A lithium-ion battery anode structure for suppressing lithium plating and its preparation method

By introducing a low-thickness lithium storage functional layer on the surface of the graphite anode, including silicon anode materials of different particle sizes, the lithium plating problem caused by non-uniform reaction in lithium-ion batteries is solved, improving the cycle life and safety of the battery. It is applicable to a variety of anode material systems and maintains high energy density.

CN120998929BActive Publication Date: 2026-11-17HUAZHONG UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510924090.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-04
Publication Date
2026-11-17
Estimated Expiration
2045-07-04

AI Technical Summary

Technical Problem

Existing lithium-ion batteries, with their thick electrode design, suffer from uneven reaction due to lithium-ion concentration gradients. This leads to excessive lithium intercalation on the surface and lithium plating, reducing the battery's reversible capacity and cycle life, and posing safety hazards.

Method used

A thin lithium storage functional layer, consisting of silicon anode materials of different particle sizes, is introduced on the surface of a graphite anode to suppress lithium plating by adjusting the lithium ion distribution and reaction rate.

Benefits of technology

It effectively suppresses lithium plating, improves battery cycle life and safety, and performs exceptionally well under fast charging conditions. It also features a simple structural design, is suitable for various anode material systems, and maintains high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120998929B_ABST
    Figure CN120998929B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lithium-ion battery technology, specifically a lithium-ion battery anode structure for suppressing lithium plating and its preparation method. It includes a stacked graphite layer and a lithium storage functional layer. The lithium storage functional layer comprises at least two silicon anode materials with different particle sizes, and the thickness of the graphite layer is greater than the thickness of the lithium storage functional layer. During charge-discharge cycling of the lithium-ion battery, the degree of lithiation of the lithium storage layer is controlled to simultaneously reduce the tendency for lithium plating and control volume expansion, thereby improving the battery's cycle life and charging safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a lithium-ion battery negative electrode structure for suppressing lithium plating and its preparation method. Background Technology

[0002] Lithium-ion batteries, as core energy devices, are widely used in portable electronic devices, electric vehicles, and energy storage systems. Their performance and lifespan largely depend on the structural stability and reaction uniformity of the anode material. Graphite, with its excellent reversible lithium intercalation performance, high initial coulombic efficiency, and low cost, has long been the mainstream anode material for lithium-ion batteries.

[0003] However, with the increasing demands for battery energy density, anode materials face greater challenges in terms of fast-charging and high-rate performance. In practical applications, especially in thick electrode designs, the reaction of graphite anodes exhibits significant inhomogeneity along the thickness direction. The region near the electrolyte (i.e., the electrode surface) tends to preferentially undergo lithium intercalation due to the shorter lithium-ion transport path and lower polarization. This leads to the surface graphite particles reaching a high degree of lithiation within a short time, even exceeding their theoretical capacity limit, thus triggering lithium metal deposition.

[0004] Lithium plating not only reduces the reversible capacity and cycle life of batteries, but can also promote the formation of lithium dendrites, posing serious safety hazards. Although existing technologies can mitigate the lithium plating problem to some extent by optimizing electrode thickness, improving electrolyte formulation, or adjusting charging strategies, they are fundamentally unable to solve the problem of excessive lithium intercalation on the surface caused by uneven reaction in the thickness direction.

[0005] Therefore, there is an urgent need for a novel negative electrode structure design method that can fully leverage the high energy density of graphite materials while effectively mitigating lithium plating caused by uneven lithium deposition, thereby improving the lifespan and safety of lithium-ion batteries. Summary of the Invention

[0006] The purpose of this invention is to provide a lithium-ion battery anode structure and its preparation method for suppressing lithium plating, by introducing a low-thickness lithium storage functional layer on the surface of a high-thickness graphite anode to solve the lithium plating problem caused by lithium-ion concentration gradient.

[0007] To achieve the above objectives, the first aspect of the present invention provides a lithium-ion battery anode structure, comprising a graphite layer and a lithium storage functional layer stacked together, wherein the lithium storage functional layer comprises a silicon anode material, and the thickness of the graphite layer is greater than the thickness of the lithium storage functional layer.

[0008] Furthermore, the thickness of the graphite layer is ≥40μm, and the thickness of the lithium storage functional layer is ≤10μm.

