Modified polypropylene composite material as well as preparation method and application thereof
By introducing two-dimensional functional fillers and supercritical assisted reactive extrusion process, modified polypropylene composite materials were prepared, which solved the bottlenecks of existing materials in terms of dimensional stability, mechanical properties and functional integration, and achieved high rigidity, low shrinkage and multifunctional material properties, which are suitable for new energy vehicles and precision electronics.
Patent Information
- Application Number
- CN202511144609.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-15
- Publication Date
- 2025-10-24
AI Technical Summary
Existing modified polypropylene composite materials have significant bottlenecks in terms of dimensional stability, mechanical properties, functional integration, and green processing, making it difficult to meet the application requirements of high-end fields such as new energy vehicles, rail transit, and medical devices.
Modified polypropylene composite materials are prepared by supercritical-assisted reaction extrusion process using two-dimensional functional fillers, multiphase toughening agents, dynamic crosslinkers, flame retardants, antistatic agents and light stabilizers to form a micro-nano closed-cell structure and achieve efficient blending and in-situ interfacial reaction.
It significantly inhibits the growth of polypropylene spherulites, improves material rigidity and dimensional stability, enhances impact toughness, and possesses thermal conductivity, flame retardancy, and antistatic properties, enabling green processing and meeting the application requirements of high precision and high performance.
Smart Images

Figure CN120829644A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the technical field of high polymer materials, and particularly relates to a modified polypropylene composite material and a preparation method and application thereof. BACKGROUND
[0002] Polypropylene (PP) is a general-purpose polyolefin material with excellent performance and low cost. It is widely used in many fields such as automobiles, electronics, construction, and packaging due to its good comprehensive physical properties, chemical corrosion resistance, excellent processability, and high specific strength. However, as the high-end manufacturing industry puts forward higher requirements for the comprehensive performance of materials, the performance bottleneck of existing polypropylene-based composites is increasingly prominent, and it is difficult to meet the urgent demand for high-performance and high-reliability materials in the fields of new energy vehicles, rail transit, medical devices, and precision electronics.
[0003] The main performance shortcomings of existing polypropylene materials are as follows. First, due to the high crystallinity and fast crystallization rate of polypropylene molecular chains, large spherulite structures are easily formed during molding and processing, resulting in large volume shrinkage of the product, and the molding shrinkage rate is generally higher than 1.5%, which seriously affects the dimensional accuracy and stability of the product and limits its application in high-precision part manufacturing. At the same time, polypropylene exhibits poor impact toughness at low temperatures and is prone to brittle fracture failure, further restricting its application expansion in harsh environmental conditions.
[0004] To improve the dimensional stability and mechanical properties of polypropylene, existing technologies generally use reinforcing fillers (such as glass fibers, carbon fibers, and wollastonite) and toughening agents (such as rubbers and polyolefin elastomers) for synergistic modification. However, this modification approach has inherent technical defects. The polarity difference between the reinforcing filler and the polypropylene matrix is large, and the interface compatibility is poor, resulting in poor dispersion of the filler and low interfacial adhesion, which easily forms interface cavities and defects, and further leads to stress concentration in the composite material, making it difficult to improve the overall mechanical properties and dimensional stability. Although the addition of coupling agents and compatibilizers can improve the interfacial adhesion to some extent, existing compatibilizers are mostly maleic anhydride grafted polyolefins, which lack efficient interfacial activity regulation capability and are difficult to achieve interfacial strengthening and performance balance at high filler rates. In addition, the introduction of toughening agents can improve the impact performance of polypropylene, but often accompanied by a significant decrease in rigidity, and further increases the shrinkage rate, exacerbating the performance contradiction of the material, and cannot balance the rigidity and toughness and dimensional stability.
[0005] More importantly, the existing modified polypropylene composites mainly focus on mechanical properties and dimensional stability, lack of thermal conductivity, flame retardant, antistatic, low VOC release and other multifunctional integration, and are difficult to meet the application requirements of high value-added fields such as new energy vehicle power battery shell, high-speed communication equipment and medical equipment shell. At the same time, the existing modification process generally uses traditional melt blending and extrusion granulation method, the dispersion efficiency of the filler is low, the interface control means is limited, the energy consumption is high and the environmental pollution is serious in the processing process, which is difficult to adapt to the development trend of green manufacturing and low carbon environmental protection.
