In-situ synthesis reinforced high-strength aluminum alloy and manufacturing method thereof

By introducing ZrB2 particles and rare earth oxides into aluminum alloys, the problem of particle agglomeration in the in-situ synthesis method was solved, achieving high strength and uniform dispersion of aluminum alloys and improving the overall performance of the material.

CN121046676APending Publication Date: 2025-12-02ANHUI XINBO PHOTOVOLTAIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511113951.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-11
Publication Date
2025-12-02

AI Technical Summary

Technical Problem

In situ synthesis methods can lead to particle agglomeration during the solidification process in aluminum matrix composites, resulting in uneven distribution of reinforcing particles and a decline in material properties.

Method used

The method of mixing and drying with reactive salts Na2B4O7 and K2ZrF6, followed by ball milling, introduces ZrB2 particles into the aluminum alloy as a reinforcing phase through synthesis, and achieves uniform dispersion of the particles through the synergistic effect of rare earth oxides.

Benefits of technology

It improves the strength and density of aluminum alloys, reduces defects such as pores, and enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an in-situ synthesis reinforced high-strength aluminum alloy and a manufacturing method thereof, and relates to the technical field of aluminum alloys. The invention discloses a manufacturing method of an in-situ synthesized reinforced high-strength aluminum alloy. The manufacturing method comprises the following steps: S1, carrying out primary drying treatment, ball milling and secondary drying treatment on reaction salt to obtain a mixed material; s2, after an aluminum alloy matrix is melted and drossing is conducted, the mixed material and rare earth oxide are added, heating, stirring and heat preservation are conducted, and a composite aluminum alloy melt is obtained; s3, the composite aluminum alloy melt is subjected to slagging-off, refining and impurity removal, pouring and cooling forming, and a cast ingot is obtained; and S4, the cast ingot is subjected to homogenization treatment, extrusion forming, solid solution treatment and aging treatment, and the aluminum alloy is obtained. The aluminum alloy provided by the invention has high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy technology, and in particular to an in-situ synthesized reinforced high-strength aluminum alloy and its manufacturing method. Background Technology

[0002] Particle-reinforced aluminum matrix composites, with their high specific strength, excellent wear resistance, and designability, have achieved large-scale applications in aerospace (e.g., satellite brackets, engine components) and transportation (lightweight vehicle bodies, brake discs). Based on the method of introducing reinforcing particles, mainstream preparation processes are divided into two categories: external addition and in-situ synthesis. In-situ synthesis is superior to external addition because it can better generate fine, dispersed reinforcing particles in the matrix. However, in-situ synthesis still faces a serious challenge in industrial applications—the particle agglomeration effect during solidification. During melt solidification, due to interface shift, the spacing between the originally well-dispersed reinforcing particles decreases. Simultaneously, because of the small size of nanoparticles and their large surface energy, they easily adsorb each other, leading to particle agglomeration, increasing the possibility of forming defects such as pores, and affecting material properties. Summary of the Invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes an in-situ synthesis of reinforced high-strength aluminum alloy and its manufacturing method.

[0004] The present invention proposes a method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy, comprising the following steps:

[0005] S1. The reaction salt is dried once, ball-milled, and dried a second time to obtain a mixture.

[0006] S2. After melting the aluminum alloy matrix and removing the slag, add the mixed materials and rare earth oxides, heat and stir, and keep warm to obtain the composite aluminum alloy melt;

[0007] S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot;

[0008] S4. The ingot is subjected to homogenization, extrusion molding, solution treatment, and aging treatment to obtain the final product.

[0009] Preferably, in S1, the reactive salt includes Na2B4O7 and K2ZrF6.

[0010] More preferably, the mass ratio of Na2B4O7 to K2ZrF6 is 1:(2-3).

[0011] Preferably, in S1, the drying process includes drying at 350–400°C for 2–5 hours.

[0012] The purpose of the initial drying process is to remove the water of crystallization produced by the deliquescence of the reaction salts, which is beneficial for the subsequent mixing and ball milling process.