[0009] Furthermore, the thickness of the graphite layer is 40-200 μm, and the thickness of the lithium storage functional layer is 0.5-8 μm, preferably 3-5 μm.

[0010] Furthermore, the lithium storage functional layer includes at least two silicon anode materials with different particle sizes, preferably including a silicon anode material with a particle size ≤100nm and a silicon anode material with a particle size between 0.5-5μm.

[0011] Furthermore, the mass ratio of the silicon anode material with a particle size ≤100nm to the silicon anode material with a particle size between 0.5-5μm is 1:(0.5-4), preferably 1:(1-3).

[0012] Furthermore, the silicon anode material includes one or more of nano-silicon, silicon-carbon composite material, silicon oxide, and silicon-coated metal oxide; the lithium storage functional layer preferably also includes a conductive agent and a binder.

[0013] A second aspect of the present invention provides a method for preparing the lithium-ion battery negative electrode structure according to any one of the above claims, comprising the following steps:

[0014] S1. Prepare graphite slurry and lithium storage material slurry;

[0015] S2. Apply graphite slurry to the surface of the current collector, dry it, and then roll it to form a graphite layer.

[0016] S3. Apply lithium storage material slurry to the surface of the graphite layer, dry it, and then roll it to form a lithium storage functional layer.

[0017] Furthermore, the graphite slurry comprises graphite powder, a conductive agent, and a binder, and the solvent is N-methylpyrrolidone or water;

[0018] The lithium storage material slurry includes silicon anode material, conductive agent and binder, and the solvent is water or organic solvent.

[0019] A third aspect of the present invention provides a lithium-ion battery, comprising the lithium-ion battery negative electrode structure described in any of the preceding claims.

[0020] A fourth aspect of the present invention provides a method for suppressing lithium plating in a lithium-ion battery as described above, comprising: during charge-discharge cycles of the lithium-ion battery, controlling the maximum capacity of each charge-discharge cycle to be 0.2 to 0.5 times the capacity of the lithium storage functional layer and the sum of the capacity of the graphite layer, so as to suppress lithium plating on the surface of the graphite layer by utilizing the lithium storage functional layer, while reducing the expansion of the lithium storage functional layer.

[0021] In summary, compared with the prior art, the above-described technical solutions conceived by this invention mainly possess the following technical advantages:

[0022] 1. The lithium-ion battery negative electrode structure for suppressing lithium plating provided by the present invention introduces a lithium storage functional layer with a specific capacity greater than that of graphite on the surface of the graphite electrode, which can effectively adjust the lithium-ion distribution in the thickness direction of the graphite negative electrode, suppress the deposition of surface metallic lithium, and thus improve the cycle life and charging safety of the battery.

[0023] 2. This invention reduces the lifespan reduction caused by expansion by using silicon anode materials with different particle sizes, and balances lithium plating and cycle life by adjusting the ratio of the two particle sizes, resulting in a lithium-ion battery anode structure with excellent overall performance, improving cycle stability and safety performance, especially under fast charging and thick electrode conditions.

[0024] 3. By adjusting the thickness of the graphite layer and the lithium storage functional layer, the present invention can suppress lithium plating by using only a thinner lithium storage functional layer on the surface of the thicker graphite layer. At the same time, the expansion rate of the thinner lithium storage functional layer is significantly reduced, so it will not lead to a significant reduction in cycle life.

[0025] 4. The present invention has a simple structural design, which is easy to implement on existing production lines; it is applicable to a variety of negative electrode material systems and has good versatility; the thinner lithium storage functional layer will not significantly increase the electrode thickness and electrode preparation cost, and maintain a high energy density. Attached Figure Description

[0026] Figure 1 This is a schematic cross-sectional view of the graphite anode structure of the lithium storage layer of the present invention.

[0027] Figure 2 This is a SEM cross-sectional view of the graphite anode of the lithium storage layer manufactured according to the present invention.

[0028] Figure 3 This is a schematic diagram of a typical thick-axis lithium-ion distribution when a graphite anode is discharged at a 1C rate to 60% SOC.

[0029] Figure 4 A process flow diagram for manufacturing lithium storage layer electrodes.

[0030] Figure 5 The graph shows the comparison of the cycling performance curves of the lithium storage layer electrode. LSL represents the lithium storage functional layer.

