Copper nano-catalyst as well as preparation method and application thereof
The sea urchin-shaped copper nanocatalyst was prepared by the three-electrode system electrochemical deposition method, which solved the problems of harsh reaction conditions and low selectivity of copper-based catalysts in the electrocatalytic reduction of CO2, and achieved the effect of efficient electrocatalytic reduction of CO2 to ethanol.
Patent Information
- Application Number
- CN202410416833.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2025-10-14
AI Technical Summary
When copper-based catalysts are used for the electrocatalytic reduction of CO2, they have problems such as harsh reaction conditions, complex preparation process, high overpotential, and low selectivity, especially when producing ethanol, they exhibit poor catalytic stability.
A three-electrode electrochemical deposition method was adopted, using an electroplating solution containing divalent copper salt, potassium bicarbonate, potassium sodium tartrate and fluoride salt. Sea urchin-shaped copper nanocatalysts were prepared through forward and reverse electroplating and LSV scanning to regulate the binding energy of reaction intermediates and optimize the catalyst structure.
It achieved highly selective electrocatalytic reduction of CO2 to ethanol at a low overpotential, with a maximum Faradaic efficiency of 63% and a current density of 248 mA/cm2. The catalyst stability was superior to that of traditional catalysts.
Smart Images

Figure CN120776412A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalytic reduction of CO2 to produce ethanol, and in particular to a copper nanocatalyst and a preparation method and application thereof. Background Art
[0002] Overuse of fossil fuels has resulted in massive CO2 emissions, contributing to environmental problems such as the greenhouse effect, ocean acidification, and sea level rise. Therefore, reducing CO2 emissions is of vital importance. The electrocatalytic reduction (ECR) of CO2 to high-carbon (C2+) industrial feedstocks has garnered significant attention in recent years, achieving the dual goals of CO2 storage and clean energy conversion. ECR technology offers unique advantages, including mild reaction conditions, inexpensive reactants, a green process, and high efficiency, and boasts broad application prospects.
[0003] The ECR performance of a wide range of catalysts has been studied, including metal catalysts, metal sulfide catalysts, single-atom catalysts, and non-metallic catalysts. Among all monometallic catalysts, copper (Cu) is the only metal capable of electrocatalytically reducing CO2 to hydrocarbon products, particularly multi-carbon products. However, copper-based catalysts require demanding reaction conditions, high temperatures and pressures, and even the use of hazardous chemicals as raw materials. The preparation process is complex and time-consuming.
[0004] CN114277398A provides a preparation method and application of a nano-copper catalyst. The method comprises: (1) preparing a bicarbonate solution, dissolving an organic acid salt and a copper salt precursor in the bicarbonate solution; and (2) placing a conductive substrate in the solution obtained in step (1), introducing at least one of N2 and CO2 gases, and simultaneously performing electrochemical reduction to obtain a nano-copper catalyst. The catalyst preparation method of the present invention is simple, employs mild conditions, and is easy to operate. During the electrochemical reduction preparation of the copper catalyst, the organic anions can coordinate with the copper on the catalyst surface and induce the formation of oriented crystal planes, thereby improving the stability and activity of the nano-copper catalyst.
[0005] CN 115584525 A provides a catalyst for electrocatalytic CO2 synthesis of multi-carbon products and its preparation method. The catalyst is a CuInS2-x nanomaterial with Cu-In dual active centers. The method comprises the following steps: firstly, using a solvent thermal reaction to synthesize In2S3 with a flower ball-shaped ruffle cluster structure, and then, by electrochemical ion replacement, doping Cu into the defect sites of the flower ball-shaped ruffle cluster In2S3 to obtain CuInS2-x with Cu-In dual active centers. 2-x The catalyst has both high electrocatalytic activity for CO2 reduction and high selectivity for C2+ products.
