Composite anti-corrosion coating for medium heavy-duty anti-corrosion environment and preparation method of composite anti-corrosion coating

By modifying the waterborne epoxy system with fluorocarbon resin, directionally arranging nano-graphene, and using a solvent-free polyurea self-healing system, the problem of coating failure under heavy-duty anti-corrosion environments has been solved, achieving ultra-long durability and efficient self-healing, and reducing maintenance costs and corrosion rates.

CN120966319APending Publication Date: 2025-11-18TIANJIN JIZHI ENG CONSULTING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510956245.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-11
Publication Date
2025-11-18

AI Technical Summary

Technical Problem

Existing composite anti-corrosion coatings for heavy-duty anti-corrosion environments are prone to failure due to media penetration and material aging, especially under extreme conditions such as acid, alkali, salt solutions, and high-temperature water. The coatings are prone to cracking and peeling, requiring frequent maintenance.

Method used

A fluorocarbon resin-modified waterborne epoxy system combined with nano-graphene directional arrangement technology is used to form a labyrinth effect to block corrosive media. The top coating introduces a solvent-free polyurea and microcapsule self-healing system. The intermediate transition layer enhances the interlayer barrier function through directional graphene composite material. The three work together to build a dense protective network. The multi-layer composite coating is constructed by electric field-induced graphene arrangement and infrared curing.

Benefits of technology

It significantly extends the durability of the coating, and the self-healing system can actively repair micro-cracks, reduce the total life cycle maintenance cost, improve construction efficiency, reduce quality problems caused by improper substrate treatment, and reduce corrosion rate and failure probability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120966319A_ABST
    Figure CN120966319A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of anti-corrosion coatings, in particular to a composite anti-corrosion coating for a medium heavy-duty anti-corrosion environment and a preparation method of the composite anti-corrosion coating. According to the technical scheme, the composite anti-corrosion coating for the medium heavy anti-corrosion environment comprises the following components in percentage by mass: a bottom coating component, a middle transition layer component and a surface coating component, and the mass ratio of the bottom coating component to the middle transition layer component to the surface coating component is 33: 17: 50; the durability is improved through multi-dimensional material innovation, a fluorocarbon resin modified waterborne epoxy system is adopted for the bottom coating, and a nano graphene directional arrangement technology is combined, so that a labyrinth effect is formed, and a corrosion medium is blocked; a solvent-free polyurea and microcapsule self-repairing system is introduced into the surface coating, so that automatic repairing after damage is realized; the middle transition layer enhances the interlayer barrier function through the oriented graphene composite material, and the three layers cooperate to construct a compact protection network, so that the medium permeation path is obviously delayed, and the full-life-cycle maintenance cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of anticorrosive coatings, in particular to a composite anticorrosive coating for medium heavy-duty anticorrosive environment and a preparation method thereof. BACKGROUND

[0002] The composite anticorrosive coating for medium heavy-duty anticorrosive environment is a high-performance composite material developed for medium heavy-duty anticorrosive environments such as chemical equipment, offshore platforms, and sewage pipelines, which can resist long-term corrosion of strong corrosive media such as acid, alkali, salt, and high-temperature water vapor, and has a design life of more than 15 years.

[0003] The existing composite anticorrosive coating for medium heavy-duty anticorrosive environment is prone to failure in heavy-duty anticorrosive environments due to medium penetration and material aging, especially under extreme conditions such as acid, alkali, and salt solutions, and high-temperature water, and the coating is prone to cracking, peeling, and other problems, which requires frequent maintenance.

[0004] In view of the problem that the existing composite anticorrosive coating for medium heavy-duty anticorrosive environment is prone to failure in heavy-duty anticorrosive environments due to medium penetration and material aging, especially under extreme conditions such as acid, alkali, and salt solutions, and high-temperature water, and the coating is prone to cracking, peeling, and other problems, which requires frequent maintenance, the present application improves durability through multi-dimensional material innovation. The primer layer uses a fluorocarbon resin modified waterborne epoxy system combined with a directional graphene arrangement technology to form a labyrinth effect to block corrosive media. The topcoat layer introduces a solvent-free polyurea and a microcapsule self-repairing system to achieve automatic repair after damage. The intermediate transition layer enhances the interlayer barrier function through a directional graphene composite material, and the three work together to build a dense protective network, significantly delaying the medium penetration path. The improved coating has ultra-long durability, the chemical stability of fluorocarbon resin combined with the physical barrier effect of nano graphene effectively resists acid, alkali, and salt media corrosion. The self-repairing system can actively repair microcracks to avoid local failure causing overall damage. The directional graphene layer further blocks the electron path to inhibit electrochemical corrosion, significantly reducing the whole life cycle maintenance cost. SUMMARY

[0005] In order to overcome the problem that the existing composite anticorrosive coating for medium heavy-duty anticorrosive environment is prone to failure in heavy-duty anticorrosive environments due to medium penetration and material aging, especially under extreme conditions such as acid, alkali, and salt solutions, and high-temperature water, and the coating is prone to cracking, peeling, and other problems, which requires frequent maintenance.

