Mussel bionic well wall thermal insulation material for drilling fluid as well as preparation method and application thereof
By combining a mussel-inspired biomimetic adhesive polymer with nano-insulating hollow spheres, the problem of traditional drilling fluid insulation materials detaching under high temperature and high shear force was solved, achieving efficient wellbore adsorption and a stable insulation barrier, thus improving the insulation performance of ultra-deep wells.
Patent Information
- Application Number
- CN202510987799.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-17
- Publication Date
- 2025-12-05
AI Technical Summary
Traditional drilling fluid insulation materials detach due to insufficient adsorption in ultra-deep drilling, failing to effectively block heat transfer between the wellbore and the formation. Furthermore, existing materials are prone to failure under high temperature and high shear stress conditions, thus failing to meet high-temperature insulation requirements.
Adopting a mussel-inspired design, the material combines a viscous polymer, a structural reinforcement material, and a nano-insulating hollow sphere material. The viscous polymer forms chemical bonds with the well wall rock at high temperatures, and a multi-layered thermal barrier network is constructed by combining it with a nanoporous fiber network to achieve slow release and efficient adsorption of the material.
It significantly improves the thermal insulation effect in high-temperature environments, solves the problem of traditional materials easily falling off in ultra-deep well environments, provides a stable thermal insulation barrier, and ensures the safety and thermal insulation performance of the drilling process.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of oil field chemistry, and particularly relates to a mussel bionic well wall heat insulation material for drilling fluid and a preparation method and application thereof. BACKGROUND
[0002] With the acceleration of oil and gas exploration into ultra-deep layers, the bottom hole temperature generally breaks through 200 DEG C. The extreme high temperature leads to rapid heat transfer from the formation to the wellbore, increasing the risk of rheological property loss of control, filter loss surge and well wall collapse of the drilling fluid. At present, the ground cooling method has little effect on downhole cooling. With the increase of well depth by 1000 meters, the regulation efficiency of the bottom hole temperature by the ground cooling method is reduced by about 30%-50%.
[0003] In ultra-deep oil and gas drilling, heat exchange between the wellbore and the formation is the main reason for high downhole temperature. Traditional heat insulation technologies such as nitrogen annulus heat insulation, vacuum heat insulation casing or heat insulation tubing mainly reduce the heat transfer efficiency through physical blocking, but their stability has significant limitations in complex wellbore environments. The active blocking of the heat transfer path by the well wall adsorption heat insulation layer provides a new solution for downhole cooling. However, because of the extremely fast fluid flow rate in the wellbore and the high formation pressure, it is difficult for the heat insulation material to be adsorbed on the well wall, resulting in heat insulation failure. For example, the invention patent CN119504150A discloses a heat-insulating hollow microsphere with high strength and its preparation method and application. The pressure resistance of 90% volume survival rate of the hollow microsphere reaches 29.2 MPa, and the thermal conductivity is as low as 0.063 W / m·K. However, since the surface of the hollow microsphere does not have chemical bonds to adsorb the well wall rock, it cannot be applied to well wall heat insulation materials. The invention patent CN119503809A discloses a high-temperature-resistant ablation heat-insulating aerogel and its preparation method and application. The temperature resistance capacity reaches 1700 DEG C, the thermal conductivity is as low as 0.015 W / m·K, and it has excellent elasticity. However, due to the difficulty of the structure strength of the aerogel material to meet the high shear force during drilling, the structure is easily damaged; in addition, the surface chemical properties of the aerogel after high temperature treatment cannot meet the adsorption requirement of the well wall.