[0006] The electrocatalytic reduction of CO2 produces both ethylene and ethanol. The selective competition between these two reduction products often leads to problems such as high overpotential and low selectivity when using copper-based catalysts for the electrocatalytic reduction of CO2. Therefore, the rational design and preparation of copper-based catalysts for efficient electrocatalytic reduction of CO2 to ethanol is urgently needed. Summary of the Invention
[0007] The purpose of the present invention is to address the shortcomings of Cu-based catalysts in the electrocatalytic reduction of CO2 to produce hydrocarbon products, such as low selectivity and poor catalytic stability. The present invention aims to provide a copper nanocatalyst by optimizing the structure of the Cu-based catalyst, regulating the binding energy of the reaction intermediates on the catalyst surface, reducing the reaction overpotential, and improving its performance in the electrocatalytic reduction of CO2 to ethanol.
[0008] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0009] The first aspect of the present invention provides a method for preparing a copper nanocatalyst, which adopts a three-electrode system and is placed in an electroplating solution for electrochemical deposition to prepare the copper-based nanocatalyst, wherein the electroplating solution contains a divalent copper salt, potassium bicarbonate, potassium sodium tartrate and a fluoride salt.
[0010] The copper nanocatalyst prepared in this invention features a simple and short preparation cycle, avoiding the high-temperature, high-pressure, and hazardous chemical preparation requirements of most copper-based catalysts. Furthermore, the method is highly reproducible and scalable, while being less expensive than bimetallic materials. The resulting catalyst exhibits high selectivity for reducing CO2 to ethanol.
[0011] The choice of electroplating solution directly influences the reactivity of the resulting copper nanocatalyst. The tartrate radical of potassium sodium tartrate complexes with the copper ions in the copper salt solution, preventing the complete reduction of the copper ions to a zero valence state. This allows the formation of a portion of copper in an intermediate valence state between zero and two valences. Furthermore, the copper-based material prepared by this electrodeposition method exhibits excellent chemical stability. Fluoride ions partially etch the deposited copper, forming a sea urchin-like structure that facilitates the adsorption of CO2 reactant molecules, thereby promoting the formation of C2+ products.
[0012] The copper nanomaterial obtained by the preparation method of the present invention has good chemical stability. The characterization results of the catalyst after the electrocatalytic reduction of CO2 show that the copper nanomaterial still maintains the microstructure before the reaction after the electrochemical reaction process.
[0013] In some preferred embodiments, in the three-electrode system, a platinum sheet and carbon paper are used as the anode and cathode of the working electrode, and a silver / silver chloride electrode is used as the reference electrode;
[0014] Preferably, the dimensions of the anode and cathode of the working electrode are (1-5) x (1-5) cm2 ; The distance between the anode and cathode is 0.5 to 3 cm.
[0015] The present invention uses a platinum sheet as an anode, carbon paper as a cathode, and an aqueous solution containing copper ions as an electrolyte in a three-electrode electrolytic cell system. Tartaric acid radicals of potassium sodium tartrate are added to complex with copper ions in a copper salt solution. Electrodeposition is performed under specific current conditions. Fluoride salts and bicarbonate radicals are then added to give the catalyst a special morphology. After the electrodeposition is completed, the cathode is immediately removed, washed with water multiple times, and further electrochemically treated in a KHCO3 solution to obtain a copper nanocatalyst on the cathode.
[0016] In some preferred embodiments, the preparation method of the present invention obtains an electrode (such as a carbon paper electrode) loaded with copper nanocatalysts, which can be directly used in subsequent applications without separation, such as for electrocatalytic reduction of CO2.
[0017] In the present invention, the concentrations of the various components in the electroplating solution also have a significant impact on the reactivity of the resulting copper nanocatalyst. If the concentration of potassium sodium tartrate is too low, needle-like cluster structures cannot form; however, if the concentration of potassium sodium tartrate is too high, the resulting needle-like cluster crystals will aggregate, affecting the overall structure. Therefore, in the electroplating solution, the concentration of the divalent copper salt is selected to be 0.01 to 0.20 mol / L, and the concentration of potassium sodium tartrate is selected to be 0.10 to 0.40 mol / L. Potassium bicarbonate is used to adjust the acidity and alkalinity of the electrolyte, making it weakly alkaline, which is conducive to the deposition of Cu. Fluoride salts affect the morphology of Cu, etching Cu to form a needle-like cluster structure catalyst. Therefore, in the electroplating solution, the concentrations of potassium bicarbonate and fluoride salts need to be carefully selected: the concentration of potassium bicarbonate is selected to be 0.8 to 4.0 mol / L, and the concentration of fluoride salt is selected to be 0.02 to 0.08 mol / L.