[0006] The technical scheme of the present application is: a composite anticorrosive paint for medium heavy anti-corrosion environment, comprising the following components by mass percentage: base coat paint component, intermediate transition layer paint component and top coat paint component, the mass percentage of the base coat paint component, intermediate transition layer paint component and top coat paint component being 33:17:50, the base coat paint component specifically comprising the following components and component percentage: fluorocarbon resin 39%-41%, nano graphene 1%-3%, cashew nut shell oil epoxy resin 14%-16%, microcapsule A 2%-4%, curing agent 7%-9%, deionized water 29%-31% and auxiliary agent 1%-3%.

[0007] As preferred, the paint further comprises an intermediate transition layer paint component, the intermediate transition layer paint component specifically comprising the following components and component percentage: oriented graphene composite material 1%-2%, polyurea resin 34%-36%, nano titanium dioxide 1%-2% and bio-based plasticizer 4%-6%.

[0008] As preferred, the paint further comprises a top coat paint component, the top coat paint component specifically comprising the following components and component percentage: solvent-free polyurea 49%-51%, microcapsule B 4%-6%, nano zinc oxide 1%-3%, fluorosilicon modifier 2%-4% and curing accelerator 1%-3%.

[0009] As preferred, a preparation method of a composite anticorrosive paint for medium heavy anti-corrosion environment, comprising the following steps:

[0010] S11: dehydrating, dispersing, modifying and purifying the raw materials, and completing microcapsule activation and nano material surface modification;

[0011] S12: mixing the components in proportion, and preparing the base coat paint after stirring and defoaming;

[0012] S13: mixing the raw materials, and preparing the intermediate transition layer paint through stirring and filtering;

[0013] S14: mixing solvent-free polyurea, microcapsule B, nano zinc oxide and fluorosilicon modifier, and preparing the top coat paint after defoaming treatment;

[0014] S15: sequentially spraying the base coat, intermediate transition layer and top coat, and completing the construction of the multi-layer composite coating through electric field induced graphene arrangement and infrared curing;

[0015] S16: performing appearance inspection, film thickness measurement, adhesion test and salt spray resistance, impedance, self-repairing performance verification.

[0016] As preferred, when the raw material pretreatment and nano material functionalization are performed, the following steps are included:

[0017] S21: The fluorocarbon resin is placed in a vacuum drying oven, dehydrated at 80°C for 2 hours to remove residual moisture;

[0018] S22: The nanographene is mixed with ethanol at a mass ratio of 1:5, ultrasonically oscillated for 30 minutes to form a uniform suspension;

[0019] S23: 0.5% silane coupling agent is added to the cashew nut shell oil epoxy resin, stirred at 60°C for 1 hour to improve compatibility with the resin;

[0020] S24: The microcapsule A is placed in a 50°C constant temperature oven and dried for 12 hours to remove surface adsorbed moisture;

[0021] S25: The graphene is mixed with the polyurea resin at a mass ratio of 1:10, and ground to a particle size of ≤50μm by a three-roll mill;

[0022] S26: The bio-based plasticizer is filtered through a molecular sieve adsorption column to remove trace impurities;

[0023] S27: The nanometer zinc oxide is mixed with stearic acid at a mass ratio of 1:0.1, and melt blended at 120°C for 30 minutes to form a hydrophobic surface.

[0024] As preferred, when preparing the primer coating, the following steps are included:

[0025] S31: The fluorocarbon resin and nanographene suspension are added to the reaction kettle, stirred at 60°C for 1 hour;

[0026] S32: Slowly add the modified cashew nut shell oil epoxy resin, maintain the temperature at 60°C, and continue stirring for 30 minutes;

[0027] S33: The activated microcapsule A is added by vacuum suction to avoid agglomeration;

[0028] S34: Add the curing agent, adjust the pH to 8.5, and continue stirring for 20 minutes;

[0029] S35: Gradually add deionized water to control the viscosity to 2500-3000mPa·s;

[0030] S36: Add defoamer and dispersant, set the stirring speed to 200rpm at 50°C for 10 minutes;

[0031] S37: The mixture is placed in a vacuum defoaming machine for 15 minutes to remove bubbles.

[0032] As preferred, when preparing the intermediate transition layer coating, the following steps are included:

[0033] S41: Add polyurea resin to the reaction kettle, and heat to 80℃ under nitrogen protection, stir for 1 hour;

[0034] S42: Add the oriented graphene composite material through the screw feeder, maintain the temperature at 80℃, and stir for 30 minutes;

[0035] S43: Mix 1% concentration of nano-titanium dioxide with ethanol at a mass ratio of 1:3, and add the main material after ultrasonic dispersion for 15 minutes;

[0036] S44: Add a 5% concentration of bio-based plasticizer to adjust the flexibility of the system, and continue stirring for 20 minutes;

[0037] S45: Adjust the viscosity to 1800-2200 mPa·s by adding a small amount of deionized water, and set the temperature to 25℃;

[0038] S46: Add a 0.5% concentration of leveling agent, and stir at low speed for 10 minutes;

[0039] S47: Filter the mixed material through a 200-mesh filter to remove undispersed particles.