[0031] Figure 6 The images show a comparison of surface SEM images with and without lithium storage layer electrodes at 60% SOC under 3C rate. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0033] The first aspect of the present invention provides a lithium-ion battery anode structure, comprising a graphite layer and a lithium storage functional layer stacked together, wherein the lithium storage functional layer comprises at least two silicon anode materials with different particle sizes, and the thickness of the graphite layer is greater than the thickness of the lithium storage functional layer.

[0034] The lithium storage functional layer of the present invention is composed of a lithium-ion intercalation material with a capacity higher than that of graphite, which is used to absorb lithium ions that preferentially intercalate into the graphite surface during fast charging, thereby suppressing the formation of lithium dendrites on the graphite surface.

[0035] Specifically, a current collector, such as copper foil, is attached to the other side of the graphite layer to provide support and conductivity. Its surface is conventionally treated to enhance adhesion to the active layer.

[0036] The graphite layer is composed of natural or artificial graphite particles, combined with conductive agents and binders (such as PVDF, SBR / CMC, etc.), and is formed on the surface of copper foil through a first coating process. This layer serves as the main lithium-ion insertion / extraction carrier, and its thickness is typically greater than 40 μm. The purpose of this invention is to solve the problem of lithium plating on the surface of thick graphite anodes.

[0037] The graphite layer is rolled to achieve a compaction density of 1.4-1.6 g / cm³. 3 This helps to increase the overall load on the electrode.

[0038] The thickness of the graphite layer is ≥40μm, and the thickness of the lithium storage functional layer is ≤10μm.

[0039] The thickness of the graphite layer is 40-200 μm, and the thickness of the lithium storage functional layer is 0.5-8 μm, preferably 1-3 μm (when the graphite layer is <80 μm) or 3-5 μm (when the graphite layer is >80 μm). Within this thickness range, it can play a significant buffering role and avoid structural instability caused by excessive material expansion and deformation, which would affect the cycle life.

[0040] Furthermore, the silicon anode material includes silicon anode materials with a particle size ≤100nm and silicon anode materials with a particle size between 0.5-5μm. By using multiple particle size distributions, the lithium-ion reaction rate is controlled, achieving synergistic control of preferential lithium-ion absorption and reduced expansion rate, thereby effectively preventing the adverse effects of silicon anode material expansion. Preferably, the silicon anode material includes silicon anode materials with a particle size of 20-100nm and silicon anode materials with a particle size between 2-5μm. Alternatively, it includes silicon anode materials with a particle size of 20-100nm and silicon anode materials with a particle size between 0.5-1μm.

[0041] Furthermore, the silicon anode material with a particle size ≤100nm and the silicon anode material with a particle size between 0.5-5μm have a mass ratio of 1:(0.5-4), preferably 1:(1-3).

[0042] This invention proposes to control the particle size distribution of silicon anode material in lithium storage materials to regulate the lithium-ion intercalation reaction rate, specifically as follows:

[0043] Small-particle-size (e.g., nanoscale <100nm) active materials have higher specific surface area and faster reaction kinetics, enhancing initial lithium uptake capacity; large-particle-size (e.g., 0.5-5μm) active materials have slower reaction rates, reducing the initial lithium absorption rate and thus preventing interfacial expansion and structural damage under certain conditions due to excessively rapid reactions. The particle size of the lithium storage layer material is determined based on the actual operating conditions (rate, capacity).

[0044] After particle size regulation, a lithium intercalation rate gradient is formed, which better protects the graphite host layer and delays the formation of lithium dendrites.

[0045] Increasing the thickness of the graphite layer, and consequently increasing the proportion of small-particle nano-silicon, achieves superior lithium storage performance. The lithium storage layer, after adjusting the silicon particle size, can achieve the following synergistic effects:

[0046] Under fast charging conditions, fine-grained silicon on the surface of the lithium storage layer preferentially intercalates to lithium, effectively intercepting some of the high-flux lithium ions. Due to the reduced reaction rate, medium-sized silicon particles gradually participate in lithium intercalation in subsequent stages, effectively reducing the peak volume expansion. This further reduces the local lithium ion concentration on the graphite electrode surface, alleviates hyperlithiation of the graphite surface, and significantly inhibits lithium plating.

[0047] Furthermore, the silicon anode material includes nano-silicon, silicon-carbon composite materials (Si / C, Si@C, SiO2), etc. x -C), silicon oxide (SiO) x One or more of silicon-coated metal oxides; the lithium storage functional layer preferably also includes a conductive agent and a binder.

