperature field within the furnace. For example, during the furnace cooling phase, the uniform airflow prevents parts from cooling too quickly or too slowly in certain areas, reducing the risk of deformation or cracking caused by thermal stress.

[0053] As a preferred embodiment of the present invention, before the nitriding treatment is performed, high-purity nitrogen is introduced into the nitriding furnace to exhaust the air in the nitriding furnace.

[0054] This preferred implementation eliminates the risk of oxidation. Nitriding treatments are typically performed at temperatures above 500°C. If air remains in the furnace, oxygen reacts with elements like Fe and Cr on the part surface to form an oxide film, which not only damages the surface finish but also hinders the adsorption of nitrogen atoms, preventing the formation of the nitride layer or significantly reducing its uniformity. Introducing high-purity nitrogen (≥99.99%) can reduce the oxygen content in the furnace to below 0.1%, completely eliminating the risk of oxidation.

[0055] In addition, residual air will lead to unstable nitrogen potential in the furnace, affecting the nitriding rate and layer depth uniformity. By replacing with high-purity nitrogen, the nitrogen potential in the furnace can be quickly stabilized at the target value, allowing nitrogen atoms to penetrate the surface of the part at a constant rate, avoiding the deviation of the nitriding layer thickness caused by nitrogen potential fluctuations. In one embodiment, the present invention discloses a steel part, which is manufactured using the above-mentioned steel part processing method.

[0056] Specifically, after rough processing, φ60 4Cr5MoSiV1 round steel is heated and gas quenched in a vacuum high-pressure gas quenching furnace. First, vacuum is drawn, then the temperature is raised to 650±10℃ and kept for 50-60 minutes, then raised to 850±5℃ and kept for 50-60 minutes, and finally raised to 1000±5℃ and kept for 90-120 minutes. Then, it is quenched with 15-18 bar nitrogen and cooled to below 60℃ before being taken out of the furnace.

[0057] Within half an hour after being taken out of the furnace, transfer it to a vacuum tempering furnace and temper it at a temperature of 550±5℃ for 120~150min, and then temper it at a temperature of 595±5℃ for 120~150min. After each tempering, use a blower to cool it to room temperature.

[0058] After tempering is completed, it is subjected to quenching and tempering treatment, then the machine is turned for semi-finishing, the working parts are finished by turning, and then gas nitriding treatment is carried out.

[0059] Before gas nitriding, clean all parts thoroughly. Place the parts in a frame and place them in the furnace. Once in the furnace, introduce 2-3 times the volume of high-purity nitrogen to expel all air from the furnace. Heat the parts to 350±5°C. Simultaneously, introduce tetrachloroethylene liquid (4.5×the total surface area of ​​the workpiece + 20) L / min and ammonia gas at 5-10 L / min. Hold for 3-5 minutes. Then, introduce tetrachloroethylene liquid (4.5×the total surface area of ​​the workpiece + 30) L / min and ammonia gas at 5-10 L / min. Hold for another 3-5 minutes. Then, heat the parts to 520±5°C. Simultaneously introduce ammonia gas at 30-35 L / min. Set the nitrogen potential factor (Kn) to 10 and hold for 1-2 hours. Then, set the nitrogen potential factor (Kn) to 0.8-1.0 and hold for 20±1 hours. Then, set the temperature to 540±5°C, the nitrogen potential factor (Kn) to 0.5-0.6, and hold for 40±1 hours. Finally, high-purity nitrogen is introduced to maintain a slightly positive pressure in the furnace. After the furnace is cooled for 2 hours, it is cooled to below 120°C by a blower and then taken out of the furnace for air cooling. Subsequently, the various parts are machined accordingly to meet the use requirements.

[0060] Test results: The hardness at 0.05mm on both end faces of the part is 1018~1130HV1, the depth of the nitriding layer can reach about 0.33~0.36mm, the vein shape of the nitriding layer is level 2, the nitriding quality is equivalent to that of the grinding surface, and can meet the design requirements.

[0061] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or modification made by those skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A method for processing steel parts, characterized in that: include: The blank is subjected to rough machining, vacuum quenching, tempering, quenching and tempering, turning finishing and nitriding treatment in sequence; The vacuum quenching adopts a gradient temperature rising method and uses nitrogen for quenching; The nitriding treatment comprises the following steps: S1, heat the machined parts to 350±5℃, introduce tetrachloroethylene liquid and ammonia gas at the same time, and keep the temperature for the preset time; S2, set the temperature to 520±5℃, introduce ammonia gas, set the nitrogen potential factor to 10, and keep warm for 1-2 hours; S3, set the temperature to 540±5℃, the nitrogen potential factor to 0.8-1.0, and keep warm for 20±1h; S4, set the nitrogen potential factor to 0.5-0.6 and keep warm for 40 ± 1 h; S5, cooling to room temperature to obtain a finished product.

2. The method for processing steel parts according to claim 1, characterized in that: The vacuum quenching specifically includes: in a vacuum state, keeping the roughly processed parts at a temperature of 650±10°C for 50 to 60 minutes, then heating it to 850±5°C and keeping it for 50 to 60 minutes, and finally heating it to 1000±5°C and keeping it for 90 to 120 minutes, then quenching it with nitrogen at a pressure of 15 to 18 bar, and cooling it to below 60°C before taking it out of the furnace.

3. The method for processing steel parts according to claim 1, characterized in that: The tempering treatment includes: transferring the parts into a tempering furnace for a first tempering treatment within a preset time after vacuum quenching, and performing a second tempering treatment after air cooling to room temperature.

4. The method for processing steel parts according to claim 3, characterized in that: The temperature of the first tempering treatment is set to 550±5°C, and the holding time is set to 120-150min; The temperature of the second tempering treatment is set to 595±5°C, and the holding time is set to 120-150 minutes.

5. The method for processing steel parts according to claim 1, characterized in that: Said S1 specifically includes: Heat the finished parts to 350±5℃, and simultaneously introduce AL / min of tetrachloroethylene liquid and 5~10L / min of ammonia gas, keep warm for 3~5 minutes, then simultaneously introduce BL / min of tetrachloroethylene liquid and 5~10L / min of ammonia gas, and keep warm for 3~5 minutes; A=4.5×total surface area of ​​parts+20; B=4.5×total surface area of ​​parts+30.

6. The method for processing a steel part according to claim 1, wherein: The S4 specifically includes: introducing high-purity nitrogen to maintain a slightly positive pressure in the furnace, cooling the furnace for 2 hours, then air-cooling to below 120° C., taking the furnace out of the furnace and air-cooling to room temperature to obtain the finished product.

7. The method for processing a steel part according to claim 6, wherein: The nitrogen purity is ≥99.99%; The micro-positive pressure is 50-500 Pa, that is, the pressure inside the furnace is 50-500 Pa higher than the external atmospheric pressure.

8. The method for processing a steel part according to claim 1, wherein: Before the nitriding treatment is carried out, high-purity nitrogen is introduced into the nitriding furnace to exhaust the air in the nitriding furnace.

9. A steel part, characterized in that: The steel part is manufactured by the processing method of any one of claims 1 to 8.