[0006] Therefore, the existing modified polypropylene composites still have significant bottlenecks in dimensional stability, mechanical properties, functional integration and green processing. It is urgent to provide a new type of modified polypropylene composite material, which breaks through the above technical limitations through innovative material system design and preparation process. SUMMARY
[0007] The technical problem to be solved by the present application is to provide a modified polypropylene composite material and its preparation method and application to solve the problems mentioned in the background art or achieve better technical effects.
[0008] In order to solve the above technical problems, the present application discloses a modified polypropylene composite material, each component includes 50-80 parts by weight of polypropylene, 2-10 parts by weight of two-dimensional functional filler, 5-20 parts by weight of multi-phase toughening agent, 0.5-3 parts by weight of dynamic crosslinking agent, 5-15 parts by weight of flame retardant, 0.5-2 parts by weight of antistatic agent, 0.1-1.5 parts by weight of antioxidant and 0.1-2 parts by weight of light stabilizer.
[0009] The two-dimensional functional filler is selected from one or more of fumed silica, graphene, carbon nanosheet and MXene. These two-dimensional materials have extremely high specific surface area, which can effectively act as a heterogeneous nucleating agent to inhibit the formation of PP large spherulites, thereby fundamentally reducing the molding shrinkage of the material.
[0010] The two-dimensional functional filler is surface-activated by a reactive compatibilizer containing epoxy, carboxyl or amino group to form a reactive layer. The amount of reactive compatibilizer is 5% to 30% of the weight of the two-dimensional functional filler. This activation treatment gives the non-polar filler surface chemical reactivity, laying a foundation for subsequent firm combination with the matrix and crosslinking agent.
[0011] Further, each component includes 50 parts by weight of polypropylene, 10 parts by weight of two-dimensional functional filler, 20 parts by weight of multi-phase toughening agent, 3 parts by weight of dynamic crosslinking agent, 15 parts by weight of flame retardant, 0.5 parts by weight of antistatic agent, 1.5 parts by weight of antioxidant and 0.5 parts by weight of light stabilizer.
[0012] Further, the multi-phase toughening agent is selected from one or both of polyolefin elastomer microparticles of hard core and soft shell structure and liquid crystal polymer microfibers. The system synergistically acts through multiple toughening mechanisms to greatly improve the impact toughness of the material without significantly sacrificing rigidity.
[0013] Further, the dynamic crosslinking agent is selected from one or both of a bis-olefinic silane and an isocyanate group reaction type crosslinking agent.
[0014] Further, the flame retardant is a phosphorus-nitrogen synergistic type halogen-free flame retardant selected from one or more of a red phosphorus coated flame retardant, ammonium polyphosphate, melamine polyphosphate, and dipentaerythritol phosphate.
[0015] Further, the antistatic agent is selected from one or more of conductive carbon black, conductive carbon nanotubes, graphene, and quaternary ammonium salt modified ionic antistatic agents.
[0016] Further, the antioxidant is selected from one or more of a hindered phenol primary antioxidant, a phosphite and a sulfide auxiliary antioxidant; and the light stabilizer is selected from one or both of a hindered amine light stabilizer and an ultraviolet absorber.
[0017] Further, the preparation method of any of the modified polypropylene composite materials described above is as follows:
[0018] (1) Surface activation treatment of two-dimensional functional fillers: a reactive compatibilizer containing an epoxy group, a carboxyl group, or an amine group is used to perform surface activation treatment on the two-dimensional functional fillers to form a reactive layer; the reactive compatibilizer containing an epoxy group is polypropylene grafted glycidyl methacrylate or an epoxy resin; the reactive compatibilizer containing a carboxyl group is polypropylene grafted maleic anhydride; and the reactive compatibilizer containing an amino group is an amino silane coupling agent, such as 3-aminopropyl triethoxysilane.
[0019] (2) Supercritical assisted reaction extrusion: the modified fillers obtained in step (1), polypropylene, a multi-phase toughening agent, a dynamic crosslinking agent, a flame retardant, an antistatic agent, an antioxidant, and a light stabilizer are jointly added to a high-shear reaction extruder under the conditions of 180-230°C and 200-400 rpm, and supercritical CO2 is injected to build a micro-nano closed pore structure, achieve efficient blending, in-situ interface reaction, and structure regulation, and obtain a functional modified polypropylene composite material.
[0020] (3) Pelletizing and post-treatment: the functional modified polypropylene composite material obtained is extrusion pelletized and annealed at 110-150°C to obtain a modified polypropylene composite material.
[0021] Further, in step (2), the pressure of the injected supercritical CO2 is 7-10 MPa, and the duration is 5-20 min.