[0013] Preferably, in S1, ball milling includes ball milling at a rotation speed of 100-500 rpm for 1-3 hours.

[0014] Preferably, in S1, the secondary drying process includes drying at 250–300°C for 1–5 hours.

[0015] The powder after ball milling is subjected to a second drying process for use in subsequent reactions.

[0016] Preferably, in S2, the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu: 0.15–0.4, Mn: 0.15, Mg: 0.8–1.2, Zn: 0.2–0.25, Cr: 0.04–0.35, Ti: 0.1–0.15, Si: 0.4–0.8, Fe ≤ 0.7, with the balance being Al and unavoidable impurities.

[0017] Preferably, in the S2, the melting temperature is 850–900°C.

[0018] Preferably, in S2, the rare earth oxide is selected from one or more of CeO2 and La2O3.

[0019] Preferably, in S2, the amount of rare earth oxide added is 0.05% to 0.5% of the mass of the aluminum alloy matrix.

[0020] Preferably, in S2, the amount of the mixture added is 2% to 3% of the mass of the aluminum alloy matrix.

[0021] Preferably, in step S2, the heating temperature is 900–950°C.

[0022] Preferably, in step S2, the heat preservation time is 1 to 3 hours.

[0023] Preferably, in step S3, refining and impurity removal includes using a protective gas and a refining agent to spray and refine the molten aluminum alloy liquid.

[0024] More preferably, the amount of the refining agent is 1-2 kg / t of aluminum alloy liquid.

[0025] Preferably, in step S4, the homogenization process includes holding at 560–580°C for 8–10 hours and then cooling to room temperature by air cooling.

[0026] This invention achieves homogenization of alloy material composition and eliminates some casting defects through homogenization treatment.

[0027] Preferably, in step S4, the extrusion molding includes an extrusion temperature of 400–520°C and an extrusion ratio of (9–10):1.

[0028] Controlling the extrusion temperature and extrusion ratio during extrusion molding helps improve the density of alloy materials and reduce casting defects such as weld porosity. After heat treatment, some refractory precipitates still exist in the composite material. Some of these precipitates dissolve, and subsequently, dispersed Mg2Si nano-reinforcing phases precipitate, which is beneficial to improving the strength of the material.

[0029] Preferably, in step S4, the solution treatment includes holding at 540–560°C for 8–10 hours and then cooling to room temperature with water.

[0030] Preferably, in S4, the aging treatment includes heating to 160-180°C at a rate of 50-100°C / h, holding at that temperature for 1-3 hours, and then cooling to room temperature by air cooling.

[0031] The present invention also proposes an aluminum alloy prepared by the above preparation method.

[0032] The beneficial effects of this invention are as follows:

[0033] This invention introduces in-situ synthesized ZrB2 particles as a reinforcing phase by adding reactive salts to the alloy material, which is beneficial for improving the strength of the aluminum alloy material. Furthermore, by adding rare earth oxides to the alloy material, the rare earth metals in the oxides can fill lattice defects and synergistically enhance the overall strength with the reactive salts. This also helps to improve the uniform dispersion of ZrB2 particles formed by the reactive salts within the melt, reducing particle aggregation and ensuring that the particles are uniformly distributed in the matrix during solidification, thus achieving stable dispersion of nanoparticles. Detailed Implementation

[0034] The technical solution of the present invention will be described in detail through specific embodiments.

[0035] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.

[0036] Example 1

[0037] A method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy includes the following steps:

[0038] S1. Na2B4O7 and K2ZrF6 are dried separately at 350℃ for 3h. Na2B4O7 and K2ZrF6 are mixed evenly at a mass ratio of 1:2.8 and ball-milled at 150rpm for 3h. The ball-milled powder is dried at 280℃ for 1h to obtain the mixture.