[0048] The binder in the lithium storage functional layer may be the same as or different from that in the graphite layer. It is preferred to use a flexible binder system such as SBR / CMC or LA133 to buffer the expansion of silicon-based materials and enhance cycle stability.

[0049] Please see Figure 1 and 4 The second aspect of the present invention provides a method for preparing the lithium-ion battery negative electrode structure according to any one of the above claims, comprising the following steps:

[0050] S1. Prepare graphite slurry and lithium storage material slurry;

[0051] S2. Apply graphite slurry (such as doctor blade coating or slot die coating) to the surface of the current collector, and roll it after drying to form a graphite layer.

[0052] S3. Apply lithium storage material slurry to the surface of the graphite layer, dry it, and then roll it to form a lithium storage functional layer.

[0053] The dried double-layer negative electrode sheet can be used directly for cell assembly, or it can be further rolled or cut.

[0054] Furthermore, the graphite slurry comprises graphite powder, a conductive agent, and a binder, and the solvent is N-methylpyrrolidone or water; the mass ratio of graphite powder to conductive agent is (85-95):(5-10).

[0055] The lithium storage material slurry comprises 60-70 wt% silicon anode material, 15-20 wt% conductive agent, and 15-20 wt% binder, and the solvent is water or an organic solvent.

[0056] The lithium storage functional layer and the graphite main layer are in contact through a physical interface and have good interfacial bonding strength.

[0057] A third aspect of this invention provides a lithium-ion battery comprising the lithium-ion battery negative electrode structure described in any of the preceding embodiments. This invention is applicable to various types of graphite negative electrodes, and is particularly suitable for thick electrodes with high loading density. As the graphite thickness increases, the lithium storage layer thickness can be increased accordingly.

[0058] A fourth aspect of the present invention provides a method for suppressing lithium plating in a lithium-ion battery as described above, comprising: during charge-discharge cycles of the lithium-ion battery, controlling the maximum capacity of each charge-discharge cycle to be 0.2 to 0.5 times the capacity of the lithium storage functional layer plus the capacity of the graphite layer, so as to utilize the lithium storage functional layer to suppress lithium plating on the surface of the graphite layer and simultaneously reduce the expansion of the lithium storage functional layer. Furthermore, since the specific capacity of the lithium storage functional layer is higher than that of graphite, the overall charge-discharge capacity is still higher than that of the graphite layer alone.

[0059] This invention can significantly reduce lithium plating and improve battery cycle life under charge and discharge rates of 2C and above.

[0060] Specifically, the preparation method of the lithium-ion battery negative electrode structure includes the following steps:

[0061] (1) Preparation of graphite host layer

[0062] Slurry preparation

[0063] Natural or artificial graphite powder is mixed with a conductive agent (such as super carbon black) in a certain ratio (e.g., graphite: conductive agent = 90:5, by mass). A binder (such as polyvinylidene fluoride PVDF or SBR / CMC system) is added, along with an appropriate amount of N-methylpyrrolidone (NMP) or water as a solvent. The mixture is stirred until homogeneous to obtain a graphite slurry.

[0064] Coating and drying

[0065] Graphite slurry is applied to the surface of pretreated copper foil (or other current collector) using blade coating, slot die coating, or other conventional coating equipment. Coating parameters are adjusted according to the desired electrode thickness (e.g., 40-200 micrometers dry film thickness). After coating, heat drying is performed at room temperature or 50-60°C, typically for about 60 minutes, to ensure complete solvent evaporation.

[0066] Compaction

[0067] The dried graphite electrodes are then subjected to a rolling process, with the pressure adjusted to increase the negative electrode density while ensuring close contact between the particles. The rolling pressure is typically in the range of 0.5-1 MPa, and can be optimized according to specific requirements.

[0068] (2) Preparation of lithium storage functional layer

[0069] Slurry preparation

[0070] Lithium storage materials are made of silicon powder or silicon-based composite materials. To reduce the silicon expansion effect and improve cycle stability, pre-coated silicon particles or silicon-carbon composite materials can be used. The mixing ratio can be set as follows: active material (silicon or composite material) accounts for 60-70% of the total solids, conductive agent (such as carbon black or conductive carbon fiber) accounts for 15-20%, and binder (such as flexible systems such as SBR / CMC or LA133) accounts for 15-20%. Water or environmentally friendly organic solvents can be used as solvents, and the mixture should be stirred until the slurry is uniformly dispersed.