[0022] Further, the modified polypropylene composite material of any of the above applications in new energy vehicles, battery shell, medical equipment, precision electronic structural parts and rail transit equipment.
[0023] Compared with the prior art, the beneficial effects of the present application are as follows:
[0024] (1) The present application significantly inhibits the excessive growth of polypropylene spherulites by introducing two-dimensional functional fillers with high specific surface area, excellent thermal conductivity and outstanding interfacial activity, systematically improves the rigidity, heat resistance and dimensional stability of the material, and stabilizes the 24h molding shrinkage rate to below 0.08%, which can meet the strict tolerance requirements of high-precision fields such as new energy vehicle battery boxes and precision electronic shells.
[0025] (2) The present application significantly improves the impact strength of the material, especially the low-temperature impact toughness, while maintaining high rigidity, through the synergistic effect of dual dynamic crosslinking network and multiphase toughening system, solving the contradiction between rigidity and toughness of traditional modified PP.
[0026] (3) The present application makes the material integrally possess UL-94 V-0 level halogen-free flame retardant and controllable surface resistance in the range of 10 6 ~ 10 9 Ω by introducing phosphorus-nitrogen synergistic flame retardant and composite antistatic agent, combined with the thermal conductivity improvement brought by two-dimensional fillers, building a "thermal management-flame retardant-antistatic" integrated solution.
[0027] (4) The present application realizes efficient and uniform dispersion of fillers, compatibilizers and toughening agents in the polypropylene matrix by using high-shear reactive extrusion process combined with supercritical CO2 assisted micro-nano controlled pore technology, promotes in-situ interface reaction, significantly reduces stress concentration caused by filler agglomeration during processing, further reduces the risk of warping, deformation and cracking of the product, realizes lightweight and green processing of the material, reduces the overall manufacturing cost, and improves the stability and controllability of the material during processing and molding. BRIEF DESCRIPTION OF DRAWINGS
[0028] Figure 1 The modified polypropylene composite material prepared in Example 1 of the present application is shown in the scanning electron microscope surface morphology diagram. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific embodiments of the present application will be described in detail below.
[0030] The raw materials or reagents used in the following examples and comparative examples are commercially available products or prepared by conventional technical means unless otherwise specified.
[0031] The gas-phase silicon dioxide, graphene, carbon nanosheet and MXene are purchased from Nanjing Xianfeng Nanometer Material Technology Co., Ltd.
[0032] The polyolefin elastomer microparticle with hard core and soft shell structure and liquid crystal polymer microfiber are purchased from Dow Chemical Company.
[0033] The diene-based silane (vinyl trimethoxysilane) and isocyanate group reaction type crosslinking agent (4,4'-diphenyl methane diisocyanate) are purchased from Wanhua Chemical Group Co., Ltd.
[0034] The red phosphorus coated flame retardant, ammonium polyphosphate, melamine polyphosphate and dipentaerythritol phosphate are purchased from Jiangsu Yakke Technology Co., Ltd.
[0035] The conductive carbon black, conductive carbon nanotube, graphene and quaternary ammonium salt modified ionic antistatic agent are purchased from Shanghai Titan Technology Co., Ltd.
[0036] The antioxidant: the main antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1010); the auxiliary antioxidant is tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168), both of which are purchased from BASF.
[0037] The light stabilizer: bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (light stabilizer 770) is purchased from BASF.
[0038] The detection methods of the modified polypropylene composite materials in the following examples and comparative examples are as follows:
[0039] The test of 24h shrinkage rate (%) is carried out according to GB / T 33924-2017 (equivalent to ISO 294-4:2017). The material is injection molded into a sample plate of 120mm×120mm×3mm, and after being placed in an environment of 23±2℃ and relative humidity of 50±5% for 24 hours, the shrinkage rates in the parallel and vertical flow directions are respectively measured, and the average value can be given as needed.
[0040] The test of tensile strength (MPa) is carried out according to GB / T 1040.2-2022 (equivalent to ISO 527-2:2012), using type 1A dumbbell-shaped sample, and the test speed is 50mm / min.
[0041] The impact strength (kJ / m 2 ): The test is carried out according to GB / T 1043.1-2008 (simply supported beam impact, A-type notch, edgewise impact, equivalent to ISO 179-1:2000).
[0042] Thermal conductivity (W / mK): tested by Transient Plane Source (TPS) method, according to GB / T 32064-2015 (equivalent to ISO 22007-2:2008).
