Quantitative calculation method for crack development of epoxy resin material

By conducting thermal-electrical-mechanical combined aging tests on epoxy resin materials, modifying the Arrhenius life model and constructing a crack length equation, the problem of being unable to quantitatively calculate the crack development of epoxy resin insulation materials in existing technologies was solved, and accurate evaluation under multiple stresses was achieved.

CN120724792APending Publication Date: 2025-09-30HARBIN UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510848965.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-24
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

Existing technologies are unable to accurately quantify and calculate the crack development law of epoxy resin insulation materials under thermal-electrical-mechanical combined aging. Traditional models fail to consider the coupling relationship of multiple factors, resulting in inaccurate evaluation.

Method used

By conducting thermal-electrical-mechanical combined aging tests on epoxy resin samples, the Arrhenius life model was modified. Combined with the activation energy of molecular bond breakage, a quantitative calculation method for crack development was established. Flat electrodes were used to simulate the actual electric field and construct the crack length equation.

Benefits of technology

Accurately evaluate the crack development law of epoxy resin materials under multiple stresses, overcome the shortcomings of traditional models, and provide more accurate quantitative calculation of crack length.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120724792A_ABST
    Figure CN120724792A_ABST
Patent Text Reader

Abstract

The invention discloses a quantitative calculation method for crack development of an epoxy resin material, belongs to the technical field of insulation aging crack evaluation, and aims at correcting molecular bond fracture activation energy by considering that the molecular bond fracture activation energy is reduced under the action of external stress, and further correcting an Arrhenius life model under thermal aging, so that the crack development of the epoxy resin material is evaluated. Obtaining a life model under heat-electricity-machine combined aging, and fully considering a coupling relationship among aging stresses; obtaining the net frequency f * of molecular bond breakage in the material according to a life model under heat-electricity-machine combined aging; and calculating the molecular bond fracture number N under the heat-electricity-machine combined aging: substituting the molecular bond fracture number N under the heat-electricity-machine combined aging into the equation of the critical crack length, establishing an average expansion model of the crack, and quantitatively calculating the critical crack length of the epoxy resin under the heat-electricity-machine combined aging. And the crack development law under different aging stresses can be accurately evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulation aging cracking assessment, and in particular relates to a quantitative calculation method for crack development of epoxy resin materials. Background Art

[0002] Epoxy resin insulation materials are mainly used in cast-type high-voltage electrical equipment such as dry-type transformers, reactors, and motors. They are widely used because of their good insulation properties and mechanical strength after curing. However, for power equipment in long-term complex working environments, their insulation is subjected to the combined effects of electric fields, high temperatures, and vibration mechanical stresses for a long time, which causes the insulation performance to deteriorate. According to data, a more common problem with dry-type electrical equipment is cracking of epoxy resin materials under complex stresses. The cracked insulation is susceptible to moisture intrusion, further aggravating the aging of the insulation. At the same time, under the action of the electric field, space charges will accumulate at the cracks and cause concentration / distortion of the electric field, which will seriously affect the stable operation of the dry-type electrical equipment. Therefore, it is crucial to clarify the development law of cracks in epoxy resin materials under the combined electric-thermal-mechanical aging stress and to realize a quantitative calculation method for crack development.

[0003] The lifespan of epoxy resin insulation materials will vary under varying stresses. The fundamental cause of crack development and fracture in epoxy resin insulation is the thermal motion of atoms. The energy required to produce fractures is not simply the work done by the external force, but largely stems from the energy fluctuations generated by the thermal motion of atoms. The external force acts to promote thermal damage, causing the molecular chains to develop in a certain direction. Currently, in accelerated aging tests that investigate the relationship between factors affecting lifespan, commonly used accelerated stresses or aging factors include temperature, electrical stress, and humidity. Models corresponding to accelerated stresses include the Arrhenius model, the inverse power law model, and the Eyring model. This allows for the establishment of a functional relationship between aging lifespan and accelerated stress.