[0004] Therefore, it is of great significance to develop a drilling fluid heat insulation material that breaks through the limitation of low adhesion strength of traditional materials and has high heat insulation, high strength and high adhesion. SUMMARY
[0005] In view of the deficiencies of the prior art, the present application provides a kind of drilling fluid with mussel bionic well wall heat insulation material and its preparation method and application.The drilling fluid with mussel bionic well wall heat insulation material of the present application is prepared from viscous polymer, structural reinforcement material, nano heat insulation hollow ball material and coating material, and has the characteristics of low thermal conductivity, high strength, slow release of viscosity, and high adhesive strength;When the heat insulation material reaches the high temperature stratum, the outermost coating layer gradually breaks down under the action of high temperature and high speed shear force, and the inner layer of viscous polymer-structural reinforcement material-nano heat insulation hollow ball material composite material is slowly released, the viscous polymer is combined with the well wall rock through chemical bond, so that the above-mentioned composite material is tightly adsorbed on the well wall to form a stable heat insulation barrier, solving the problem of falling caused by insufficient adsorption force of traditional materials, and significantly improving the heat insulation effect in high temperature environment.
[0006] The technical scheme of the present application is as follows: A kind of drilling fluid with mussel bionic well wall heat insulation material, it is prepared from the following raw materials: viscous polymer, structural reinforcement material, nano heat insulation hollow ball material and coating material. The preparation method of viscous polymer includes the steps of: dispersing catechol-4-carboxylic acid and monomer in solvent, adding initiator aqueous solution, and obtaining viscous polymer by reaction;The monomer is one or a combination of two or more of N, N-dimethyl acrylamide, dimethyl diallyl ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, 2-acrylamido-2-methylpropane sulfonic acid or sodium acrylsulfonate; The structural reinforcement material is one or a combination of two or more of nano-porous silica fiber, nano-porous titanium dioxide fiber or nano-porous zirconium oxide fiber; The nano heat insulation hollow ball material is one or a combination of two or more of nano silica hollow ball, nano titanium dioxide hollow ball or nano zirconium oxide hollow ball; The coating material is one or a combination of two or more of phenolic epoxy resin, acrylic resin or polyphenylene sulfide.
[0007] According to the present application, in the preparation method of viscous polymer, the mass ratio of catechol-4-carboxylic acid, monomer and solvent is 1: (1.5-5.5): (2-6).
[0008] According to the present application, in the preparation method of viscous polymer, the solvent is a mixed solution of water and ethanol, and the mass ratio of water and ethanol is 8:1-3.
[0009] According to the present application, in the preparation method of viscous polymer, after catechol-4-carboxylic acid and monomer are added to the solvent, stirring and mixing are carried out in a protective gas atmosphere at 60-80℃ for 1-5h to disperse them sufficiently.
[0010] According to the application, preferably, in the preparation method of the viscous polymer, the initiator is azobisdimethylimidazoline hydrochloride, azobisdimethylformamide hydrochloride, ammonium persulfate or potassium persulfate, and the mass concentration of the aqueous initiator solution is 2%-10%.
[0011] According to the application, preferably, in the preparation method of the viscous polymer, the mass of the initiator is 1%-5% of the total mass of the pyrocatechol-4-carboxylic acid and the monomer.
[0012] According to the application, preferably, in the preparation method of the viscous polymer, the reaction temperature is 60-80℃, the reaction time is 4-10h, and the reaction is carried out in a protective gas atmosphere and under stirring. The protective gas is nitrogen or argon.
[0013] According to the application, preferably, the structural reinforcement material has a diameter of 30-80nm, a length of 1-5μm, a porosity of 30%-60%, and a thermal conductivity of 0.032W / m·K-0.041W / m·K.
[0014] According to the application, preferably, the nano thermal insulation hollow sphere material has a diameter of 80-200nm, a shell thickness of 2-8nm, and a thermal conductivity of 0.017W / m·K-0.031W / m·K.
[0015] According to the application, preferably, the mass ratio of the viscous polymer, the structural reinforcement material and the nano thermal insulation hollow sphere material is 1:(0.01-0.04):(0.02-0.1), and preferably 1:(0.02-0.03):(0.04-0.06); and the mass ratio of the total mass of the viscous polymer, the structural reinforcement material and the nano thermal insulation hollow sphere material to the mass of the coating material is 1:(0.1-1), and preferably 1:(0.5-0.6).