[0071] Coating and drying

[0072] The aforementioned lithium storage slurry is uniformly coated onto the surface of a pre-prepared, dried, and compacted graphite electrode. To ensure the uniformity and thickness control of the lithium storage layer, a precision-controlled coating machine can be used during the coating process. The target thickness is controlled at 0.5-8 micrometers, preferably 3-5 micrometers. After coating, a second drying process is performed at 50-80°C for 6-8 hours to ensure complete evaporation of the solvent in the slurry.

[0073] Roll curing (optional step)

[0074] Applying a light re-rolling process to the two-layer structure helps to further improve the interfacial contact between the lithium storage layer and the graphite layer, thereby enhancing the overall mechanical strength and conductivity. The pressure is typically low to avoid damaging the lithium storage material.

[0075] (3) Electrode post-processing and assembly

[0076] According to actual needs, the double-layer electrode sheets are cut, edge-trimmed, and preheated to ensure that the electrode sheets are of consistent size and have a flat surface.

[0077] Example 1

[0078] A method for preparing a lithium-ion battery negative electrode structure includes the following steps:

[0079] (1) Preparation of graphite host layer

[0080] Graphite powder and conductive super carbon black were mixed at a mass ratio of 90:5, polyvinylidene fluoride (PVDF) was added as a binder, and an appropriate amount of N-methylpyrrolidone (NMP) was added as a solvent. The mixture was stirred and mixed evenly to obtain graphite slurry.

[0081] Graphite slurry is coated onto the pretreated copper foil surface. After coating, it is heat-dried at 70°C for about 6 hours to ensure that the solvent evaporates completely.

[0082] The dried graphite electrode sheets are subjected to roller pressing treatment. The pressure is adjusted to increase the density of the negative electrode while ensuring close contact between the particles. The roller pressing pressure is in the range of 0.5-1MPa.

[0083] (2) Preparation process of lithium storage layer composed of multi-size silicon particles

[0084] The following components are selected in the preparation of lithium storage slurry:

[0085] Silicon active material: Nano-silicon (denoted as Si1) with a particle size D50≈80nm and silicon microparticles (denoted as Si2) with a particle size D50≈3μm are mixed at a mass ratio of 1:1, with a total addition amount of 60wt%.

[0086] Conductive agent: Conductive carbon black (20wt%);

[0087] Adhesive: SBR / CMC (20wt%);

[0088] Solvent: Deionized water.

[0089] After thorough mixing and ultrasonic dispersion, the mixture is coated onto the surface of the graphite substrate and lightly rolled after drying. Figure 2 As shown, the graphite layer in the composite negative electrode prepared in this embodiment has a thickness of approximately 54.5 μm, and the lithium storage functional layer has a thickness of approximately 4.69 μm.

[0090] The resulting electrode can be cycled 96 times under fast charging (2C) conditions, and the battery cycle life is improved by about 100% compared with the pure graphite electrode, and the lithium plating phenomenon is significantly alleviated.

[0091] The treated negative electrode sheet is assembled with a separator, electrolyte, lithium metal or pre-lithiated positive electrode material to form a prototype cell (half-cell), and its electrochemical performance is tested and verified. During the cycle performance test, the maximum capacity of each discharge is controlled to be the sum of 0.4 times the capacity of the lithium storage functional layer and the capacity of the graphite layer.

[0092] Example 2

[0093] The difference from Example 1 is that in step 2, nano-silicon (denoted as Si1) with a particle size D50≈80nm and silicon microparticles (denoted as Si2) with a particle size D50≈3μm are mixed at a mass ratio of 1:3. Everything else is the same as in Example 1 and will not be repeated here.

[0094] Example 3

[0095] The difference from Example 1 is that step 2 only includes nano-silicon with a particle size of D50≈80nm. Everything else is the same as in Example 1 and will not be repeated here.

[0096] from Figure 3 It can be seen that adding a lithium storage functional layer increases the rate and amount of lithium insertion into the layer, reducing concentration on the graphite surface and suppressing lithium plating. From... Figure 6 It can be seen that after adding the lithium storage functional layer, there is basically no lithium precipitation at 60% SOC under 3C rate, while lithium dendrites appear on the surface of the graphite layer without the lithium storage functional layer.