[0043] Surface resistance (Ω): tested according to GB / T 1410-2006 (equivalent to ASTM D257-99), test voltage is 500V, test ambient temperature is 21-25℃, relative humidity is 45-55%.
[0044] Flame retardant grade: tested according to UL-94 Vertical Burning Test Vertical Method (UL-94V). Five 127mm x 12.7mm x thickness samples are conditioned at 23℃, 50% RH for 48 hours. The samples are clamped vertically, and a cotton ball is placed 150mm below the sample. A 20mm high Bunsen burner flame is used to vertically burn the free end of the sample for 10 seconds, then the flame is removed. The flame-out time is recorded, then the sample is re-ignited for 10 seconds, then the flame is removed again. The second flame-out time and whether the falling molten drops ignite the cotton are recorded. According to the UL-94 standard, if the flame is extinguished within 10 seconds after the flame is removed each time, and there are no burning molten drops to ignite the cotton, the sample meets the V-0 level requirement; if the flame-out time is within 30 seconds and there is no ignition of cotton, it is V-1; if there are molten drops to ignite the cotton or the burning time is longer, it is V-2 or unqualified. The flame retardant grade results in this paper are evaluated according to the UL-94V standard.
[0045] Example 1
[0046] A modified polypropylene composite material, by weight, each component includes: 70 parts of polypropylene, 5 parts of modified silica, 8 parts of POE / SEBS toughening agent with hard core and soft shell structure, 2 parts of bis-olefinic silane dynamic crosslinking agent, 10 parts of nitrogen-phosphorus synergistic halogen-free flame retardant, 1 part of conductive carbon black, 1 part of antioxidant system (1010 / 168 mass ratio is 1:2), 1 part of light stabilizer 770.
[0047] The preparation method of the above modified polypropylene composite material, the steps are as follows:
[0048] (1) 5 parts of fumed silica is surface modified in 0.5 parts of 3-aminopropyl triethoxysilane ethanol solution, stirred at room temperature for 30 minutes, then dried at 80℃ for 2 hours to obtain modified silica; the ethoxy group of 3-aminopropyl triethoxysilane is hydrolyzed into silicon hydroxyl, which reacts with the hydroxyl group on the surface of silica, and the amino group is exposed outside to form a surface layer with reactivity;
[0049] (2) 70 parts of polypropylene and 5 parts of the activated silica obtained in step (1) are fed into an extruder (a twin-screw extruder with a length-diameter ratio of 48:1) from the main feeding port, and after the polymer is completely melted at the middle section (5th zone) of the extruder, a mixed liquid of 8 parts of a hard-soft shell structure POE / SEBS toughener, 2 parts of a bis-olefinic silane dynamic crosslinking agent, 10 parts of a nitrogen-phosphorus synergistic halogen-free flame retardant, 1 part of conductive carbon black, 1 part of an antioxidant system and 1 part of a light stabilizer is injected through a liquid metering pump; at the end of the extruder, 8 MPa of supercritical CO2 is injected through a high-pressure pump. The temperature of each zone of the extruder is set to 180 / 190 / 200 / 210 / 210 / 200 / 190 / 190 / 180°C, and the screw rotation speed is 250 rpm. The residence time of the material in the extruder is about 15 minutes. This segmented feeding mode can ensure that the fillers are preliminarily dispersed before the polymer is melted, and the reactive aids are added after the reduction of the melt viscosity, so as to improve the reaction efficiency and reduce the degradation of the polymer.
[0050] (3) The mixture obtained in step (2) is granulated by a twin-screw extruder and annealed at 120°C for 4 hours to obtain a modified polypropylene composite material, as shown in Figure 1
[0051] Example 2
[0052] A modified polypropylene composite material, each component includes, by weight parts: 65 parts of polypropylene, 6 parts of modified graphene, 15 parts of liquid crystal polymer microfiber toughener, 1.5 parts of 4,4-diphenyl methane diisocyanate, 10 parts of melamine polyphosphate, 1 part of conductive nanocarbon tube, 1 part of antioxidant, 1 part of quaternary ammonium salt type antistatic agent and 1 part of light stabilizer 770.