[0040] As preferred, when preparing the topcoat paint, the following steps are included:

[0041] S51: Place the solvent-free polyurea in the reaction kettle, heat to 70℃, and vacuum degas for 30 minutes;

[0042] S52: Disperse the microcapsule B uniformly in the polyurea system by an air flow crusher, maintain the temperature at 70℃, and stir for 20 minutes;

[0043] S53: Add the surface-modified nano-zinc oxide, and disperse at high speed for 15 minutes;

[0044] S54: Add a fluorosilicon modifier to adjust the surface energy, and continue stirring for 10 minutes;

[0045] S55: Mix the curing accelerator with a small amount of ethanol, and add it to the main material in a spray manner, and stir for 5 minutes;

[0046] S56: Adjust the viscosity to 3500-4000 mPa·s by adding a trace diluent with a concentration ≤1%, and set the temperature to 25℃;

[0047] S57: Place the mixed material in an ultrasonic debubbling instrument, set the frequency to 20kHz, and process for 10 minutes to ensure no bubbles.

[0048] As preferred, when performing interlayer compounding and molding, the following steps are included:

[0049] S61: Sandblast the metal substrate, ultrasonically clean it with acetone, and dry it;

[0050] S62: Adopt high pressure airless spray machine to spray primer, film thickness control 1.0mm, leveling at room temperature for 2 hours, 80 DEG C baking for 4 hours;

[0051] S63: Apply alternating current field on the surface of the primer, induce vertical arrangement of graphene, spin coating intermediate transition layer, film thickness 0.5mm;

[0052] S64: Intermediate transition layer is cured at room temperature for 24 hours to form an elastic buffer layer;

[0053] S65: Adopt electrostatic spraying process to spray topcoat, film thickness 1.5mm, infrared radiation curing for 30 minutes, set wavelength 3-5um, intensity 100W / cm 2 ;

[0054] S66: Test interlayer adhesion by drawing method, ensure interlayer bonding strength ≥5MPa;

[0055] S67: The edges of the coating are sealed with polyurea sealant to prevent medium penetration.

[0056] As preferred, during post-processing and performance verification, the following steps are included:

[0057] S71: Visually inspect the coating surface to detect whether there are pinholes, cracks and sagging defects;

[0058] S72: Use a coating thickness gauge to detect the thickness of each layer, film thickness deviation ≤±10%;

[0059] S73: Perform crosshatch adhesion test according to GB / T 9286 standard, adhesion rating ≤1 level;

[0060] S74: Perform 4000 hour neutral salt spray test according to GB / T 1771 standard, no corrosion propagation at scratch;

[0061] S75: Test by electrochemical impedance spectroscopy, low frequency impedance modulus value ≥1×10 9 Ω·cm2;

[0062] S76: Manually create a 500um wide scratch, observe the self-repairing effect by microscope within 24 hours, repair rate ≥85%;

[0063] S77: Detect VOC content according to GB 18582-2020 standard, ensure environmental protection index detection ≤50g / L.

[0064] The beneficial effects of the present application are:

[0065] 1. Existing composite anti-corrosion coatings for heavy-duty environments are prone to failure due to media penetration and material aging, especially under extreme conditions such as acid, alkali, salt solutions, and high-temperature water. These coatings are susceptible to cracking and peeling, requiring frequent maintenance. This solution enhances durability through multi-dimensional material innovation. The base coat uses a fluorocarbon resin-modified waterborne epoxy system combined with oriented graphene nanoparticles to create a labyrinth effect that blocks corrosive media. The top coat incorporates solvent-free polyurea and a microcapsule self-healing system for automatic repair after damage. The intermediate transition layer enhances the interlayer barrier function through oriented graphene composite materials. These three elements work together to construct a dense protective network, significantly slowing down media penetration. The improved coating exhibits ultra-long durability. The chemical stability of the fluorocarbon resin combined with the physical barrier effect of the graphene nanoparticles effectively resists corrosion from acids, alkalis, and salts. The self-healing system actively repairs microcracks, preventing localized failure from leading to overall destruction. The oriented graphene layer further blocks electronic pathways, inhibiting electrochemical corrosion and significantly reducing the total life-cycle maintenance cost.

[0066] 2. Existing composite anti-corrosion coatings for heavy-duty anti-corrosion environments require multiple layers and come in various models, placing high demands on the technical skills of the construction team. Rigid coatings also have strict requirements for substrate preparation, resulting in low construction efficiency and unstable quality. This solution optimizes the coating system and construction process. The base coat uses a water-based system, supporting minimal surface preparation and simplifying the pretreatment process. The intermediate transition layer uses an electric field to control the directional arrangement of graphene, achieving improved adhesion for thin layers. The top coat uses solvent-free polyurea, supporting multiple processes such as spraying and roller coating. At the same time, bio-based solvents replace traditional solvents, reducing the requirements for the construction environment, effectively improving the construction efficiency of a single project, and reducing quality problems caused by improper substrate preparation.

