A near-net shape continuous casting system, method and application for directly producing hollow tube blanks
Patent Information
- Application Number
- CN202511213091.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-28
- Publication Date
- 2026-06-23
- Estimated Expiration
- 2045-08-28
Smart Images

Figure CN121178805B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of continuous casting of hollow steel tube blanks and non-ferrous metal tube blanks, specifically relating to a near-net-shape continuous casting system, method and application for directly producing hollow tube blanks. Background Technology
[0002] Steel pipes, especially seamless steel pipes, are widely used in many fields such as petrochemicals, energy and power, aerospace and military, transportation, and food industry. At the same time, the output, variety, quality and technical equipment level of seamless steel pipe production are also important indicators of a country's industrial progress.
[0003] Seamless steel pipe production typically involves skew rolling of solid round billets into hollow tube blanks, followed by hot working processes such as stretching, leveling, diameter reduction, and sizing. See attached document for details. Figure 4 During the skew rolling piercing of solid round billets, the stress, deformation, and flow of the metal are complex. Circumferential shear strain, longitudinal shear deformation, and surface distortion can easily lead to defects on the inner and outer surfaces and inside the tube. Furthermore, the quality of the solid round billet directly affects the product quality and yield. In seamless steel pipe production (starting from the cast billet), the energy consumption for skew rolling piercing to produce hollow tube billets accounts for approximately 20% to 30% of the total energy consumption. If hollow tube billets were used directly instead of solid round billets to produce seamless steel pipes, the skew rolling piercing process could be eliminated, greatly simplifying the seamless steel pipe production process, improving product quality, increasing metal yield, reducing production costs, and saving on infrastructure investment. Currently, some technologies for producing hollow tube billets directly through continuous casting have emerged, such as centrifugal casting, hollow casting (with internal and external double crystallizers), and near-net-shape continuous casting machine technologies for producing hollow tube billets using spray deposition. However, these technologies are mostly in the theoretical or experimental research stage due to their high technical difficulty, low metal yield, and high production costs, and are rarely applied in large-scale production practice. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a near-net-shape continuous casting system, method, and application for directly producing hollow tube blanks.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] A near-net-shape continuous casting system for directly producing hollow tube billets includes a ladle, a long nozzle, a tundish, a separation ring, a crystallizer, a fan-shaped section, a fan-shaped section drive device, secondary cooling water nozzles, a billet cutting device, and a billet discharge device. The ladle and tundish are arranged vertically and connected by a long nozzle. The bottom of the tundish is connected to the crystallizer, which is inclined upwards at the outlet, via the separation ring. The outlet end of the crystallizer is inclinedly connected to the fan-shaped section, which is connected to the fan-shaped section drive device. The bottom of the tundish, the separation ring, and the crystallizer form a connected solidification cavity for molten steel at an angle θ to the horizontal plane. A secondary cooling water nozzle for cooling is provided in the middle of the fan-shaped section. The billet cutting device is located at the billet outlet end of the fan-shaped section and is used to cut the hollow tube billets. The billet discharge device is located in the billet discharge direction at the billet outlet end of the fan-shaped section and is used to output the hollow tube billets.
[0007] It also includes a billet core blowing device; the billet core blowing device is located at the billet outlet end of the fan-shaped section and is used to blow inert protective gas into the core of the hollow tube billet.
[0008] The core blowing device for the billet includes at least a track, a control device, a nozzle, and an air source; the nozzle is connected to the track; the air source is connected to the nozzle for providing air jets to the nozzle; the control device is connected to the nozzle and the air source for controlling the supply and interruption of the air source, and simultaneously controlling the nozzle to move synchronously with the hollow billet.
[0009] The upward direction of the crystallizer and the sector segment forms the same angle with the horizontal line of the hollow tube blank output direction; the crystallizer is a circular crystallizer.
[0010] The included angle is θ, where 0° < θ < 90°.
[0011] The billet cutting device includes at least a slide rail, a drive device, and a cutting torch; the cutting torch is connected to the slide rail; the drive device is used to drive the cutting torch to move synchronously with the hollow tube billet on the slide rail.
[0012] The separation ring is a ring-shaped refractory seal made of zirconium oxide; the separation ring is used for sealing the connection between the tundish and the crystallizer.
[0013] Application of a near-net-shape continuous casting system for directly producing hollow tube blanks: This near-net-shape continuous casting system is applied to the continuous casting of hollow tube blanks of all non-ferrous metals or non-ferrous metal alloys or ferrous metals or ferrous metal alloys.