[0016] According to the application, preferably, the drilling fluid bivalve biomimetic well wall thermal insulation material has a thermal conductivity of 0.055-0.074W / m·K and an adhesive strength of 14.2-20.4MPa.
[0017] The preparation method of the drilling fluid bivalve biomimetic well wall thermal insulation material comprises the following steps: (1) The viscous polymer, the structural reinforcement material and the nano thermal insulation hollow sphere material are fully mixed and uniformly dispersed, and then freeze-dried and ground to obtain a viscous polymer composite nano material; (2) The coating material is heated to be molten, the viscous polymer composite nano material is added and fully mixed and uniformly dispersed, and then freeze-dried and ground to obtain the drilling fluid bivalve biomimetic well wall thermal insulation material.
[0018] According to the application, preferably, in step (1), the viscous polymer, the structure reinforcing material and the nano thermal insulation hollow sphere material are mixed, and then stirred at 60-80 DEG C for 1-5 hours to fully mix and disperse uniformly.
[0019] According to the application, preferably, in step (1), the viscous polymer composite nano material is ground to a particle size of 10-80 mu m.
[0020] According to the application, preferably, in step (2), after the viscous polymer composite nano material is added, stirring is carried out at a melting temperature for 1-6 hours to fully mix and disperse uniformly.
[0021] According to the application, preferably, in step (2), the grinding is carried out to a particle size of 10-80 mu m.
[0022] The application of the mussel-bionic well wall thermal insulation material for drilling fluid in the thermal insulation of a drilling wellbore.
[0023] The technical features and beneficial effects of the application are as follows: 1. The application first mixes a viscous polymer, a structure reinforcing material and a nano thermal insulation hollow sphere material to prepare a viscous polymer composite nano material, and then coats the viscous polymer composite nano material with a coating material, thereby effectively preventing the viscous component from being adsorbed on the inner wall of a drill pipe during the circulation of drilling fluid. When the thermal insulation material reaches a high-temperature formation, the coating layer is gradually broken under the action of high temperature and high-speed shearing force, and the viscous polymer composite nano material is slowly released. This viscous slow-release design not only avoids adhesion loss during the material transportation stage, but also ensures efficient use at the target location.
[0024] 2. The concept of mussel-bionics originates from the unique adhesion mechanism of the byssal thread protein of marine mussels. The adhesive protein secreted by the byssal thread of mussels can firmly adhere to the surface of a substrate such as rock in a moist, high-salt and dynamic marine environment, and the core function originates from the catechol group in the molecule. The catechol group can form quinone substances through oxidation, and chelate with the surface of the substrate to form stable covalent bonds, thereby realizing high-strength adhesion. The viscous polymer in the application has excellent temperature resistance, and at the same time, the viscous polymer has the characteristics of mimicking the secretion of viscous protein by mussels, and the viscosity gradually increases at high temperatures. After the coating layer of the thermal insulation material is broken, the viscous polymer in the viscous polymer composite nano material is combined with the rock of the well wall through chemical bonds, so that the viscous polymer composite nano material is tightly adsorbed on the well wall to form a stable thermal insulation barrier. The problem of falling off caused by insufficient adhesion of traditional materials is solved, and the thermal insulation effect in a high-temperature environment is significantly improved.
[0025] 3、The added nano-porous silica fiber structure reinforcing material not only has low thermal conductivity, avoids increasing the overall thermal conductivity, but also strengthens the polymer matrix through the fiber network, avoids mechanical damage caused by high-speed shearing of the drilling fluid, and can realize the synergistic optimization of thermal insulation performance and durability.
[0026] 4、The preparation steps of the application are simple, clear and easy to control, and have broad prospects for industrial production. The raw material composition and preparation method of the application work together to make the thermal insulation material have the advantages of low thermal conductivity, high strength, slow release of viscosity, and high adhesion strength.