[0004] Due to the complex operating environment of actual electrical equipment, such as the combined effects of thermal, electrical and mechanical stresses, the application scope of traditional single aging models is extremely small. For example, traditional electrical aging models of insulating materials are all tested using step voltage withstand tests. The electrode structure during the test mostly uses needle-plate electrodes with concentrated electric fields, which is different from the electric fields that actual electrical equipment is subjected to. Therefore, this model cannot be applied to the establishment of a multi-factor joint aging model. The calculation of the traditional multi-factor joint aging life model adopts superposition quantification, multiplying the thermal aging model by the electrical aging model by the vibration aging model. The undetermined parameters in each aging model are obtained based on their own experiments, without considering the coupling relationship between each other, resulting in inaccurate aging assessment models constructed by simple superposition principles, which in turn makes it impossible to quantify the crack development process of epoxy resin insulation materials.

[0005] Therefore, a new technical solution is urgently needed in the existing technology to solve this problem. Summary of the Invention

[0006] In order to overcome the shortcomings of the existing technology, the present invention provides a quantitative calculation method for crack development of epoxy resin materials, which is used to solve the problem that the crack development process of epoxy resin insulation materials under thermal-electrical-mechanical combined aging cannot be quantitatively calculated.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is: a quantitative calculation method for crack development of epoxy resin material, comprising the following steps:

[0008] S1. Conduct thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging tests on multiple groups of epoxy resin samples;

[0009] S2. Conduct mass loss tests on thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging samples with different aging cycles to obtain the mass loss reaction rate;

[0010] S3. Combining the mass loss reaction rate data in S2 and the molecular bond breaking activation energy of the epoxy resin material under thermal aging conditions, the Arrhenius life model under thermal aging is modified to obtain a life model under thermal-electrical-mechanical combined aging.

[0011] S4. According to the lifespan model under the combined thermal-electrical-mechanical aging in S3, the net frequency f* of molecular bond fracture in the material at a constant temperature can be obtained; the net frequency f* of molecular bond fracture is multiplied by the lifespan L of the epoxy resin insulation material under a single mechanical stress. σ Calculate the number of molecular bond breaks N under combined thermal-electrical-mechanical aging:

[0012] S5. According to the crack development characteristics under mechanical stress, a molecular bond breaking number N and mechanical stress σ are constructed. m The equation for the critical crack length with is a variable;

[0013] S6. Substitute the molecular bond breaking number N under the thermal-electrical-mechanical combined aging obtained in S4 into the critical crack length equation of S5 to quantitatively calculate the critical crack length of the epoxy resin under the thermal-electrical-mechanical combined aging.

[0014] Preferably, the reaction rate of mass loss in S2 is characterized by the relationship between mass loss and aging time at the aging temperature, and the average value of the multi-segment fitting slope is used as the equivalent reaction rate.

[0015] Preferably, the modification of the Arrhenius life model under thermal aging in S3 is a modification of the molecular bond breaking activation energy by taking into account the effect of external stress so as to reduce the molecular bond breaking activation energy; the external stress includes electrical stress and mechanical stress.

[0016] Preferably, the electrodes used in the thermal-electric combined aging and thermal-electric-mechanical combined aging tests described in S1 are flat plate electrodes.

[0017] Through the above design scheme, the present invention can bring the following beneficial effects:

[0018] 1. The molecular bond breaking activation energy is corrected by taking into account the effect of external stress, which reduces the molecular bond breaking activation energy. This leads to a correction of the Arrhenius life model under thermal aging, resulting in a life model under thermal-electrical-mechanical combined aging. This model fully considers the coupling relationship between the various aging stresses, i.e., the undetermined coefficients in the aging model.

[0019] 2. Substituting the molecular bond breaking number N under combined thermal-electrical-mechanical aging into the critical crack length equation, an average crack growth model was established to quantitatively calculate the critical crack length of epoxy resin under combined thermal-electrical-mechanical aging, and accurately evaluate the crack development law under different aging stresses;

[0020] 3. The electrodes used in the thermal-electric combined aging and thermal-electric-mechanical combined aging tests are flat electrodes with a uniform electric field inside, which applies uniform electric stress, the same as the electric field that actual electrical equipment is subjected to. This overcomes the problem that traditional electrical aging uses needle-plate electrodes with concentrated electric fields, making it impossible to use traditional electrical aging models for multi-factor combined aging models. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention provides a flow chart of a quantitative calculation method for crack development in epoxy resin materials.

[0022] Figure 2 This is a graph showing epoxy resin mass loss under different aging factors in an embodiment of a quantitative calculation method for crack development of an epoxy resin material according to the present invention.