[0053] The preparation method of the above modified polypropylene composite material, the steps are as follows:
[0054] (1) 6 parts of graphene sheet is dispersed in 1.5 parts of polypropylene grafted maleic anhydride xylene solution, heated to 120°C and stirred for 60 minutes. The anhydride groups of polypropylene grafted maleic anhydride react with the oxygen-containing functional groups (such as -OH) on the edge of graphene through esterification reaction, or are adsorbed on the surface of graphene through van der Waals force to form a reactive layer. Then vacuum dried at 80°C for 2 hours to obtain modified graphene;
[0055] (2) 65 parts of polypropylene, 6 parts of modified graphene are added from the main feeding port, 15 parts of liquid crystal polymer micro-fiber toughening agent, 1.5 parts of 4, 4-diphenyl methane diisocyanate, 1.5 parts of 3-aminopropyl triethoxysilane, 10 parts of melamine polyphosphate, 1 part of conductive nanocarbon tube, 1 part of antioxidant, 1 part of quaternary ammonium salt type antistatic agent and 1 part of light stabilizer mixture are added in the middle. 9 MPa of supercritical CO2 is injected at the end. The extruder temperature is set to 185 / 195 / 205 / 215 / 215 / 205 / 195 / 195 / 185℃, and the screw rotation speed is 300 rpm.
[0056] (3) The mixture obtained in step (2) is granulated by double screw extrusion, and annealed at 130℃ for 6 hours to obtain a modified polypropylene composite material.
[0057] Example 3
[0058] A modified polypropylene composite material, each component includes, by weight: 72 parts of polypropylene, 7 parts of modified carbon nanosheet, 10 parts of POE / PA multi-phase toughening agent, 2 parts of 4, 4-diphenyl methane diisocyanate, 12 parts of ammonium polyphosphate flame retardant, 1.5 parts of conductive carbon black, 1 part of antioxidant, 0.5 parts of light stabilizer.
[0059] The preparation method of the above modified polypropylene composite material, the steps are as follows:
[0060] (1) 7 parts of carbon nanosheet are dispersed in toluene solution containing 1 part of polypropylene grafted maleic anhydride, heated to 110℃ and stirred for 50 minutes, the epoxy group of polypropylene grafted maleic anhydride reacts with the carboxyl or hydroxyl group at the edge of carbon nanosheet to form stable chemical bond. Then vacuum dried at 90℃ for 2 hours to obtain modified carbon nanosheet;
[0061] (2) 72 parts of polypropylene, 7 parts of modified carbon nanosheet are added from the main feeding port, 10 parts of POE / SEBS multi-phase toughening agent, 2 parts of 4, 4-diphenyl methane diisocyanate, 12 parts of ammonium polyphosphate flame retardant, 1.5 parts of conductive carbon black, 1 part of antioxidant, 0.5 parts of light stabilizer are added in the middle. 7 MPa of supercritical CO2 is injected at the end. The extruder temperature is set to 175 / 185 / 195 / 205 / 205 / 195 / 185 / 185 / 175℃, and the screw rotation speed is 250 rpm;
[0062] (3) The mixture obtained in step (2) is granulated by double screw extrusion, and annealed at 110℃ for 4 hours to obtain a modified polypropylene composite material.
[0063] Example 4
[0064] A modified polypropylene composite material, by weight fraction, each component includes: 60 parts of polypropylene, 8 parts of MXene nanosheet, 12 parts of SEBS toughening agent, 3 parts of bis-alkenyl silane crosslinking agent, 15 parts of red phosphorus coated flame retardant, 1 part of conductive carbon nanotube, 1 part of antioxidant, 1 part of light stabilizer.
[0065] The preparation method of the above-mentioned modified polypropylene composite material, the steps are as follows:
[0066] (1) 8 parts of MXene nanosheet is dispersed in isopropyl alcohol / water mixed solvent containing 2 parts of polypropylene grafted maleic anhydride, the abundant-OH, -F and other functional groups on the surface of MXene react with the epoxy groups of polypropylene grafted maleic anhydride to form strong interfacial bonding. After stirring at 55℃ for 50 minutes, vacuum drying at 80℃ for 2 hours, modified MXene nanosheet is obtained;
[0067] (2) 60 parts of polypropylene, 8 parts of modified MXene nanosheet are added from the main feeding port, 12 parts of POE / SEBS toughening agent, 3 parts of vinyl trimethoxysilane, 15 parts of red phosphorus coated flame retardant, 1 part of conductive carbon nanotube, 1 part of antioxidant, 1 part of light stabilizer are added in the middle, and 10 MPa of supercritical CO2 is injected at the end. The temperature of the extruder is set to 190 / 200 / 210 / 220 / 220 / 210 / 200 / 200 / 190℃, and the screw rotation speed is 350 rpm;
[0068] (3) The mixture obtained in step (2) is granulated by double screw extrusion, and annealed at 140℃ for 5 hours to obtain the modified polypropylene composite material.