[0067] 3. Existing composite anti-corrosion coatings for heavy-duty environments, while complementary in performance to the topcoat, lack tight bonding. For example, the BY01 primer has a high water absorption rate, while the STWD850 topcoat has extremely high requirements for the substrate. When combined, the coating is prone to peeling or failure due to interlayer stress or media penetration. This solution enhances synergy through functional interlayer design. The primer layer incorporates microcapsules A to achieve initial barrier and self-healing trigger functions. The intermediate transition layer uses a composite material of polyurea resin and oriented graphene to buffer the stress difference between the primer and topcoat, while forming a gradient barrier structure. The topcoat layer introduces microcapsules B and fluorosilicone modifiers to improve weather resistance and reduce surface energy, thereby reducing media residue. The oriented graphene composite material effectively disperses stress concentration, preventing interlayer peeling caused by temperature changes or mechanical vibration. The gradient barrier structure extends the media penetration path to more than twice that of traditional structures, significantly reducing the corrosion rate. The fluorosilicone modifier improves the self-cleaning properties of the coating surface, reducing localized corrosion caused by dirt adhesion and effectively lowering the probability of failure of the composite coating in harsh environments such as marine and chemical plants. Attached Figure Description

[0068] Figure 1 A medium heavy anti-corrosion environment composite anti-corrosion paint preparation method workflow schematic diagram is shown.

[0069] Figure 2 A medium heavy anti-corrosion environment composite anti-corrosion paint preparation method bottom coating paint preparation workflow schematic diagram is shown.

[0070] Figure 3 A medium heavy anti-corrosion environment composite anti-corrosion paint preparation method intermediate transition layer paint preparation workflow schematic diagram is shown.

[0071] Figure 4 A medium heavy anti-corrosion environment composite anti-corrosion paint preparation method top coating paint preparation workflow schematic diagram is shown. DETAILED DESCRIPTION

[0072] The application will be further described below in conjunction with the drawings and examples.

[0073] Please refer to Figures 1-4 The application provides an embodiment: a medium heavy anti-corrosion environment composite anti-corrosion paint, which comprises the following components in mass percentage: a bottom coating paint component, an intermediate transition layer paint component, and a top coating paint component, and the mass percentage of the bottom coating paint component, the intermediate transition layer paint component, and the top coating paint component is 33:17:50; the bottom coating paint component specifically comprises the following components and the component percentage: fluorocarbon resin 39%-41%, nano graphene 1%-3%, cashew nut shell oil epoxy resin 14%-16%, microcapsule A 2%-4%, curing agent 7%-9%, deionized water 29%-31%, and auxiliary agent 1%-3%.

[0074] As a preferred, the paint further comprises an intermediate transition layer paint component, and the intermediate transition layer paint component specifically comprises the following components and the component percentage: directional graphene composite material 1%-2%, polyurea resin 34%-36%, nano titanium dioxide 1%-2%, and bio-based plasticizer 4%-6.

[0075] As a preferred, the paint further comprises a top coating paint component, and the top coating paint component specifically comprises the following components and the component percentage: solvent-free polyurea 49%-51%, microcapsule B 4%-6%, nano zinc oxide 1%-3%, fluorosilicon modifier 2%-4%, and curing accelerator 1%-3%.

[0076] A medium heavy anti-corrosion environment composite anti-corrosion paint preparation method, comprising the following steps:

[0077] S11: Dehydrate, disperse, modify, and purify the raw materials, and complete microcapsule activation and nano material surface modification;

[0078] S12: proportionally mix the components, and prepare the primer coating after stirring and defoaming;

[0079] S13: mix the raw materials, and prepare the intermediate transition layer coating by stirring and filtering;

[0080] S14: mix the solvent-free polyurea, microcapsule B, nano-zinc oxide, and fluorosilicon modifier, and prepare the top coating after defoaming treatment;

[0081] S15: spray the primer coating, the intermediate transition layer, and the top coating in sequence, and complete the multi-layer composite coating construction through electric field-induced graphene arrangement and infrared curing;

[0082] S16: perform appearance inspection, film thickness measurement, adhesion testing, and salt spray resistance, impedance, and self-repairing performance verification.