[0023] Figure 3 This is a development trend diagram of epoxy resin crack length under different stresses in an embodiment of a quantitative calculation method for epoxy resin material crack development of the present invention. DETAILED DESCRIPTION

[0024] The following is a detailed description of the specific embodiments of the present invention with reference to the accompanying drawings.

[0025] To more clearly illustrate the present invention, the present invention is further described below with reference to preferred embodiments. Those skilled in the art will appreciate that the detailed description below is illustrative and non-restrictive, and that the user may make various changes to the following parameters without departing from the mechanism and scope of the invention as set forth in the claims. To avoid obscuring the essence of the present invention, well-known methods and processes are not described in detail.

[0026] By the attached Figures 1 to 3 As shown: A quantitative calculation method for crack development of epoxy resin material, comprising the following steps:

[0027] S1. Conduct thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging tests on multiple groups of epoxy resin samples;

[0028] S2. Conduct mass loss tests on thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging samples with different aging cycles to obtain the mass loss reaction rate;

[0029] S3. Combining the mass loss reaction rate data in S2 and the molecular bond breaking activation energy of the epoxy resin material under thermal aging conditions, the Arrhenius life model under thermal aging is modified to obtain a life model under thermal-electrical-mechanical combined aging.

[0030] S4. According to the lifespan model under the combined thermal-electrical-mechanical aging in S3, the net frequency f* of molecular bond fracture in the material at a constant temperature can be obtained; the net frequency f* of molecular bond fracture is multiplied by the lifespan L of the epoxy resin insulation material under a single mechanical stress. σ Calculate the number of molecular bond breaks N under combined thermal-electrical-mechanical aging:

[0031] S5. According to the crack development characteristics under mechanical stress, a molecular bond breaking number N and mechanical stress σ are constructed. m The equation for the critical crack length with is a variable;

[0032] S6. Substitute the molecular bond breaking number N under the thermal-electrical-mechanical combined aging obtained in S4 into the critical crack length equation of S5 to quantitatively calculate the critical crack length of the epoxy resin under the thermal-electrical-mechanical combined aging.

[0033] Furthermore, in order to apply uniform electrical stress, which is the same as the electric field that actual electrical equipment is subjected to, the electrodes used in the thermal-electric combined aging and thermal-electrical-mechanical combined aging tests described in S1 are flat electrodes.

[0034] Furthermore, the reaction rate of mass loss in S2 is characterized by the reaction rate at the aging temperature based on the relationship between mass loss and aging time, and the average value of the multi-segment fitting slope is used as the equivalent reaction rate.

[0035] Furthermore, the modification of the Arrhenius life model under thermal aging described in S3 is to modify the molecular bond breaking activation energy by taking into account the effect of external stress, which reduces the molecular bond breaking activation energy; the external stress includes electrical stress and mechanical stress. The specific steps are as follows:

[0036] According to the Arrhenius model, the reaction rate k T The relationship with aging temperature is:

[0037] k T =A T exp(-ΔE / kT)1

[0038] Where A T is the unknown parameter of the reaction rate model; ΔE is the activation energy of epoxy resin molecular bond breaking, unit: joule; k is the Boltzmann constant, 1.38×10 -23 Joule / Kelvin; T is the absolute temperature at which the chemical reaction takes place, unit: Kelvin.

[0039] Thermal aging life L T for:

[0040] L T =K T exp(ΔE / kT) 2

[0041] Where K T is an undetermined constant, which is related to the material performance degradation at the end of its life, that is, the mass loss Δm and the parameter A in the reaction rate model. T Related, K T =Δm / A T ;

[0042] The external electric field will cause the effect of electric stress through the internal potential difference. Under the electric stress, the energy required for the transition when the molecular bond of the epoxy resin material is broken will be reduced. The electric stress σ acting on the unit electrode area is E It can be calculated by the work done by the electrostatic field of the flat plate capacitor, and the formula is as follows:

[0043]

[0044] Where ε0 is the dielectric constant of vacuum, 8.854×10 -12 Farad / meter; ε r is the power frequency relative dielectric constant of epoxy resin material; E is the applied electric field strength, unit: volt / meter.