[0069] Example 5
[0070] A modified polypropylene composite material, by weight fraction, each component includes: 80 parts of polypropylene, 2 parts of fumed silica, 5 parts of POE / SEBS toughening agent, 0.5 parts of vinyl trimethoxysilane, 5 parts of ammonium polyphosphate, 2 parts of conductive carbon black, 0.1 parts of antioxidant system and 0.1 parts of light stabilizer.
[0071] The preparation method of the above-mentioned modified polypropylene composite material is the same as example 1, wherein the supercritical carbon dioxide assisted reaction pressure is 7 MPa, the extrusion temperature is 180℃, the rotation speed is 200 rpm, and the annealing temperature is 110℃.
[0072] Example 6
[0073] A modified polypropylene composite material, each component includes, by weight fraction: 50 parts of polypropylene, 10 parts of graphene, 20 parts of liquid crystal polymer microfiber, 3 parts of a mixture of vinyl trimethoxysilane and 4, 4-diphenyl methane diisocyanate (mass ratio 1:1), 15 parts of melamine polyphosphate, 0.5 parts of conductive carbon nanotube, 1.5 parts of antioxidant system and 2.0 parts of light stabilizer.
[0074] The preparation method of the above modified polypropylene composite material is the same as that in Example 2, wherein the supercritical carbon dioxide assisted reaction pressure is 15 MPa, the extrusion temperature is 230℃, the rotation speed is 400 rpm, and the annealing temperature is 150℃.
[0075] Example 7
[0076] A modified polypropylene composite material, each component includes, by weight fraction: 80 parts of polypropylene, 2 parts of MXene, 5 parts of liquid crystal polymer microfiber, 0.5 parts of 4, 4-diphenyl methane diisocyanate, 5 parts of red phosphorus coated flame retardant, 2 parts of quaternary ammonium salt antistatic agent, 0.1 parts of antioxidant system and 0.1 parts of light stabilizer.
[0077] The preparation method of the above modified polypropylene composite material is the same as that in Example 4, wherein the supercritical carbon dioxide assisted reaction pressure is 7 MPa, the extrusion temperature is 180℃, the rotation speed is 200 rpm, and the annealing temperature is 110℃.
[0078] Example 8
[0079] A modified polypropylene composite material, each component includes, by weight fraction: 50 parts of polypropylene, 10 parts of modified carbon nanosheet, 20 parts of POE / SEBS toughening agent, 3 parts of vinyl trimethoxysilane, 15 parts of ammonium polyphosphate, 0.5 parts of graphene (as antistatic agent), 1.5 parts of antioxidant system and 0.5 parts of light stabilizer.
[0080] The preparation method of the above modified polypropylene composite material is the same as that in Example 3, wherein the supercritical carbon dioxide assisted reaction pressure is 15 MPa, the extrusion temperature is 230℃, the rotation speed is 400 rpm, and the annealing temperature is 150℃.
[0081] Comparative Example 1
[0082] A modified polypropylene composite material has exactly the same formula as Example 4, but no supercritical CO2 is injected in the preparation step (2), and the rest of the process parameters remain the same.
[0083] Comparative Example 2
[0084] The formula is similar to Example 4, but the amount of two-dimensional functional filler MXene is increased to 15 parts, and the rest of the components and process parameters are the same as Example 4.
[0085] Comparative Example 3
[0086] The formulation is exactly the same as Example 4, but in the preparation step (1), polypropylene grafted maleic anhydride is not used for surface activation treatment of MXene, and untreated MXene is directly used for subsequent extrusion, and the remaining process parameters are the same as Example 4.
[0087] The modified polypropylene composite materials prepared in Examples 1-8 and Comparative Examples 1-3 above are injection molded (injection molding machine model: Haitian MA1200 II, barrel temperature 190-220℃, mold temperature 80℃, injection pressure 90MPa, holding pressure 60MPa), and then their various properties are tested according to the standard method described above, and the test results are shown in Table 1.