[0039] S2. After melting the aluminum alloy matrix at 850℃ and removing the slag, add 2.5wt% of mixed materials and 0.3wt% of rare earth oxides, heat to 920℃ and stir, and hold for 2 hours to obtain a composite aluminum alloy melt; the rare earth oxides are composed of CeO2 and La2O3 in a mass ratio of 6:1; the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu:0.3, Mn:0.15, Mg:1.1, Zn:0.25, Cr:0.09, Ti:0.15, Si:0.7, Fe:0.35, with the balance being Al and unavoidable impurities;

[0040] S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot;

[0041] S4. Homogenize the ingot: hold at 560℃ for 8 hours, then air-cool to room temperature; Extrusion molding: extrusion temperature is 480℃, extrusion ratio is 9:1; Solution treatment: hold at 540℃ for 9 hours, then water-cool to room temperature; Aging treatment: heat to 170℃ at a rate of 50℃ / h, hold for 2 hours, then air-cool to room temperature to obtain the final product.

[0042] Example 2

[0043] A method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy includes the following steps:

[0044] S1. Na2B4O7 and K2ZrF6 are dried separately at 400℃ for 3 hours. Na2B4O7 and K2ZrF6 are mixed evenly at a mass ratio of 1:2.8 and ball-milled at 200 rpm for 2 hours. The ball-milled powder is dried at 300℃ for 1 hour to obtain the mixture.

[0045] S2. After melting the aluminum alloy matrix at 850℃ and removing the slag, add 2wt% of mixed materials and 0.1wt% of rare earth oxides, heat to 920℃ and stir, and hold for 2 hours to obtain a composite aluminum alloy melt; the rare earth oxides are composed of CeO2 and La2O3 in a mass ratio of 6:1; the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu: 0.3, Mn: 0.15, Mg: 1.1, Zn: 0.25, Cr: 0.09, Ti: 0.15, Si: 0.7, Fe: 0.35, with the balance being Al and unavoidable impurities;

[0046] S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot;

[0047] S4. Homogenize the ingot: Hold at 560℃ for 8 hours, then air-cool to room temperature; Extrusion molding: Extrusion temperature is 480℃, extrusion ratio is 9:1; Solution treatment: Hold at 540℃ for 9 hours, then water-cool to room temperature; Aging treatment: Heat to 175℃ at a rate of 50℃ / h, hold for 2 hours, then air-cool to room temperature to obtain the final product.

[0048] Example 3

[0049] A method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy includes the following steps:

[0050] S1. Na2B4O7 and K2ZrF6 are dried separately at 350℃ for 3h. Na2B4O7 and K2ZrF6 are mixed evenly at a mass ratio of 1:2.8 and ball-milled at 100rpm for 3h. The ball-milled powder is dried at 300℃ for 1h to obtain the mixture.

[0051] S2. After melting the aluminum alloy matrix at 850℃ and removing the slag, add 3wt% of mixed materials and 0.5wt% of rare earth oxides, heat to 950℃ and stir, and hold for 2 hours to obtain a composite aluminum alloy melt; the rare earth oxides are composed of CeO2 and La2O3 in a mass ratio of 6:1; the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu: 0.3, Mn: 0.15, Mg: 1.1, Zn: 0.25, Cr: 0.09, Ti: 0.15, Si: 0.7, Fe: 0.35, with the balance being Al and unavoidable impurities;

[0052] S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot;

[0053] S4. Homogenize the ingot: hold at 560℃ for 8 hours, then air-cool to room temperature; Extrusion molding: extrusion temperature is 480℃, extrusion ratio is 9:1; Solution treatment: hold at 540℃ for 9 hours, then water-cool to room temperature; Aging treatment: heat to 170℃ at a rate of 50℃ / h, hold for 2 hours, then air-cool to room temperature to obtain the final product.

[0054] Example 4

[0055] A method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy includes the following steps:

[0056] S1. Na2B4O7 and K2ZrF6 are dried separately at 350℃ for 3h. Na2B4O7 and K2ZrF6 are mixed evenly at a mass ratio of 1:2.8 and ball-milled at 180rpm for 3h. The ball-milled powder is dried at 280℃ for 1h to obtain the mixture.