[0018] In some preferred embodiments, in the electroplating solution, the concentration of the divalent copper salt is 0.01 to 0.20 mol / L (e.g., 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.05 mol / L, 0.08 mol / L, 0.10 mol / L, 0.12 mol / L, 0.15 mol / L, 0.20 mol / L, etc.), and the concentration of the potassium bicarbonate is 0.8 to 4.0 mol / L (e.g., 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.5 mol / L, 2.8 mol / L, 3 .0mol / L, 3.2mol / L, 3.6mol / L, 4.0mol / L, etc.), the concentration of potassium sodium tartrate is 0.10-0.40mol / L (for example, 0.10mol / L, 0.15mol / L, 0.20mol / L, 0.25mol / L, 0.30mol / L, 0.35mol / L, 0.40mol / L, etc.), and the concentration of fluoride salt is 0.02-0.08mol / L (for example, 0.02mol / L, 0.03mol / L, 0.04mol / L, 0.05mol / L, 0.06mol / L, 0.07mol / L, 0.08mol / L, etc.).
[0019] In some preferred embodiments, the preparation of the electroplating solution may include the following process:
[0020] 1) preparing a divalent copper salt solution as a first solution;
[0021] 2) adding potassium sodium tartrate to an aqueous solution of potassium bicarbonate to obtain a second solution;
[0022] 3) The first solution and the second solution are mixed, and fluoride salt is added to obtain the electroplating solution.
[0023] In some preferred embodiments, the volume ratio of the first solution to the second solution is 1:4 to 1:8; and the concentration of the fluoride salt in the electroplating solution is 0.02 to 0.08 mol / L.
[0024] In some preferred embodiments, the divalent copper salt is selected from one or more of copper nitrate, copper sulfate, and copper chloride; and the fluoride salt is selected from ammonium fluoride or sodium fluoride.
[0025] The method of scanning the LSV curve is selected to prepare the copper catalyst. It is based on the fact that the LSV reverse scanning can further reduce the surface valence state and reprocess the surface morphology of the copper catalyst deposited on the carbon paper surface as the applied voltage changes slowly, ensuring that more Cu+ and Cu0 states participate in the catalytic reaction. At the same time, multiple scanning under different conditions can ensure the full exposure of the effective crystal surface, which is beneficial to the adsorption of CO2 in subsequent applications.
[0026] In some preferred embodiments, the preparation method further comprises: performing LSV scanning on the copper nanocatalyst prepared by electrochemical deposition;
[0027] Preferably, the LSV scanning process is as follows: selecting at least three different scanning ranges in the voltage range of 0 to -3 V and scanning in sequence, with a scanning speed of 20 to 50 mV / s;
[0028] More preferably, the scanning range of the LSV scan is at least 3 of 0 to -2.5 V, 0 to -2 V, 0 to -1.5 V, 0 to -1 V, 0 to -0.5 V, 0 to -0.25 V, and -0.15 to -0.25 V, preferably 3 to 6;
[0029] The LSV scan described above involves performing one LSV scan within each scanning voltage range, i.e., the number of LSV scans corresponds to the number of scanning ranges. The selected scanning voltages are all negative, intended to further gently reduce the catalyst surface and achieve the desired catalyst micromorphology. The LSV scan equipment and specific procedures are commonly used in the art.
[0030] Preferably, the LSV scan uses a KHCO3 solution with a concentration of 0.5 to 2 mol / L as the electrolyte.
[0031] The inventors have experimentally discovered that forward and reverse electroplating improves the hydrophobicity of copper nanocatalysts compared to direct reverse electroplating, which is beneficial for the long-term stability of catalytic electrode evaluation. The electroplating parameters were further optimized by the inventors based on experimental results. Forward electroplating deposition times greater than 60 seconds, for example, 120 seconds, and reverse electroplating currents less than -200 mA, for example, -100 mA, both resulted in correspondingly poorer performance.