[0088] Table 1 Comparison of various properties of modified polypropylene composite materials prepared in Examples 1-8 and Comparative Examples 1-3
[0089]
[0090]
[0091] From the comparison of the data in Table 1 above, it can be seen that, comparing Example 4 with Comparative Example 1, under the condition that the formulations are exactly the same, Example 4 using scCO2 assisted process, its shrinkage rate is sharply reduced from 1.35% to 0.075%, the tensile strength is increased from 60.1MPa to 78.2MPa, and the impact strength is increased from 15.3kJ / m 2 to 29.4kJ / m 2 . This fully proves that the introduction of supercritical carbon dioxide assisted reaction is the key to achieving a leap in performance. The mechanism lies in that the plasticizing effect of supercritical carbon dioxide assisted reaction improves the dispersion of fillers and reduces the internal stress caused by agglomeration; the reaction enhancement effect promotes the interfacial bonding and matrix crosslinking; the closed cell structure formed by the micro-foaming effect can effectively absorb and dissipate impact energy, acting as a crack termination point, thereby simultaneously improving the dimensional stability and mechanical properties. In addition, the introduction of supercritical carbon dioxide assisted reaction also improves the dispersion of the flame retardant, making the flame retardant grade increase from V-1 to V-0.
[0092] Comparing Example 4 with Comparative Example 3, it can be seen that surface activation treatment of two-dimensional fillers is crucial. The unactivated filler (Comparative Example 3) has weak interfacial bonding with the matrix, resulting in ineffective stress transmission, and the mechanical properties (tensile strength of Comparative Example 3 is 55.4MPa, impact strength is 18.2kJ / m 2 ; while the tensile strength of Example 4 is 78.2MPa, and the impact strength is 29.4kJ / m 2) and the shrinkage is also much higher than that of the activated sample. The difference in the interface bonding strength can be verified by dynamic mechanical analysis (DMA). The material of Comparative Example 3 shows a higher peak of loss factor near the glass transition temperature than that of Example 4, indicating that there is more segment free motion and energy dissipation in the interface region, i.e. the interface bonding is poor, which weakens the movement ability of the matrix segments.
[0093] Comparative Example 4 and Comparative Example 2, when the amount of two-dimensional filler is too much (beyond the defined range of the present application), although the shrinkage is reduced, due to the increased tendency of filler agglomeration, defects are generated in the material, and the impact strength and tensile strength are both significantly decreased.
[0094] Examples 1-8 of the present application all exhibit excellent comprehensive performance, especially Examples 2 and 6 which use a combination of ethenyltrimethoxysilane and 4,4-diphenylmethane diisocyanate crosslinking system, achieving the highest mechanical properties. This proves the effectiveness of the synergistic effect of “matrix crosslinking” and “interface crosslinking”. The formation of this network can be further characterized by dynamic rheology testing. The material of the present application exhibits a feature of higher storage modulus than loss modulus and a platform in the low frequency region, which is a typical crosslinking network behavior, indicating that the material has formed a stable three-dimensional network structure in the molten state, which endows the material with excellent creep resistance and dimensional stability.
[0095] Example 9
[0096] The modified polypropylene composite particles prepared in Example 8 are prepared into the upper cover of a certain model of new energy vehicle power battery by injection molding process under the conditions of mold temperature 80℃, injection pressure 90MPa, and holding pressure 60MPa.
[0097] After detection, compared with the battery upper cover made of 30% glass fiber reinforced PP (GF30-PP) commonly used in the prior art, the product of the present application has the following significant advantages:
[0098] Lightweight: due to the microporous structure formed by the supercritical carbon dioxide assisted reaction in the preparation process, the density of the product of the present application is about 1.05g / cm 3 , which is about 8.7% lower than that of GF30-PP (density about 1.15g / cm 3 ), achieving effective weight reduction, which helps to improve the vehicle's cruising range;
[0099] High precision and high sealing: the molding shrinkage of the product is less than 0.08%, far lower than GF30-PP (usually 0.2-0.5%), which ensures the high matching precision between the battery cover and the battery box, improves the overall sealing performance (IP level) of the battery pack, and is crucial for preventing moisture intrusion and ensuring battery safety;
[0100] Comprehensive safety improvement: the flame retardant grade of the product reaches UL-94V-0, which is better than ordinary GF30-PP (usually HB or V-2 level), and meets the stringent fire safety standards of power batteries. At the same time, the surface resistance is 1x10 6 Ω, which is within the range of static electricity dissipation, can effectively prevent the electric spark caused by static electricity accumulation, and further improves the safety;
[0101] Design freedom and appearance: compared with GF30-PP containing long glass fibers, the material has better flowability, no fiber floating phenomenon on the surface, better product appearance quality, and more advantages in designing thin-walled and complex structure parts.