[0027] 5、In the mussel-biomimetic well wall thermal insulation material for drilling fluid, nano-hollow microspheres are added, which have low thermal conductivity and small size, and can be uniformly dispersed in the polymer after addition to reduce the thermal conductivity and can build a high-efficiency and long-lasting thermal insulation barrier. The unique closed hollow structure of these microspheres can effectively block heat transfer, and in combination with nano-porous fiber materials, a multi-level thermal resistance network is formed. When the material reaches a high-temperature formation, the microspheres are firmly attached to the surface of the well wall rock with the viscous polymer, which can significantly reduce the conduction of formation heat to the wellbore, effectively solving the problem of easy falling and failure of traditional thermal insulation materials in ultra-deep well environment, and providing protection for safe drilling. DETAILED DESCRIPTION
[0028] The application will be further described below in conjunction with specific examples, but is not limited thereto.
[0029] Meanwhile, the experimental methods described in the following examples are all conventional methods unless otherwise specified; and the reagents and materials described are all commercially available unless otherwise specified.
[0030] Example 1 A preparation method of a mussel-biomimetic well wall thermal insulation material for drilling fluid, comprising the following steps: (1) Put catechol-4-carboxylic acid and 2-acrylamido-2-methylpropane sulfonic acid in a three-necked flask, add a mixed solution of water and ethanol (wherein the mass ratio of water to ethanol is 8:2), continuously stir at 800 rpm under 70℃ water bath and nitrogen atmosphere for 1h, then add 3% mass concentration of azobisimidozolin hydrochloride aqueous solution, stir at 800 rpm under 70℃ water bath and nitrogen atmosphere for 6h to obtain a viscous polymer. The mass ratio of catechol-4-carboxylic acid, 2-acrylamido-2-methylpropane sulfonic acid and solvent is 1:3:4, and the mass of the initiator azobisimidozolin hydrochloride is 3% of the total mass of catechol-4-carboxylic acid and 2-acrylamido-2-methylpropane sulfonic acid.
[0031] (2) The viscous polymer, nano-porous silica fiber and nano-silica hollow sphere are mixed, and then stirred at 70°C in a water bath for 2h at a stirring speed of 600rpm until uniformly dispersed to form a mixed solution, wherein the mass ratio of the viscous polymer, nano-porous silica fiber and nano-silica hollow sphere is 1:0.02:0.06, the nano-porous silica fiber has a diameter of 50nm, a length of 3μm, a porosity of 40% and a thermal conductivity of 0.037W / m·K, and the nano-silica hollow sphere has a diameter of 100nm, a shell thickness of 4nm and a thermal conductivity of 0.021W / m·K.
[0032] (3) The mixed solution in step (2) is freeze-dried, and then ground into fine powder to form a viscous polymer composite nanomaterial, wherein the freeze-drying temperature is -50°C, the freezing time is 36h, and the particle size of the ground fine powder is 50μm.
[0033] (4) The phenolic epoxy resin (epoxy equivalent weight: 170-200, epoxy value≥0.5) is heated to have excellent fluidity, and then poured into the viscous polymer composite nanomaterial in step (3) and stirred at a melting temperature for 3h at 500rpm to uniformly coat the fine powder with the coating material. The mass ratio of the viscous polymer composite nanomaterial to the phenolic epoxy resin is 1:0.5.
[0034] (5) The mixed solution obtained in step (4) is freeze-dried, and then ground into fine powder to obtain a mussel-bionic well wall thermal insulation material for drilling fluid, wherein the freeze-drying temperature is -50°C, the freezing time is 36h, and the particle size of the ground fine powder is 50μm.
[0035] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.055W / m·K, the adhesion strength (after the thermal insulation material is heated to flow at a high temperature, it is coated on a metal (carbon steel sheet) substrate, and the adhesion strength is tested by shear strength) is 19.6MPa, and the reinforcing material and nano-thermal insulation hollow sphere are uniformly dispersed in the polymer.