[0083] As preferred, when the raw material pretreatment and nanomaterial functionalization are performed, the following steps are included:

[0084] S21: place the fluorocarbon resin in a vacuum drying oven, and perform dehydration treatment at 80°C for 2 hours to remove residual moisture;

[0085] S22: mix the nano-graphene and ethanol at a mass ratio of 1:5, and perform ultrasonic oscillation for 30 minutes to form a uniform suspension;

[0086] S23: add 0.5% of the silane coupling agent to the cashew nut shell oil epoxy resin, and stir at 60°C for 1 hour to improve the compatibility with the resin;

[0087] S24: place the microcapsule A in a 50°C constant temperature oven and dry for 12 hours to remove the surface adsorbed moisture;

[0088] S25: mix the graphene and polyurea resin at a mass ratio of 1:10, and grind to a particle size of ≤50μm through a three-roll grinder;

[0089] S26: filter the bio-based plasticizer through a molecular sieve adsorption column to remove trace impurities;

[0090] S27: mix the nano-zinc oxide and stearic acid at a mass ratio of 1:0.1, melt and blend at 120°C for 30 minutes to form a hydrophobic surface.

[0091] As preferred, when the primer coating preparation is performed, the following steps are included:

[0092] S31: add the fluorocarbon resin and the nano-graphene suspension to the reaction kettle, and stir at 60°C for 1 hour;

[0093] S32: slowly add the modified cashew nut shell oil epoxy resin, maintain the temperature at 60°C, and continue stirring for 30 minutes;

[0094] S33: The activated microcapsule A is added by vacuum suction to avoid agglomeration;

[0095] S34: The curing agent is added, the pH is adjusted to 8.5, and stirring is continued for 20 minutes;

[0096] S35: Deionized water is gradually added, and the viscosity is controlled to 2500-3000 mPa·s;

[0097] S36: The defoaming agent and dispersant are added, and low-speed stirring is set at 200 rpm for 10 minutes at 50°C;

[0098] S37: The mixture is placed in a vacuum defoaming machine for 15 minutes to remove bubbles.

[0099] As preferred, when preparing the intermediate transition layer coating, the following steps are included:

[0100] S41: The polyurea resin is added to the reaction kettle, and the temperature is raised to 80°C under nitrogen protection, and stirring is continued for 1 hour;

[0101] S42: The directional graphene composite material is added through a screw feeder, and the temperature is maintained at 80°C, and stirring is continued for 30 minutes;

[0102] S43: The nano-titanium dioxide with a concentration of 1% is mixed with ethanol at a mass ratio of 1:3, and after ultrasonic dispersion for 15 minutes, it is added to the main material;

[0103] S44: The bio-based plasticizer with a concentration of 5% is added to adjust the flexibility of the system, and stirring is continued for 20 minutes;

[0104] S45: The viscosity is adjusted to 1800-2200 mPa·s by adding a small amount of deionized water, and the temperature is set to 25°C;

[0105] S46: The leveling agent with a concentration of 0.5% is added, and low-speed stirring is continued for 10 minutes;

[0106] S47: The mixture is filtered through a 200-mesh filter to remove undispersed particles.

[0107] As preferred, when preparing the topcoat layer coating, the following steps are included:

[0108] S51: The solvent-free polyurea is placed in the reaction kettle, and the temperature is raised to 70°C, and vacuum degassing is continued for 30 minutes;

[0109] S52: The microcapsule B is uniformly dispersed in the polyurea system by an air flow crusher, and the temperature is maintained at 70°C, and stirring is continued for 20 minutes;

[0110] S53: The surface-modified nano-zinc oxide is added, and high-speed dispersion is continued for 15 minutes;

[0111] S54: Add fluorosilicon modifier, adjust surface energy, continue stirring for 10 minutes;

[0112] S55: Mix the curing accelerator with a small amount of ethanol, add it to the main material in a spray manner, and stir for 5 minutes;

[0113] S56: Adjust the viscosity to 3500-4000 mPa·s by adding trace diluent with a concentration ≤1%, and set the temperature to 25°C;

[0114] S57: Place the mixture in an ultrasonic debubbling instrument, set the frequency to 20 kHz, and process for 10 minutes to ensure no bubbles.

[0115] As preferred, during interlayer compounding and molding, the following steps are included:

[0116] S61: Sandblasting treatment is performed on the metal substrate, followed by acetone ultrasonic cleaning and drying;

[0117] S62: Use a high-pressure airless sprayer to spray the primer layer, with a film thickness of 1.0 mm. After leveling at room temperature for 2 hours, bake at 80°C for 4 hours;

[0118] S63: Apply an alternating current field to the surface of the primer layer to induce vertical arrangement of graphene, and spin-coat the intermediate transition layer with a film thickness of 0.5 mm;

[0119] S64: The intermediate transition layer is cured at room temperature for 24 hours to form an elastic buffer layer;

[0120] S65: Use electrostatic spraying process to spray the topcoat, with a film thickness of 1.5 mm. Perform infrared radiation curing for 30 minutes, with a wavelength of 3-5 μm and an intensity of 100 W / cm 2 ;

[0121] S66: Test the interlayer adhesion by the pull-off method to ensure that the interlayer bonding strength is ≥5 MPa;

[0122] S67: Seal the edges of the coating with polyurea sealant to prevent medium penetration.