[0102] The modified polypropylene composite material provided by the application successfully integrates multiple properties such as low shrinkage, high toughness, high strength, lightweight, flame retardance and antistatic property, and provides a performance excellent and cost competitive solution for high-end application fields such as new energy automobile battery systems.
Claims
1. A modified polypropylene composite, characterized in that, The components include, by weight fraction, 50-80 parts of polypropylene, 2-10 parts of two-dimensional functional filler, 5-20 parts of multi-phase toughening agent, 0.5-3 parts of dynamic crosslinking agent, 5-15 parts of flame retardant, 0.5-2 parts of antistatic agent, 0.1-1.5 parts of antioxidant, and 0.1-2 parts of light stabilizer. The two-dimensional functional filler is selected from one or more of fumed silica, graphene, carbon nanosheet, and MXene; the two-dimensional functional filler is surface-activated by a reactive compatibilizer containing an epoxy group, a carboxyl group, or an amino group to form a reactive layer; The reactive compatibilizer containing an epoxy group is polypropylene grafted glycidyl methacrylate or epoxy resin; the reactive compatibilizer containing a carboxyl group is polypropylene grafted maleic anhydride; and the reactive compatibilizer containing an amino group is amino silane coupling agent.
2. The modified polypropylene composite of claim 1, wherein, The components include, by weight fraction, 50 parts of polypropylene, 10 parts of two-dimensional functional filler, 20 parts of multi-phase toughening agent, 3 parts of dynamic crosslinking agent, 15 parts of flame retardant, 0.5 parts of antistatic agent, 1.5 parts of antioxidant, and 0.5 parts of light stabilizer.
3. The modified polypropylene composite of claim 1, wherein, The multi-phase toughening agent is selected from one or both of polyolefin elastomer microparticles with a hard core and soft shell structure and liquid crystal polymer microfibers.
4. The modified polypropylene composite of claim 1, wherein, The dynamic crosslinking agent is selected from one or both of bis-olefin silane and isocyanate group reactive crosslinking agent.
5. The modified polypropylene composite of claim 1, wherein, The flame retardant is a phosphorus-nitrogen synergistic halogen-free flame retardant selected from one or more of red phosphorus coated flame retardant, ammonium polyphosphate, melamine polyphosphate, and dipentaerythritol phosphate.
6. The modified polypropylene composite of claim 1, wherein, The antistatic agent is selected from one or more of conductive carbon black, conductive carbon nanotube, graphene, and quaternary ammonium salt modified ionic antistatic agent.
7. The modified polypropylene composite of claim 1, wherein, The antioxidant is selected from one or more of hindered phenol main antioxidant, phosphite and sulfide auxiliary antioxidant; and the light stabilizer is selected from one or both of hindered amine light stabilizer and ultraviolet absorber.
8. A process for the production of a modified polypropylene composite material as claimed in any one of claims 1 to 7, characterized in that The steps are as follows: (1) The two-dimensional functional filler is surface-activated by a reactive compatibilizer containing an epoxy group, a carboxyl group, or an amino group to form a reactive layer; (2) The modified filler obtained in step (1), polypropylene, multi-phase toughening agent, dynamic crosslinking agent, flame retardant, antistatic agent, antioxidant, and light stabilizer are jointly added into a high-shear reactive extruder under the conditions of 180-230℃ and 200-400rpm, and supercritical CO2 is injected to build micro-nano closed pore structure, realize efficient blending, in-situ interface reaction, and structure regulation, and obtain functional modified polypropylene composite material; (3) The functional modified polypropylene composite material obtained is extruded and granulated, and annealed at 110-150℃ to obtain the modified polypropylene composite material.
9. The preparation method according to claim 8, characterized in that In step (2), the pressure of the injected supercritical CO2 is 7-10MPa, and the duration is 5-20min.
10. Application of the modified polypropylene composite material of any one of claims 1-7 in new energy vehicles, battery cases, medical devices, precision electronic structural parts, and rail transit equipment.
Citation Information
Patent Citations
High-strength polypropylene foam bead and production technology
CN106566078A
Foamed polypropylene composite sheet and preparation method thereof
CN110549707A
Antistatic polypropylene foam material, preparation method thereof and semiconductor packaging material
CN114249918A
Halogen-free flame-retardant glass fiber modified polypropylene material and preparation method thereof
CN120230342A
Polypropylene resin composition with excellent conductivity and high stiffness
KR1020030053820A
Cited By
Cable preparation method and cable
CN121171717A