[0036] Example 2 A method for preparing a mussel-bionic well wall thermal insulation material for drilling fluid is as described in Example 1, except that in step (1), the monomer is replaced by dimethyldiallylammonium chloride. The other steps and conditions are the same as in Example 1.
[0037] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.059W / m·K, the adhesion strength is 17.6MPa, and the reinforcing material and nano-thermal insulation hollow sphere are uniformly dispersed in the polymer.
[0038] Example 3 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Embodiment 1, except that in step (1), the monomer is replaced by a combination of 2-acrylamido-2-methylpropanesulfonic acid and dimethyldiallylammonium chloride, wherein the mass ratio of 2-acrylamido-2-methylpropanesulfonic acid to dimethyldiallylammonium chloride is 1:0.4, and the total mass ratio of catechol-4-carboxylic acid to monomer is 1:3. The other steps and conditions are the same as in Embodiment 1.
[0039] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.057 W / m·K, the adhesive strength is 18.2 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0040] Embodiment 4 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Embodiment 1, except that in step (1), the mass ratio of catechol-4-carboxylic acid to monomer is 1:4. The other steps and conditions are the same as in Embodiment 1.
[0041] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.057 W / m·K, the adhesive strength is 16.2 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0042] Embodiment 5 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Embodiment 1, except that in step (2), the nano thermal insulation hollow sphere material is nano titanium dioxide hollow spheres (diameter 100 nm, shell thickness 4 nm, thermal conductivity 0.027 W / m·K). The other steps and conditions are the same as in Embodiment 1.
[0043] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.061 W / m·K, the adhesive strength is 18.9 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0044] Embodiment 6 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Embodiment 1, except that in step (2), the mass ratio of viscous polymer, nano porous silica fiber, and nano silica hollow sphere is 1:0.03:0.04. The other steps and conditions are the same as in Embodiment 1.
[0045] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.072 W / m·K, the adhesive strength is 20.4 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0046] Embodiment 7 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (2), the type of structural reinforcement material is nano-porous titanium dioxide fiber (diameter of 60 nm, length of 3.2 μm, porosity of 33%, and thermal conductivity of 0.04 W / m·K). The other steps and conditions are the same as in Example 1.
[0047] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.062 W / m·K, the adhesive strength is 19.3 MPa, and the reinforcement material and nano-thermal hollow spheres are uniformly dispersed in the polymer.
[0048] Example 8 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (4), the mass ratio of the viscous polymer composite nano-material to the phenolic epoxy resin is 1:0.6. The other steps and conditions are the same as in Example 1.
[0049] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.074 W / m·K, the adhesive strength is 14.2 MPa, and the reinforcement material and nano-thermal hollow spheres are uniformly dispersed in the polymer.
[0050] Example 9 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (4), the coating material is acrylic resin. The other steps and conditions are the same as in Example 1.
[0051] The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid prepared in this example is 0.065 W / m·K, the adhesive strength is 17.8 MPa, and the reinforcement material and nano-thermal hollow spheres are uniformly dispersed in the polymer.
[0052] Comparative Example 1 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (1), catechol-4-carboxylic acid is not added. The other steps and conditions are the same as in Example 1.
[0053] The well wall thermal insulation material for drilling fluid prepared in this comparative example does not have the high adsorption strength of a mussel-bionic material, the thermal conductivity is 0.057 W / m·K, the adhesive strength is 3.6 MPa, and the reinforcement material and nano-thermal hollow spheres are uniformly dispersed in the polymer.
[0054] Comparative Example 2 A preparation method of a mussel-bionic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (1), 2-acrylamido-2-methylpropane sulfonic acid is not added. The other steps and conditions are the same as in Example 1.
[0055] The high temperature resistance of the well wall thermal insulation material for drilling fluid prepared in this comparative example is reduced compared to Example 1, the thermal conductivity is 0.059 W / m·K, the adhesive strength is 11.3 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0056] Comparative Example 3 A preparation method of a mussel biomimetic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (2), the mass ratio of the adhesive polymer, nano-porous silica fiber and nano-silica hollow sphere is 1:0.03:0.15. The other steps and conditions are the same as in Example 1.