[0045] By modifying the traditional Arrhenius model under thermal aging, we can obtain:

[0046] L TE =K TEexp((ΔE-γ E σ E / M e ) / kT) 4

[0047] Where K TE is an undetermined constant, which is related to the performance degradation of the material at the end of its life; E is a constant with volume dimension, which is the activation volume of polymer molecular bond dissociation under electrical stress, approximately the sample volume under the effective electrode area, unit: cubic meter; σ E The electric stress is the stress on the effective surface of the epoxy resin material electrode caused by the electric field energy. It can be calculated by formula 3. The unit is N / m2. e It is the number of molecules inside the effective volume of the epoxy resin sample test, which can be calculated based on the molar mass of the epoxy resin and the mass of the effective volume of the epoxy resin sample test, unit: piece.

[0048] Considering that mechanical stress reduces the activation energy required for molecular breakage, the traditional Arrhenius model under thermal aging is modified to obtain:

[0049] L Tσ =K Tσ exp((ΔE-γ m σ m / M e ) / kT) 5

[0050] Where K Tσ is an undetermined constant; γ m is a constant with volume dimension, which is the activation volume of polymer molecular bond dissociation under mechanical stress, approximately the sample volume under the effective electrode area, unit: cubic meter; σ m Mechanical stress, that is, the stress on the effective surface of the electrode caused by mechanical load, can be calculated by the mass of the sample and the mechanical stress vibration acceleration. Unit: Newton / square meter; M e It is the number of molecules inside the effective volume of the epoxy resin sample test, which can be calculated based on the molar mass of the epoxy resin and the mass of the effective volume of the epoxy resin sample test, unit: piece.

[0051] Similarly, the thermal-electrical-mechanical combined aging life model can be obtained:

[0052] L TEσ =K TEσ exp((ΔE-γ m σ m / M e -γ E σ E / M e ) / kT)6

[0053] Where K TEσ is an undetermined constant related to the amount of material degradation at the end of its life;

[0054] Further, the calculation formula for the net frequency f* of molecular bond breaking in the material at a constant temperature as described in S4 is as follows:

[0055]

[0056] Where f0 is the vibration frequency of the atom, and its value is 10 12 ~10 13 , K TEσ is an undetermined constant related to the performance degradation of the material at the end of its life; L TEσ It is the combined thermal-electrical-mechanical aging life.

[0057] Further, the equation for the critical crack length described in S5 is:

[0058]

[0059] Where x c is the critical crack length; C, t, q are constants; N is the number of molecular bond breaks; σ m is the mechanical stress. The specific derivation process is as follows:

[0060] Under mechanical stress, composite insulation materials can produce degradation of dielectric properties such as mechanical properties and insulation resistance due to long-term vibration fatigue. Assuming that the total length of cracks generated by the number of bonds is dN and is dx, the average crack extension length satisfies the following formula:

[0061]

[0062] Where x is the length of the crack, C', t, and q are constants, and η is the internal strain of the material, which can usually be expressed as the ratio of the stress corresponding to the internal strain of the material to the Young's modulus, that is:

[0063]

[0064] Substituting formula 12 into formula 11, we have:

[0065]

[0066] Integrating both sides of Equation 13, we can get:

[0067]

[0068] Where w is a constant.

[0069] According to the initial crack condition, when σ = 0, x = x0, substituting into Equation 14 and further solving the above differential equation, we can obtain:

[0070]

[0071] If the critical length of the crack is defined as x c , when the initial crack length x0 = 0, the simplified equation can be obtained as:

[0072]

[0073] The equation for the critical crack length is then obtained as:

[0074]

[0075] Calculate the life of epoxy resin insulation material L under single mechanical stress using formulas 4 and 6. σ ,

[0076] L σ =L TE / L TEσ 9

[0077] The molecular bond fracture number N of epoxy insulation materials under thermal-electrical-mechanical combined aging can be calculated according to the following formula: This fully considers the coupling relationship between the aging stresses.

[0078] N=L σ f * 10

[0079] The calculation method of constants C, t, and q is as follows:

[0080] Considering the life model under single mechanical stress:

[0081] L σ =K m σ m -t 16

[0082] Where K m , t is a constant to be determined;

[0083] Combined with Formula 9, the life of epoxy resin material under different mechanical stresses is calculated when the aging temperature and field strength remain unchanged. Substituting it into Formula 16 can calculate the parameter t.