[0032] In some preferred embodiments, the electrochemical deposition process comprises: depositing in a forward direction for 10 to 60 seconds under an applied current of 200 to +800 mA; and immediately depositing in a reverse direction for 2 to 10 minutes under an applied current of -200 to -800 mA.
[0033] Preferably, the stirring is performed at a speed of 200 to 600 r / min during the electrochemical deposition process.
[0034] The second aspect of the present invention provides a copper nanocatalyst prepared according to the above preparation method.
[0035] Preferably, the copper nanocatalyst contains Cu, O, C, K, and F elements.
[0036] More preferably, the copper nanocatalyst is in the shape of a sea urchin.
[0037] Further preferably, the copper nanocatalyst is supported on the working electrode cathode of the three-electrode system.
[0038] The third aspect of the present invention provides the use of the above-mentioned copper nanocatalyst in the electrocatalytic reduction of CO2.
[0039] The copper nanocatalyst of the present invention is used in the electrocatalytic reduction of CO2 to achieve the reduction reaction of CO2 to ethanol products, with a maximum Faradaic efficiency of 63% and a current density of 248 mA / cm 2 , and the catalyst has high stability.
[0040] A fourth aspect of the present invention provides a method for electrocatalytic reduction of CO2, using the above-mentioned copper-based nanomaterial as an electrocatalyst;
[0041] Preferably, the method for electrocatalytic reduction of CO2 uses the electrode loaded with the copper nanocatalyst as the working electrode cathode, places it in the cathode electrolyte, and introduces CO2 into the cathode electrolyte to prepare an electrocatalytic reduction product mainly composed of ethanol.
[0042] In some preferred embodiments, the electrolyte is a KHCO3 solution with a concentration of 0.5 to 2 mol / L; the potential is -0.3 to -1 V (vs. RHE), and the electrolysis time is 0.5 to 2 h; the flow rate of continuous CO2 introduction is 20 to 50 mL / min, which is conducive to catalyzing the electron transfer and mass transfer process of the CO2 reduction reaction, thereby obtaining a C2+ product with higher selectivity.
[0043] The technical solution provided by the present invention has the following beneficial effects:
[0044] 1. The present invention prepares copper nanocatalysts with special morphology through a one-step electrochemical cathode deposition process. The product has high purity, requires less equipment, has a short cycle, and is simple to operate. It is suitable for large-scale production without the need for additional CO2 raw material consumption.
[0045] 2. The present invention uses fluorine modification to make the copper nanocatalyst appear sea urchin-shaped, and the nanostructure size is uniform.
[0046] 3. The copper nanocatalyst of the present application can realize the conversion of CO2 to ethanol product in the process of electrocatalytic reduction of CO2, with the highest Faraday efficiency of 63% and the current density of 248 mA / cm 2 Compared with the existing catalyst, the catalyst can realize higher ethanol selectivity at lower overvoltage, and the stability of the catalyst is better than that of the traditional catalyst.
[0047] 4. The electroplating method of the present application adopts forward and reverse electroplating processes, which improves the stability of the catalyst. BRIEF DESCRIPTION OF DRAWINGS
[0048] Figure 1 SEM image of the copper nanocatalyst of Example 1 before the electrocatalytic reduction of CO2 reaction;
[0049] Figure 2 SEM local enlarged image of the copper nanocatalyst of Example 1 before the electrocatalytic reduction of CO2 reaction;
[0050] Figure 3 SEM image of the copper nanocatalyst of Example 1 after the electrocatalytic reduction of CO2 reaction;
[0051] Figure 4 Element distribution map of the copper nanocatalyst of Example 1;
[0052] Figure 5 SEM image of the copper nanocatalyst of Comparative Example 2;
[0053] Figure 6 Ethanol and ethylene selectivity chart of the copper nanocatalyst of Example 1 in the electrocatalytic reduction of CO2 at different voltages;
[0054] Figure 7 Product distribution chart of the copper nanocatalyst of Example 1 in the reduction of CO2 at-0.75 V voltage;
[0055] Figure 8 Raman chart of the copper-based nanomaterial prepared in Example 1;
[0056] Figure 9 SEM image of the copper nanocatalyst of Comparative Example 3 (without LSV scanning treatment). DETAILED DESCRIPTION
[0057] The present application will be further described below through specific examples, and the examples described in the present application are only used to illustrate the present application, and do not mean that the scope of the present application is limited to the examples.