[0123] As preferred, during post-processing and performance verification, the following steps are included:

[0124] S71: Visually inspect the coating surface to detect whether there are pinholes, cracks, and sagging defects;

[0125] S72: Use a coating thickness gauge to detect the thickness of each layer, with a film thickness deviation of ≤±10%;

[0126] S73: Perform crosshatch adhesion test according to GB / T 9286 standard, with an adhesion rating of ≤1 level;

[0127] S74: 4000 hours neutral salt spray test according to GB / T 1771 standard, no corrosion propagation at scratch;

[0128] S75: Low frequency impedance modulus value ≥ 1 x 10 9 Ω·cm2;

[0129] S76: Artificially make a 500 μm wide scratch, and observe the self-repairing effect by microscope within 24 hours, the repair rate ≥ 85%;

[0130] S77: Detect VOC content according to GB 18582-2020 standard, and ensure that the environmental protection index is ≤ 50 g / L.

[0131] Example 1 Application of Offshore Platform Steel Structure Heavy Anti-corrosion Engineering

[0132] Implementation background: A steel structure of a coastal oil platform, use environment: salt spray concentration 3%, water temperature 25-35℃, annual corrosion rate 0.3mm / a, originally used traditional epoxy glass flake paint, large area rust appeared within 3 years, emergency repair was needed, and the existing technical defects included: (1) insufficient durability: the service life of traditional paint in salt spray environment was only 5 years; (2) high construction requirement: it was required to reach Sa2.5 level of rust removal standard, and it was difficult to work at high altitude on the platform; (3) easy interlayer peeling: the adhesion between epoxy primer and polyurethane topcoat was poor, and interlayer cracking occurred after thermal shock test.

[0133] Implementation steps:

[0134] S81: Put the FEVE resin in a vacuum drying box, the residual moisture is ≤0.1%, mix with ethanol at a ratio of 1:5, and form a suspension by ultrasonic, the particle size is ≤200nm;

[0135] S82: Add 0.5% silane coupling agent, stir at 60℃ / 300rpm for 1h, the contact angle is increased from 65° to 82°, dry at 50℃ for 12h, the surface moisture content is ≤0.2%;

[0136] S83: Mix with polyurea resin at a ratio of 1:10, three-roll mill to particle size ≤50μm, conductivity is increased to 15S / cm, filter by molecular sieve adsorption column, metal ion content is ≤5ppm, mix with stearic acid at a ratio of 1:0.1, melt and blend at 120℃ for 30min, the water contact angle is increased from 0° to 120°;

[0137] S84: Add the fluorocarbon resin and graphene suspension into a reaction kettle, stir at 60℃ / 500rpm for 1h, slowly add the modified cashew nut shell oil epoxy, continue to stir at 60℃ for 30min, the viscosity is increased to 2000mPa·s;

[0138] S85: Vacuum suction of microcapsule A, dispersion uniformity ≥95%, addition of modified amine curing agent, pH adjustment to 8.5, gel time control at 45 min;

[0139] S86: Gradual addition of deionized water, viscosity control at 2500-3000 mPa·s, addition of BYK-066N defoaming agent and Disperbyk-180 dispersant, 50°C / 200 rpm stirring for 10 min, -0.1 MPa degassing for 15 min, bubble rate ≤0.5 per / cm 2 ;

[0140] S87: Addition of polyurea resin to the reaction kettle, N2 protection, heating to 80°C, 400 rpm stirring for 1 h, spiral feeder addition of oriented graphene, 80°C stirring for 30 min, thermal conductivity improvement to 1.2 W / (m·K);

[0141] S88: 1% nano-TiO2 mixed with ethanol 1:3, addition after ultrasonic treatment for 15 min, UV shielding rate improvement to 90%, addition of bio-based plasticizer, flexibility improvement of 30%;

[0142] S89: Addition of deionized water, viscosity control at 1800-2200 mPa·s, addition of BYK-358 leveling agent, 150 rpm stirring for 10 min, leveling time reduction to 8 min, 200 mesh filter screen filtration, undispersed particles ≤10 μm;

[0143] S810: Solvent-free polyurea heating to 70°C, vacuum degassing for 30 min, bubble rate ≤0.1%, airflow pulverizer dispersion of microcapsule B in polyurea, 70°C stirring for 20 min, dispersion uniformity ≥98%;

[0144] S811: Addition of modified nano-ZnO, 800 rpm high-speed dispersion for 15 min, antibacterial rate improvement to 99.9%, addition of fluorosilicon modifier, surface energy reduction to 18 mN / m, water contact angle improvement to 150°;

[0145] S812: Addition of accelerator after mixing with ethanol, 5 min completion of activation, addition of diluent, viscosity control at 3500-4000 mPa·s, 20 kHz / 10 min treatment, bubble rate ≤0.2%;

[0146] S813: Sand blasting to Sa2.5 level, acetone ultrasonic cleaning for 20 min, drying to water content ≤2%, high-pressure airless spraying, film thickness 1.0 mm, leveling for 2 h, 80°C baking for 4 h, adhesion 5 MPa;