[0057] The thermal conductivity of the mussel biomimetic well wall thermal insulation material for drilling fluid prepared in this comparative example is 0.046 W / m·K, the adhesive strength is 5.3 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0058] Comparative Example 4 A preparation method of a mussel biomimetic well wall thermal insulation material for drilling fluid, as described in Example 1, except that in step (2), no coating material is added, i.e. steps (4) and (5) are omitted. The other steps and conditions are the same as in Example 1.
[0059] The mussel biomimetic well wall thermal insulation material for drilling fluid prepared in this comparative example will be adsorbed prematurely and cannot reach the target formation, the thermal conductivity is 0.055 W / m·K, the adhesive strength is 18.6 MPa, and the reinforcing material and nano thermal insulation hollow spheres are uniformly dispersed in the polymer.
[0060] Test Example 1 Adhesion performance study (1) Prepare the base drilling fluid with the formula of water, bentonite, ultra-fine calcium carbonate, and barite. Mix the materials in the formula, then disperse at 5000 rpm for 1 h, and then age at room temperature for 24 h for standby. The mass ratio of water, bentonite, ultra-fine calcium carbonate, and barite is 100:4:3:2; (2) Disperse the thermal insulation materials prepared in the examples and comparative examples into the base drilling fluid of step (1), stir at 2000 rpm for 1 h, then put the core into the aging tank together with the thermal insulation materials, the mass ratio of drilling fluid to thermal insulation material is 1:0.05, the heat rolling temperature is 120℃, 160℃, 200℃ respectively, and the heat rolling time is 16 h; (3) After cooling the aging tank in step (2), take out the core, dry the core, then weigh it, and then subtract the weight of the core itself from the weight of the dried core to get the adsorption amount. The test results are shown in Tables 1 and 2.
[0061] Test Example 2 Thermal insulation performance study The thermal insulation material was heated to melt, and then coated on the core piece, the coating thickness was 5mm, and the thermal conductivity of the core piece with the coating was tested after the coating was cured. The test results are shown in Table 3.
[0062] The above-described embodiments only express the implementation of the present application, but cannot be interpreted as a limitation to the scope of the patent of the present application. It should be pointed out that, for those skilled in the art, without departing from the concept of the present application, a number of modifications and improvements can be made, which all belong to the protection scope of the present application.
Claims
1. A mussel-biomimetic well wall thermal insulator for drilling fluids, characterized by, The preparation of the adhesive polymer, the structural reinforcement material, the nano thermal insulation hollow sphere material and the coating material are as follows: The preparation method of the adhesive polymer comprises the following steps: dispersing catechol-4-carboxylic acid and monomers in a solvent, adding an initiator aqueous solution, and reacting to obtain the adhesive polymer; the monomers are one or a combination of two or more of N,N-dimethyl acrylamide, dimethyldiallylammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, 2-acrylamido-2-methylpropanesulfonic acid and sodium allylsulfonate; The structural reinforcement material is one or a combination of two or more of nano-porous silica fiber, nano-porous titanium dioxide fiber or nano-porous zirconium oxide fiber; The nano thermal insulation hollow sphere material is one or a combination of two or more of nano-silica hollow sphere, nano-titanium dioxide hollow sphere or nano-zirconium oxide hollow sphere; The coating material is one or a combination of two or more of phenolic epoxy resin, acrylic resin or polyphenylene sulfide.