[0058] In the following examples, the preparation method of the copper nanocatalyst comprises:
[0059] The copper nanocatalyst is prepared by electrochemical deposition in a plating solution using a three-electrode system, wherein the plating solution contains divalent copper salt, potassium bicarbonate, potassium sodium tartrate and fluoride salt.
[0060] In the three-electrode system, a platinum sheet and carbon paper are used as the anode and cathode of the working electrode, and a silver / silver chloride electrode is used as the reference electrode.
[0061] The dimensions of the anode and cathode of the working electrode are (1-5)×(1-5) cm 2 ; The distance between the anode and the cathode is 0.5 to 3 cm.
[0062] The divalent copper salt is selected from one or more of copper nitrate, copper sulfate, and copper chloride; and the fluoride salt is selected from ammonium fluoride or sodium fluoride.
[0063] In the electroplating solution, the concentration of the divalent copper salt is 0.01 to 0.20 mol / L, the concentration of the potassium bicarbonate is 0.8 to 4.0 mol / L, the concentration of the potassium sodium tartrate is 0.10 to 0.40 mol / L, and the concentration of the fluoride salt is 0.02 to 0.08 mol / L.
[0064] 1) preparing a copper salt solution as a first solution;
[0065] 2) adding potassium sodium tartrate powder to the aqueous solution of potassium bicarbonate and stirring to dissolve to obtain a second solution;
[0066] 3) The first solution and the second solution are mixed, and fluoride salt is added to obtain a transparent liquid as an electroplating solution.
[0067] The electrochemical deposition process includes: depositing in a forward direction for 10 to 60 seconds under an applied current of 200 to +800 mA; and then immediately depositing in a reverse direction for 2 to 10 minutes under an applied current of -200 to -800 mA.
[0068] During the electrochemical deposition process, stirring is performed at a speed of 200 to 600 r / min;
[0069] The copper nanocatalyst prepared by electrochemical deposition is subjected to LSV scanning; the LSV scanning process is as follows: at least three different scanning ranges are selected in the voltage range of 0 to -3 V and scanned in sequence at a scanning speed of 20 to 50 mV / s;
[0070] Preferably, the scanning range of the LSV scan is at least 3 of 0 to -2.5 V, 0 to -2 V, 0 to -1.5 V, 0 to -1 V, 0 to -0.5 V, 0 to -0.25 V, and -0.15 to -0.25 V, preferably 3 to 6;
[0071] The LSV scan uses a KHCO3 solution with a concentration of 0.5 to 2 mol / L as the electrolyte.
[0072] In the following examples, the copper nanocatalyst was prepared according to the above preparation method;
[0073] The copper nanocatalyst contains Cu, O, C, K, and F elements, wherein the content of each element is as follows by mass ratio: Cu is 50-70%; O is 5-20%; C is 5-20%; K is 1-10%; and F is 3-20%. The copper nanocatalyst is in the shape of a sea urchin.
[0074] The copper nanocatalyst is loaded on the working electrode cathode of the three-electrode system.
[0075] In the following examples, the electrocatalytic reduction of CO2 employs the copper nanocatalyst described above as the electrocatalyst. Preferably, the electrocatalytic reduction of CO2 employs an electrode loaded with the copper nanocatalyst as a working electrode cathode, which is placed in a catholyte, and CO2 is introduced into the catholyte to produce an electrocatalytic reduction product primarily composed of ethanol. The electrolyte is a KHCO3 solution having a concentration of 0.5 to 2 mol / L; the potential is -0.3 to -1 V (vs. RHE), the electrolysis time is 0.5 to 2 hours, and the CO2 is continuously introduced at a flow rate of 20 to 50 mL / min.