[0057] S2. After melting the aluminum alloy matrix at 850℃ and removing the slag, add 2.5wt% of mixed materials and 0.25wt% of rare earth oxides, heat to 950℃ and stir, and hold for 2 hours to obtain a composite aluminum alloy melt; the rare earth oxides are composed of CeO2 and La2O3 in a mass ratio of 6:1; the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu:0.3, Mn:0.15, Mg:1.1, Zn:0.25, Cr:0.09, Ti:0.15, Si:0.7, Fe:0.35, with the balance being Al and unavoidable impurities;

[0058] S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot;

[0059] S4. Homogenize the ingot: Hold at 560℃ for 8 hours, then air-cool to room temperature; Extrusion molding: Extrusion temperature is 480℃, extrusion ratio is 10:1; Solution treatment: Hold at 540℃ for 9 hours, then water-cool to room temperature; Aging treatment: Heat to 170℃ at a rate of 50℃ / h, hold for 2 hours, then air-cool to room temperature to obtain the final product.

[0060] The tensile strength, yield strength, and elongation of the above aluminum alloy were tested. The test results are shown in Table 1.

[0061] Table 1

[0062] Group Tensile strength (MPa) Yield strength (MPa) Elongation (%) Example 1 465 433 12.5 Example 2 445 420 11.8 Example 3 478 459 13.1 Example 4 461 432 12.3

[0063] In summary, the aluminum alloy prepared by this invention has high strength.

[0064] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for manufacturing an in-situ synthesized reinforced high-strength aluminum alloy, characterized in that, Includes the following steps: S1. The reaction salt is dried once, ball-milled, and dried a second time to obtain a mixture. S2. After melting the aluminum alloy matrix and removing the slag, add the mixed materials and rare earth oxides, heat and stir, and keep warm to obtain the composite aluminum alloy melt; S3. Remove slag from the composite aluminum alloy melt, refine and remove impurities, pour and cool to form an ingot; S4. The ingot is subjected to homogenization, extrusion molding, solution treatment, and aging treatment to obtain the final product.

2. The manufacturing method according to claim 1, characterized in that, In S1, the reactive salts include Na2B4O7 and K2ZrF6.

3. The manufacturing method according to claim 2, characterized in that, The mass ratio of Na2B4O7 to K2ZrF6 is 1:(2-3).

4. The manufacturing method according to claim 1, characterized in that, In S1, the first drying process includes drying at 350-400℃ for 2-5 hours; ball milling includes ball milling at 100-500 rpm for 1-3 hours; and the second drying process includes drying at 250-300℃ for 1-5 hours.

5. The manufacturing method according to claim 1, characterized in that, In S2, the chemical composition of the aluminum alloy matrix, by mass percentage, includes: Cu: 0.15–0.4, Mn: 0.15, Mg: 0.8–1.2, Zn: 0.2–0.25, Cr: 0.04–0.35, Ti: 0.1–0.15, Si: 0.4–0.8, Fe≤0.7, with the balance being Al and unavoidable impurities.

6. The manufacturing method according to claim 1, characterized in that, In the S2 described above, the melting temperature is 850–900℃; the heating temperature is 900–950℃; and the holding time is 1–3 hours.

7. The manufacturing method according to claim 1, characterized in that, In S2, the rare earth oxide is selected from one or more of CeO2 and La2O3; the amount of rare earth oxide added is 0.05% to 0.5% of the mass of the aluminum alloy matrix; the amount of the mixture added is 2% to 3% of the mass of the aluminum alloy matrix.

8. The manufacturing method according to claim 1, characterized in that, In S3, refining and impurity removal includes using protective gas and refining agent to spray and refine the molten aluminum alloy liquid to remove impurities.

9. The manufacturing method according to claim 1, characterized in that, In S4, the homogenization process includes holding at 560–580°C for 8–10 hours and then air-cooling to room temperature; the extrusion molding process includes an extrusion temperature of 400–520°C and an extrusion ratio of (9–10):1; the solution treatment process includes holding at 540–560°C for 8–10 hours and then water-cooling to room temperature; and the aging treatment process includes heating to 160–180°C at a rate of 50–100°C / h, holding for 1–3 hours, and then air-cooling to room temperature.

10. An aluminum alloy obtained by the manufacturing method according to any one of claims 1 to 9.