[0097] Comparative Example 1

[0098] The difference from Example 1 is that the negative electrode only contains the graphite layer prepared in step 1. Everything else is the same as in Example 1, and will not be repeated here.

[0099] Table 1. Performance test results of the examples and comparative examples.

[0100]

[0101] In Table 1, cycle life refers to the capacity decreasing to 80% of the theoretical initial capacity.

[0102] As shown in Table 1, the rate performance and cycle life of pure graphite electrodes are relatively low, with lithium plating occurring at 1.5C. In contrast, Example 3, which incorporates pure nano-silicon, achieves no lithium plating at both 1.5C and 3C rates, and its cycle life is improved compared to pure graphite electrodes. Using silicon particles of two different sizes further enhances the cycle life, with the highest cycle life achieved when Si1:Si2 = 1:3. This is because larger particles have a relatively smaller specific surface area, resulting in a slower reaction rate and lower expansion. Furthermore, larger particles form the basic framework, while smaller particles, due to their smaller size, collide within the pores formed by the framework, preventing damage to the overall structure. Therefore, appropriately increasing the mass ratio of larger particles further improves the cycle life. However, further increasing the mass ratio of larger particles, while reducing silicon expansion and extending cycle life, gradually exacerbates lithium plating at high rates. Therefore, by rationally controlling the content of silicon of two different particle sizes, lithium plating and cycle life can be comprehensively regulated, resulting in a lithium-ion battery with excellent overall performance.

[0103] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A lithium-ion battery anode structure, characterized by, It includes a graphite layer and a lithium storage functional layer stacked together, and a current collector is attached to the other side of the graphite layer. The lithium storage functional layer includes a silicon anode material, and the thickness of the graphite layer is greater than the thickness of the lithium storage functional layer. The lithium storage functional layer includes at least two silicon anode materials with different particle sizes, including silicon anode materials with a particle size ≤100nm and silicon anode materials with a particle size between 0.5-5µm. The mass ratio of the silicon anode material with a particle size ≤100nm to the silicon anode material with a particle size between 0.5-5µm is 1:1; The thickness of the graphite layer is ≥40µm, and the thickness of the lithium storage functional layer is 3-5µm.

2. The lithium-ion battery negative electrode structure according to claim 1, characterized in that, The thickness of the graphite layer is 40-200µm.

3. The lithium-ion battery negative electrode structure according to claim 1, characterized in that, The silicon anode material includes one or more of nano-silicon, silicon-carbon composite material, silicon oxide, and silicon-coated metal oxide; the lithium storage functional layer also includes a conductive agent and a binder.

4. A method for preparing a lithium-ion battery negative electrode structure according to any one of claims 1-3, characterized in that, Includes the following steps: S1. Prepare graphite slurry and lithium storage material slurry; S2. Apply graphite slurry to the surface of the current collector, dry it, and then roll it to form a graphite layer. S3. Apply lithium storage material slurry to the surface of the graphite layer, dry it, and then roll it to form a lithium storage functional layer.

5. The method for preparing the lithium-ion battery negative electrode structure according to claim 4, characterized in that, The graphite slurry comprises graphite powder, a conductive agent, and a binder, and the solvent is N-methylpyrrolidone or water; The lithium storage material slurry includes silicon anode material, conductive agent and binder, and the solvent is water or organic solvent.

6. A lithium-ion battery, characterized in that, The lithium-ion battery anode structure includes the lithium-ion battery anode structure according to any one of claims 1-3 or the lithium-ion battery anode structure obtained by the preparation method according to any one of claims 4-5.

7. A method for suppressing lithium plating in a lithium-ion battery as described in claim 6, characterized in that, include: When the lithium-ion battery is used for charge-discharge cycles, the maximum capacity of each charge-discharge cycle is controlled to be 0.2 to 0.5 times the capacity of the lithium storage functional layer and the sum of the capacity of the graphite layer, so as to utilize the lithium storage functional layer to suppress lithium plating on the surface of the graphite layer and reduce the expansion of the lithium storage functional layer.

Citation Information

Patent Citations

  • Electrode for lithium ion secondary battery and lithium ion secondary battery

    JP2020140895A