[0084] Consider the crack length x c When is the sample thickness, that is, the crack completely penetrates the sample in the stress direction, the molecular bond fracture number N of the epoxy resin material under different mechanical stresses calculated by Formula 10 and the parameter t can be used to calculate the parameters q and C in Formula 8, thereby obtaining the crack development model of the epoxy resin material under thermal-electrical-mechanical combined aging stress.

[0085] In the specific implementation, three groups of epoxy resin samples were subjected to accelerated thermal aging at aging temperatures of 150 degrees Celsius, 160 degrees Celsius, and 170 degrees Celsius, and their thermal mass loss was tested at 1 day, 5 days, 15 days, 30 days, and 50 days. The test results are as follows: Figure 2 As shown in the figure, according to the test results, the equivalent reaction rate of epoxy resin materials at different aging temperatures is calculated. According to the relationship between aging temperature and equivalent reaction rate, combined with formula 1, the molecular fracture activation energy ΔE of epoxy resin under thermal aging can be calculated to be 5.1048×10 -21 Joules, and using the IEC 216-2 standard to adopt a thermal mass loss rate of 3.4% as the failure standard for epoxy resin, the life model of epoxy resin material under thermal aging can be obtained:

[0086] At an aging temperature of 160 degrees Celsius, the electric field strength was 3 kV / mm, 5 kV / mm, and 8 kV / mm respectively. The epoxy resin sample was subjected to a thermal-electric combined aging test. Its thermal mass loss was tested at 1 day, 5 days, 15 days, 30 days, and 50 days. The equivalent reaction rate of the epoxy resin material under different electric field strengths at an aging temperature of 160 degrees Celsius was calculated. The influence of electrical stress on activation energy was added to the activation energy calculation part. The thermal-electric mass loss curve of the epoxy resin material is shown in the figure below. Figure 2 As shown, according to the relationship between electric field stress and equivalent reaction rate, the activation volume γ for molecular bond dissociation can be obtained. E is 7.8539×10 -6 and the undetermined constant K TE is 5733.8603, M e is 3.612×10 22 ; Electric stress σ E 384N / m 2 , and the life model of epoxy resin material under thermal-electrical combined aging is obtained:

[0087] Similarly, the thermal-mechanical combined aging model of epoxy resin materials can also be obtained through thermal-mechanical mass loss test data of different mechanical stresses, such as Figure 2 As shown, the thermal-mechanical combined aging reaction rate under different mechanical stresses is calculated, and the undetermined parameter K in the thermal-mechanical combined aging life model is obtained. Tσ is 7325.2291 and the activation volume γ for polymer molecular bond dissociation m is 7.8539×10 -6 .

[0088] Finally, according to the combined thermal-electrical-mechanical aging test, the aging temperature is 160 degrees Celsius, the electric field strength is 5 kV / mm, and the vibration acceleration is 8 m / s^2. The activation energy ΔE, the activation volume γ under electrical stress and mechanical stress are obtained by combining the above calculations. E , γm According to the reaction rate under the combined thermal-electrical-mechanical aging stress, the undetermined constant K in the combined thermal-electrical-mechanical aging life model can be calculated. TEσ It is 4822.4575.

[0089] According to formulas 9 and 10, the molecular bond breaking number N of epoxy insulation material can be calculated by changing the mechanical stress σ m , the life of epoxy resin material under single mechanical stress can be obtained σ , and according to formula 16, the undetermined constant K can be obtained m is 2464.1874 and t is 0.3577.

[0090] When the crack of epoxy resin material penetrates the specimen under stress direction, the critical length is considered as the specimen thickness, that is, x c The molecular fracture number N obtained under the two sets of mechanical stresses and t in the aging model under a single mechanical stress are combined. According to Formula 8, the undetermined constant C in the crack growth model is 1.8785×10 -17 , q is -3.5384×10 -9 .

[0091] Life under a certain mechanical stress L σ As the mechanical stress application time, the number of molecular bond breaks N under the mechanical stress time can be obtained according to formula 10. In the calculation, the atomic vibration frequency f0 is 10 13 Hertz, the crack length in epoxy resin under different mechanical stress time is as follows Figure 3 When the vibration acceleration is 5 m / s², the root mean square error of the calculation result is 0.0716; when the vibration acceleration is 8 m / s², the root mean square error of the calculation result is 0.0012.