[0147] S814: The surface of the primer layer is applied with an alternating current electric field of 25V / mm to induce vertical arrangement of graphene, the thickness of the intermediate layer is 0.5mm, the elastic modulus is controlled to be 0.8MPa, and the stress concentration is relieved after room temperature curing for 24h;

[0148] S815: Electrostatic spraying, film thickness 1.5mm, infrared curing for 30min, surface drying time ≤1h, interlayer bonding strength ≥5MPa by tensile test, no cracking by thermal shock test, polyurea sealant sealing, wet adhesion ≥3MPa, medium permeability ≤1×10-12g / cm 2 ·s;

[0149] S816: No pinhole, crack, sagging, gloss controlled at 85±5, primer 1.0±0.1mm, intermediate layer 0.5±0.05mm, topcoat 1.5±0.15mm;

[0150] S817: GB / T 9286 crosshatch method test, rating 1 level, scratch expansion width ≤0.5mm after 4000h neutral salt spray;

[0151] S818: EIS test low frequency impedance modulus ≥1×10 9 Ω·cm 2 , 500μm scratch 24h repair rate ≥85%, GB18582-2020 standard test, VOC content ≤50g / L.

[0152] Data comparison table:

[0153] Performance indicators Prior art The present solution Elevation range Salt mist resistance time 2000 4000 +100% Low-frequency impedance modulus value 8 x 10 6 ]] 1.2 x 10 9 ]]> +1400% Self-repairing efficiency 60 85 +41.7% VOC content 180 45 -75% Construction base requirements Sa2.5 Sa2.0 20% reduction Thermal shock test 3 5 +66.7%

[0154] Conclusion: The scheme realizes significant improvement in key indicators such as durability, environmental protection and construction efficiency through material innovation and process optimization, and is especially suitable for marine engineering environment with high salt mist and strong corrosion.

[0155] The embodiments of the application are described in detail above in combination with the drawings, but the application is not limited to the above embodiments, and various changes can be made within the knowledge of those skilled in the art without departing from the purpose of the application.

Claims

1. A composite anticorrosive paint for use in a heavy corrosion environment of a medium; characterized by: The coating further comprises an intermediate transition layer coating component, and the intermediate transition layer coating component specifically comprises the following components and the components account for 1-2% of the intermediate transition layer coating component: oriented graphene composite material, 34-36% of polyurea resin, 1-2% of nano-titanium dioxide, and 4-6% of bio-based plasticizer.

2. The composite anticorrosive paint for heavy-duty anticorrosive environment according to claim 1, characterized by: The coating further comprises a top coating layer coating component, and the top coating layer coating component specifically comprises the following components and the components account for 49-51% of the top coating layer coating component: solvent-free polyurea, 4-6% of microcapsule B, 1-3% of nano-zinc oxide, 2-4% of fluorosilicon modifier, and 1-3% of curing accelerator.

3. The composite anticorrosive coating for heavy-duty anticorrosive environment according to claim 2, characterized in that: The coating further comprises a top coating layer coating component, and the top coating layer coating component specifically comprises the following components and the components account for 49-51% of the top coating layer coating component: solvent-free polyurea, 4-6% of microcapsule B, 1-3% of nano-zinc oxide, 2-4% of fluorosilicon modifier, and 1-3% of curing accelerator.

4. Any of claims 1-3, characterized in that: A preparation method of a composite anticorrosive coating for medium heavy corrosion environment, comprising the following steps: S11: Dehydrate, disperse, modify and purify the raw materials, and complete the activation of microcapsules and the surface modification of nanomaterials; S12: Mix the components in proportion, stir and defoam to prepare a base coating; S13: Mix the raw materials, stir and filter to prepare an intermediate transition layer coating; S14: Mix solvent-free polyurea, microcapsule B, nano-zinc oxide and fluorosilicon modifier, and defoam to prepare a top coating layer coating; S15: Spray the base coating, the intermediate transition layer and the top coating layer in sequence, arrange graphene by electric field induction and cure by infrared to complete the construction of the multi-layer composite coating; S16: Perform appearance inspection, film thickness measurement, adhesion test and performance verification of salt spray resistance, impedance and self-repair.

5. The method of claim 4, wherein the method is characterized by: When pre-treating the raw materials and functionalizing the nanomaterials, the following steps are included: S21: Dehydrate the fluorocarbon resin in a vacuum drying oven at 80°C for 2 hours to remove residual water; S22: Mix the nano-graphene and ethanol in a mass ratio of 1:5, ultrasonically oscillate for 30 minutes to form a uniform suspension; S23: Add 0.5% of silane coupling agent to the cashew nut shell oil epoxy resin, stir at 60°C for 1 hour to improve the compatibility with the resin; S24: Dry the microcapsule A in a 50°C constant temperature oven for 12 hours to remove the surface adsorbed water; S25: Mix the graphene and polyurea resin in a mass ratio of 1:10, grind to a particle size of ≤50μm by a three-roll grinder; S26: Filter the bio-based plasticizer through a molecular sieve adsorption column to remove trace impurities; S27: Mix the nano-zinc oxide and stearic acid in a mass ratio of 1:0.1, melt and blend at 120°C for 30 minutes to form a hydrophobic surface.