[0076] Instruments and testing methods:
[0077] 1. The preparation of the working electrode and the assembly of the flow-type electrolytic cell include:
[0078] (1) A commercial flow electrolytic cell system from GOSHIRILIAN was used as an electrochemical CO2 reduction reaction device. The working electrode was made of copper-based nanomaterials with an effective area of 2×2 cm 2 , the counter electrode is a platinum electrode, and the reference electrode is a silver / silver chloride electrode;
[0079] (2) Assemble the three-electrode flow-type electrolytic cell system described in step (1), use rubber pads to isolate each component, use a commercial anion exchange membrane as an electrolyte diaphragm, and use a clamp to fix and assemble the entire test system to ensure good airtightness.
[0080] 2. The test method for evaluating the reaction of copper-based nanomaterials adopts the linear scanning method and the constant potential method.
[0081] The reaction products were detected by gas chromatography equipped with a headspace sampling device. The instrument model was Agilent GC7890B gas chromatograph, the detector was a thermal conductivity detector (TCD), the carrier gas was Ar, and the quantitative method was the external standard method.
[0082] The Faradaic efficiency (FE) is calculated as follows:
[0083]
[0084] FE is the Faradaic efficiency, in %; Z is the number of electrons transferred to produce ethanol, which is 12; n is the number of moles of a target product produced during the electrolysis process; Qtotal is the total charge consumption during the electrolysis process, in C.
[0085] Example 1
[0086] The copper nanocatalyst was prepared as follows:
[0087] 1) Build a three-electrode system: use a 2*2cm size 2 High-purity platinum metal sheet and carbon paper are used as the anode and cathode of the working electrode, with a distance of 3 cm between the two electrodes, and a silver / silver chloride electrode is used as the reference electrode;
[0088] 2) preparing a 0.5 mol / L copper nitrate aqueous solution as a first solution;
[0089] 3) adding potassium sodium tartrate powder to a 2 mol / L KHCO3 aqueous solution and stirring to dissolve the potassium sodium tartrate to a concentration of 0.25 mol / L to obtain a second solution;
[0090] 4) Mixing the first solution and the second solution in a volume ratio of 1:4 to obtain a copper nitrate concentration of 0.1 mol / L, a KHCO concentration of 1.6 mol / L, and a potassium sodium tartrate concentration of 0.2 mol / L. Ammonium fluoride was then added to obtain a concentration of 0.08 mol / L. The resulting transparent liquid was used as the electroplating solution.
[0091] 5) Place 50 ml of the above plating solution in a beaker and stir magnetically at 500 rpm. Deposit the solution using a three-electrode system at an applied current of +800 mA for 1 minute, followed by an immediate deposition at a current of -800 mA for 10 minutes.
[0092] 6) After the electrodeposition is completed, remove the carbon paper from the cathode, rinse it with deionized water, and then purge it with N2;
[0093] 7) The carbon paper was placed in a flow electrolytic cell containing a 1 M KHCO3 solution as the electrolyte and LSV scanning was performed in the following ranges: 0 to -2.5 V, 0 to -1.5 V, 0 to -0.5 V, 0 to -0.25 V, and -0.15 to -0.25 V at a scanning speed of 50 mV / s. After the scanning was completed, the copper nanocatalyst was obtained.
[0094] Table 1
[0095] element C O F Cu K Content (wt%) 11.09 9.00 17.20 56.16 6.55
[0096] Table 1 and Figure 4 This is the element distribution and composition breakdown of the copper nanocatalyst of Example 1. The results show that the elemental composition of the copper nanocatalyst is primarily Cu, C, O, F, and K. The mass ratios of these elements are as follows: Cu: 56.16%; O: 9.00%; C: 11.09%; K: 6.55%; and F: 17.20%. The copper nanocatalyst is shaped like a sea urchin.
[0097] The application of copper nanocatalysts in the electrocatalytic reduction of CO2 includes the following steps:
[0098] The carbon paper containing copper nanocatalyst prepared above was used as the working electrode for CO2 electroreduction, and the working electrode was placed in a 1 mol / L KHCO3 electrolyte at the cathode;
[0099] CO2 was introduced into the cathode electrolyte to presaturate and activate the working electrode. CO2 was then continuously introduced at a flow rate of 30 mL / min and the potential was adjusted to -0.75 V (vs. RHE). The electrolysis time was 2 h, and the Faradaic efficiency of ethanol production was 63% and the current density was 248 mA / cm 2 .