[0092] Obviously, the embodiments described above are only some of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0093] The above mainly introduces the solution of the embodiment of the present application from the perspective of the execution process of the method side. It is understandable that in order to implement the above functions, the network device includes hardware structures and / or software modules corresponding to the execution of each function. Those skilled in the art should easily realize that, in combination with the units and algorithm steps of each example described in the embodiment provided herein,

[0094] This application can be implemented in hardware or a combination of hardware and computer software. Whether a function is implemented in hardware or by computer software driving hardware depends on the specific application and design constraints of the technical solution. Professionals and technicians may use different methods to implement the described functions for each specific application, but such implementation should not be considered beyond the scope of this application.

[0095] If the above-mentioned integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable memory. Based on this understanding, the technical solution of the present application, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product. The computer software product is stored in a memory and includes a number of instructions for enabling a computer device to perform all or part of the steps of the various embodiments of the present application, such as a personal computer, server, or TRP. The aforementioned memory includes various media that can store program codes, such as a USB flash drive, a read-only memory ROM, a random access memory RAM, a mobile hard disk, a magnetic disk, or an optical disk.

Claims

1. A quantitative calculation method for crack development of epoxy resin material, characterized in that: The following steps are involved: S1. Conduct thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging tests on multiple groups of epoxy resin samples; S2. Conduct mass loss tests on thermal aging, thermal-electrical combined aging, thermal-mechanical combined aging, and thermal-electrical-mechanical combined aging samples with different aging cycles to obtain the mass loss reaction rate; S3. Combining the mass loss reaction rate data in S2 and the molecular bond breaking activation energy of the epoxy resin material under thermal aging conditions, the Arrhenius life model under thermal aging is modified to obtain a life model under thermal-electrical-mechanical combined aging. S4. According to the lifespan model under the combined thermal-electrical-mechanical aging in S3, the net frequency f* of molecular bond fracture in the material at a constant temperature can be obtained; the net frequency f* of molecular bond fracture is multiplied by the lifespan L of the epoxy resin insulation material under a single mechanical stress. σ Calculate the number of molecular bond breaks N under combined thermal-electrical-mechanical aging: S5. According to the crack development characteristics under mechanical stress, a molecular bond breaking number N and mechanical stress σ are constructed. m The equation for the critical crack length with is a variable; S6. Substitute the molecular bond breaking number N under the thermal-electrical-mechanical combined aging obtained in S4 into the critical crack length equation of S5 to quantitatively calculate the critical crack length of the epoxy resin under the thermal-electrical-mechanical combined aging.

2. The quantitative calculation method for crack development of epoxy resin material according to claim 1, characterized in that: The reaction rate of mass loss in S2 is the reaction rate at the aging temperature characterized by the relationship between mass loss and aging time, and the average value of the multi-segment fitting slope is used as the equivalent reaction rate.

3. The quantitative calculation method for crack development of epoxy resin material according to claim 1, characterized in that: The modification of the Arrhenius life model under thermal aging described in S3 is a modification of the molecular bond breaking activation energy by taking into account the effect of external stress, which reduces the molecular bond breaking activation energy; the external stress includes electrical stress and mechanical stress.

4. The quantitative calculation method for crack development of epoxy resin material according to claim 1, characterized in that: The net frequency f* of molecular bond breaking in the material at a constant temperature as described in S4 is calculated as follows: Where f0 is the vibration frequency of the atom, and its value is 10 12 ~10 13 , K TEσ is an undetermined constant related to the performance degradation of the material at the end of its life; L TEσ It is the combined thermal-electrical-mechanical aging life.

5. The quantitative calculation method for crack development of epoxy resin material according to claim 1, characterized in that: The equation for the critical crack length in S5 is: Where x c is the critical crack length; C, t, q are constants; N is the number of molecular bond breaks; σ m For mechanical stress.

6. The quantitative calculation method for crack development of epoxy resin material according to claim 1, characterized in that: The electrodes used in the thermal-electric combined aging and thermal-electric-mechanical combined aging tests described in S1 are flat plate electrodes.