6. The method of claim 4, wherein the method is characterized by: When preparing the base coating, the following steps are included: S31: Add the fluorocarbon resin and the nano-graphene suspension to a reaction kettle, stir at 60°C for 1 hour; S32: Slowly add modified cashew shell oil epoxy resin, maintain temperature 60℃, continue stirring for 30 minutes; S33: Add activated microcapsule A by vacuum suction method to avoid agglomeration; S34: Add curing agent, adjust pH to 8.5, continue stirring for 20 minutes; S35: Gradually add deionized water, control viscosity to 2500-3000 mPa·s; S36: Add defoaming agent and dispersant, set stirring speed to 200 rpm at 50℃ for 10 minutes; S37: Place the mixture in a vacuum degassing machine for 15 minutes to remove bubbles.

7. The method of claim 4, wherein the method is characterized by: When preparing the intermediate transition layer coating, the following steps are included: S41: Add polyurea resin to the reaction kettle, heat to 80℃ under nitrogen protection, and stir for 1 hour; S42: Add directional graphene composite material through the screw feeder, maintain temperature 80℃, and stir for 30 minutes; S43: Mix 1% concentration of nano titanium dioxide with ethanol at a mass ratio of 1:3, ultrasonic dispersion for 15 minutes, and then add the main material; S44: Add 5% concentration of bio-based plasticizer, adjust the flexibility of the system, and continue stirring for 20 minutes; S45: Adjust the viscosity to 1800-2200 mPa·s by adding a small amount of deionized water, and set the temperature to 25℃; S46: Add 0.5% concentration of leveling agent, low-speed stirring for 10 minutes; S47: Filter the mixture through a 200 mesh filter to remove undispersed particles.

8. The method of claim 4, wherein the method is characterized by: When preparing the topcoat layer coating, the following steps are included: S51: Place the solvent-free polyurea in the reaction kettle, heat to 70℃, and vacuum degas for 30 minutes; S52: Disperse microcapsule B uniformly in the polyurea system by air flow crusher, maintain temperature 70℃, and stir for 20 minutes; S53: Add surface modified nano zinc oxide, high-speed dispersion for 15 minutes; S54: Add fluorosilicon modifier, adjust surface energy, and continue stirring for 10 minutes; S55: Mix the curing accelerator with a small amount of ethanol, spray the main material, and stir for 5 minutes; S56: Adjust the viscosity to 3500-4000 mPa·s by adding ≤1% micro-diluent, set the temperature to 25℃; S57: Place the mixture in an ultrasonic degassing instrument, set the frequency to 20kHz, and process for 10 minutes to ensure no bubbles.

9. The method of claim 4, wherein the method is characterized by: When performing interlayer compounding and forming, the following steps are included: S61: Sandblast the metal substrate, ultrasonic clean with acetone, and dry; S62: Spray the primer layer with a high-pressure airless sprayer, control the film thickness to 1.0mm, level at room temperature for 2 hours, and bake at 80℃ for 4 hours; S63: Apply an alternating current field to the surface of the primer layer to induce vertical arrangement of graphene, and spin coat the intermediate transition layer with a film thickness of 0.5mm; S64: Curing the intermediate transition layer at room temperature for 24 hours to form an elastic buffer layer; S65: The top coat is sprayed using an electrostatic spraying process, with a film thickness of 1.5 mm, and infrared radiation curing for 30 minutes, with a set wavelength of 3-5 μm and an intensity of 100 W / cm 2 ; S66: Test the interlayer adhesion by the pull-off method to ensure that the interlayer bonding strength is ≥5MPa; S67: Seal the edges of the coating with polyurea sealant to prevent medium penetration.

10. The method of claim 4, wherein the method is characterized by: When performing post-processing and performance verification, the following steps are included: S71: Visually inspect the coating surface to detect whether there are pinholes, cracks and sagging defects; S72: Use a coating thickness gauge to detect the thickness of each layer, and the film thickness deviation is ≤±10%; S73: According to GB / T 9286 standard, carry out grid method adhesion test, and the adhesion rating is ≤1 level; S74: According to GB / T 1771 standard, carry out 4000 hour neutral salt spray test, and there is no corrosion propagation at the scratch; S75: Through electrochemical impedance spectroscopy test, the low-frequency impedance modulus value is ≥1×10 9 Ω·cm2; S76: Manually make a 500μm wide scratch, and observe the self-repairing effect by microscope within 24 hours, and the repair rate is ≥85%; S77: According to GB 18582-2020 standard, detect the VOC content, and ensure that the environmental protection index is ≤50g / L.

Citation Information

Cited By

  • An ultra-bipolar coating with repairable function and a preparation method and application thereof