[0100] Figure 1 This is an SEM image of the copper nanocatalyst of Example 1 before the electrocatalytic reduction of CO2 reaction; it shows evenly distributed clusters of sea urchin-like structures, with the size of the clusters being about 1 to 5 μm.
[0101] Figure 2 This is an enlarged SEM image of the copper nanocatalyst of Example 1 before the electrocatalytic reduction of CO2 reaction; it shows radial needle-like punctures with a diameter of 10 to 50 nm.
[0102] Figure 3 This is the SEM image of the copper nanocatalyst after the electrocatalytic reduction of CO2 in Example 1; the microstructure of the catalyst after the reaction is similar to that of the catalyst after the reaction. Figure 1 There is no obvious change compared with the control, indicating that the nanocatalyst has good stability.
[0103] Figure 6 The selectivity of copper nanocatalyst for ethanol and ethylene in the electrocatalytic reduction of CO2 at different voltages in Example 1 is shown. It can be seen that as the applied voltage increases, the selectivity of ethanol and ethylene increases continuously in general.
[0104] Figure 7This is the product distribution of the copper nanocatalyst of Example 1 when reducing CO2 at a voltage of -0.75V; the products are mainly ethanol and ethylene, and also include CO, H2, CH4 and other products.
[0105] Figure 8 This is the Raman graph of the copper-based nanocatalyst prepared in Example 1; the copper element has +1 and +2 valence bonds.
[0106] Example 2
[0107] Example 2 The copper nanocatalyst was prepared by referring to Example 1, except that the concentration of ammonium fluoride in step 4) was changed to 0.04 mol / L, and the rest of the preparation process remained unchanged.
[0108] The application process of copper nanocatalysts in the electrocatalytic reduction of CO2 remains unchanged, and the Faradaic efficiency of ethanol is 51%.
[0109] Example 3
[0110] Example 3 The copper nanocatalyst was prepared by referring to Example 1, except that: in step 7), LSV scanning was performed with the scanning ranges of 0 to -0.5 V, 0 to -0.25 V, and -0.15 to -0.25 V, respectively, at a scanning speed of 50 mV / s, and the rest of the preparation process remained unchanged.
[0111] The application process of copper nanocatalysts in the electrocatalytic reduction of CO2 remains unchanged, and the Faradaic efficiency of ethanol is 49%.
[0112] Example 4
[0113] Based on Example 1, after 5 cycles of electrolysis (2 h each reaction), the catalyst electrocatalytically reduced CO2 to ethanol with a Faradaic efficiency of 59% and a current density of 219 mA / cm 2 The catalytic performance of the catalyst was lost by 4%, which was within an acceptable range and had good stability.
[0114] Comparative Example 1
[0115] The difference between Comparative Example 1 and Example 1 is that potassium sodium tartrate powder is not added, and the rest of the preparation process remains unchanged.
[0116] The application process of copper nanocatalysts in the electrocatalytic reduction of CO2 remains unchanged, and the Faradaic efficiency of ethanol is 37%.
[0117] Comparative Example 2
[0118] The difference between Comparative Example 2 and Example 1 is that ammonium fluoride is not added, and the rest of the preparation process remains unchanged.
[0119] The application process of copper nanocatalysts in the electrocatalytic reduction of CO2 remains unchanged, and the Faradaic efficiency of ethanol is 11%.
[0120] Figure 5 This is the SEM image of the copper nanocatalyst of Comparative Example 2. It can be seen that when the electroplating solution does not contain fluoride ions, sea urchin-shaped copper nanomaterials cannot be obtained and the catalytic effect is significantly deteriorated.
[0121] Comparative Example 3
[0122] The difference between Comparative Example 1 and Example 1 is that the secondary electrolysis of the KHCO3 solution in step 7) is not performed, the obtained copper nanocatalyst is directly dried, and the rest of the preparation process remains unchanged.