2. The mussel-bionic well wall thermal insulation material for drilling fluid according to claim 1, characterized in that, In the preparation method of the adhesive polymer, one or more of the following conditions is included: i. The mass ratio of catechol-4-carboxylic acid, monomers and solvent is 1:(1.5-5.5):(2-6); ii. The solvent is a mixed solution of water and ethanol, and the mass ratio of water to ethanol is 8:1-3; iii. After catechol-4-carboxylic acid and monomers are added to the solvent, stirring and mixing are carried out in a protective gas atmosphere at 60-80℃ for 1-5h to achieve sufficient dispersion; the protective gas is nitrogen or argon; iv. The initiator is azobisimidozolinium hydrochloride, azobisimidazolinium hydrochloride, ammonium persulfate or potassium persulfate, and the mass concentration of the initiator aqueous solution is 2%-10%; v. The mass of the initiator is 1%-5% of the total mass of catechol-4-carboxylic acid and monomers; vi. The reaction temperature is 60-80℃, the reaction time is 4-10h, and the reaction is carried out in a protective gas atmosphere under stirring; the protective gas is nitrogen or argon.
3. The mussel-bionic well wall thermal insulation material for drilling fluid according to claim 1, characterized in that, The diameter of the structural reinforcement material is 30-80nm, the length is 1-5μm, the porosity is 30%-60%, and the thermal conductivity is 0.032W / m·K-0.041W / m·K.
4. The mussel-bionic well wall thermal insulating material for drilling fluid according to claim 1, characterized in that, The diameter of the nano thermal insulation hollow sphere material is 80-200nm, the shell thickness is 2-8nm, and the thermal conductivity is 0.017W / m·K-0.031W / m·K.
5. The mussel-inspired wellbore heat shield material for drilling fluids of claim 1, wherein, The mass ratio of the adhesive polymer, the structural reinforcement material and the nano thermal insulation hollow sphere material is 1:(0.01-0.04):(0.02-0.1), and preferably 1:(0.02-0.03):(0.04-0.06); the mass ratio of the total mass of the adhesive polymer, the structural reinforcement material and the nano thermal insulation hollow sphere material to the mass of the coating material is 1:(0.1-1), and preferably 1:(0.5-0.6).
6. The mussel-bionic well wall thermal insulator for drilling fluid according to claim 1, characterized in that, The thermal conductivity of the mussel-bionic well wall thermal insulation material for drilling fluid is 0.055-0.074W / m·K, and the adhesive strength is 14.2-20.4MPa.
7. The preparation method of the mussel-bionic well wall thermal insulation material for drilling fluid according to any one of claims 1-6, comprising the following steps: (1) The viscous polymer, the structure reinforcing material, and the nano thermal insulation hollow sphere material are mixed and dispersed uniformly, and then freeze-dried and ground to obtain the viscous polymer composite nano material; (2) The coating material is heated to be molten, the viscous polymer composite nano material is added, and then mixed and dispersed uniformly, and then freeze-dried and ground to obtain the mussel bionic well wall thermal insulation material for drilling fluid.
8. The method of claim 7, wherein the method is characterized by: In step (1), one or more of the following conditions is included: i. After mixing the viscous polymer, the structure reinforcing material, and the nano thermal insulation hollow sphere material, stirring is performed at 60-80°C for 1-5h to sufficiently mix and disperse the materials; ii. The viscous polymer composite nano material is ground to a particle size of 10-80μm.
9. The method of claim 7, wherein the method is characterized by: In step (2), one or more of the following conditions is included: i. After adding the viscous polymer composite nano material, stirring is performed at the melting temperature for 1-6h to sufficiently mix and disperse the materials; ii. The material is ground to a particle size of 10-80μm.
10. Use of the mussel bionic well wall thermal insulation material for drilling fluid according to any one of claims 1-6 in thermal insulation of a drilling wellbore.
Citation Information
Patent Citations
High-temperature-ablation-resistant heat-insulating aerogel as well as preparation method and application thereof
CN119503809A
Heat-insulating hollow microsphere with high strength as well as preparation method and application of heat-insulating hollow microsphere
CN119504150A
Cited By
Silicon dioxide hollow microsphere shaft thermal insulation material prepared by taking lignin particles as template as well as preparation method and application of silicon dioxide hollow microsphere shaft thermal insulation material
CN122188600A
A kind of hollow silica microsphere wellbore thermal insulation material prepared by lignin particle as template and its preparation method and application
CN122188600B