[0123] The copper nanocatalyst's application in the electrocatalytic reduction of CO2 remained unchanged, with a Faradaic efficiency of 33% for ethanol. This suggests that LSV scanning treatment can further improve the catalytic effect of copper nanomaterials, while without this treatment, the catalytic effect significantly deteriorates. Figure 9 The SEM image of the copper nanocatalyst of comparative example 3 (not subjected to LSV scanning treatment); the constituent units of the cluster structure include nanoparticles and nanorods, and their structural consistency, exposed area and one-dimensional size characteristics are compared with Figure 2 Obviously worse.
[0124] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will readily appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.
Claims
1. A method for preparing a copper nanocatalyst, characterized in that: The copper nanocatalyst is prepared by electrochemical deposition in a plating solution using a three-electrode system, wherein the plating solution contains divalent copper salt, potassium bicarbonate, potassium sodium tartrate and fluoride salt.
2. The method for preparing the copper nanocatalyst according to claim 1, wherein In the three-electrode system, a platinum sheet and carbon paper are used as the anode and cathode of the working electrode, and a silver / silver chloride electrode is used as the reference electrode; Preferably, the dimensions of the anode and cathode of the working electrode are (1-5) x (1-5) cm 2 ; The distance between the anode and the cathode is 0.5 to 3 cm.
3. The method for preparing a copper nanocatalyst according to claim 1 or 2, wherein: In the electroplating solution, the concentration of the divalent copper salt is 0.01 to 0.20 mol / L, the concentration of the potassium bicarbonate is 0.8 to 4.0 mol / L, the concentration of the potassium sodium tartrate is 0.10 to 0.40 mol / L, and the concentration of the fluoride salt is 0.02 to 0.08 mol / L.
4. The method for preparing a copper nanocatalyst according to any one of claims 1 to 3, characterized in that: The divalent copper salt is selected from one or more of copper nitrate, copper sulfate, and copper chloride; The fluoride salt is selected from ammonium fluoride or sodium fluoride.
5. The method for preparing a copper nanocatalyst according to any one of claims 1 to 4, characterized in that: The preparation method further comprises: performing LSV scanning on the copper nanocatalyst prepared by electrochemical deposition; Preferably, the LSV scanning process is as follows: selecting at least three different scanning ranges in the voltage range of 0 to -3 V and scanning in sequence, with a scanning speed of 20 to 50 mV / s; More preferably, the scanning range of the LSV scan is at least 3 of 0 to -2.5 V, 0 to -2 V, 0 to -1.5 V, 0 to -1 V, 0 to -0.5 V, 0 to -0.25 V, and -0.15 to -0.25 V, preferably 3 to 6; Preferably, the LSV scan uses a KHCO3 solution with a concentration of 0.5 to 2 mol / L as the electrolyte.
6. The method for preparing a copper nanocatalyst according to any one of claims 1 to 5, characterized in that: The electrochemical deposition process includes: depositing in a forward direction for 10 to 60 seconds under an applied current of 200 to +800 mA; and then immediately depositing in a reverse direction for 2 to 10 minutes under an applied current of -200 to -800 mA. Preferably, the stirring is performed at a speed of 200 to 600 r / min during the electrochemical deposition process.
7. A copper nanocatalyst prepared according to the preparation method of any one of claims 1 to 6; Preferably, the copper nanocatalyst is in the shape of a sea urchin; More preferably, the copper nanocatalyst is supported on the working electrode cathode of the three-electrode system.
8. Use of the copper nanocatalyst according to claim 7 in electrocatalytic reduction of CO2.
9. A method for electrocatalytic reduction of CO2, characterized in that: Using the copper nanocatalyst according to claim 7 as an electroreduction catalyst; Preferably, the method for electrocatalytic reduction of CO2 uses the electrode loaded with the copper nanocatalyst as the working electrode cathode, places it in the cathode electrolyte, and introduces CO2 into the cathode electrolyte to prepare an electrocatalytic reduction product mainly composed of ethanol.
10. The method for electrocatalytic reduction of CO2 according to claim 9, characterized in that: The electrolyte is a KHCO3 solution with a concentration of 0.5 to 2 mol / L; the potential is -0.3 to -1 V (vs. RHE), the electrolysis time is 0.5 to 2 h; and the flow rate of continuous CO2 is 20 to 50 mL / min.