[0014] A casting method for a near-net-shape continuous casting system that directly produces hollow tube blanks includes the following steps.
[0015] Step 1: The steel smelting system produces qualified liquid steel;
[0016] Step 2: Molten steel flows from the ladle into the tundish through the long nozzle;
[0017] Step 3: Formation of the initial solidified shell;
[0018] Molten steel flowing into the tundish passes through the immersion nozzle and separation ring at the bottom of the tundish and flows into the crystallizer. Under the forced cooling of the crystallizer, the molten steel near the side wall surface of the crystallizer first solidifies to form a primary solidified shell with a certain thickness. The molten steel in the center of the solidified shell is still liquid.
[0019] Step 4: The solidified shell exiting the crystallizer is continuously pulled out obliquely upwards in a spiral under the traction force and radial rotation force of the fan-shaped section;
[0020] Step 5: The solidified shell is further cooled;
[0021] The solidified billet shell exiting the crystallizer is further cooled by spraying with two cooling water nozzles set on the fan-shaped section, which further thickens the solidified billet shell.
[0022] Step Six: Formation of Hollow Tube Blank;
[0023] When the solidified billet shell is pulled upward at an angle θ to a height higher than the molten steel surface in the tundish, only a solidified hollow billet shell with a certain thickness is left inside the tube blank, thus forming a hollow tube blank.
[0024] Step 7: The billet cutting device cuts and outputs the hollow tube billet;
[0025] When the hollow tube billet passes through the cutting area where the billet cutting device is located, the billet cutting device cuts the hollow tube billet to the specified length according to the fixed length requirement. Then, the billet exiting equipment swings the hollow tube billet to a horizontal state and transports it to the steel rolling workshop.
[0026] In step four, the solidified shell is continuously pulled out obliquely upwards at a speed of 0.01 to 10 m / min under the traction force and radial rotation of the fan-shaped section.
[0027] Beneficial effects:
[0028] (1) The present invention can eliminate the hot rolling and piercing process from solid billet to hollow billet, which will greatly simplify the production process of seamless steel pipe, reduce the total energy consumption of seamless steel pipe production (from continuous casting billet) by 25% to 40%, and increase the metal yield by more than 2% to 5%.
[0029] (2) The present invention can realize the fully sealed casting of hollow tube blanks, which can effectively reduce the secondary oxidation of molten steel and effectively improve the purity of the casting blank.
[0030] (3) The hollow tube blank produced by the present invention does not undergo bending and straightening processes, which effectively solves the problem of cracks caused by bending and straightening forces in solidified casting blanks produced by arc continuous casting machines.
[0031] (4) The core of the hollow tube blank produced by the present invention does not participate in solidification, and the porosity and segregation in the center of the billet can be completely solved.
[0032] (5) The implementation of this invention is relatively simple, the equipment is simple, the investment cost is low, and it is very conducive to its application in industrial production.
[0033] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0034] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0035] Figure 1 This is a schematic diagram of the present invention.
[0036] Figure 2 This is a production flow diagram of the hollow tube blank of the present invention.
[0037] Figure 3 The production process of seamless steel pipes using hollow tube blanks.
[0038] Figure 4 This refers to the traditional seamless steel pipe production process.
[0039] In the diagram: 1. Ladle; 2. Long nozzle; 3. Tundish; 4. Separation ring; 5. Crystallizer; 6. Sector section; 7. Sector section drive device; 8. Secondary cooling water nozzle; 9. Hollow tube billet; 10. Billet cutting device; 11. Billet core blowing device; 12. Billet unloading equipment. Detailed Implementation
[0040] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0041] Example 1:
[0042] according to Figure 1 and Figure 2 The diagram illustrates a near-net-shape continuous casting system for directly producing hollow tube billets, comprising a ladle 1, a long nozzle 2, a tundish 3, a separation ring 4, a crystallizer 5, a fan-shaped section 6, a fan-shaped section drive device 7, secondary cooling water nozzles 8, a billet cutting device 10, and a billet discharge device 12. The ladle 1 and tundish 3 are arranged vertically and connected by the long nozzle 2. The bottom of the tundish 3 is connected to the crystallizer 5, which is inclined upwards at its outlet, via the separation ring 4. The outlet end of the crystallizer 5 is inclinedly connected to the fan-shaped section 6, which is connected to the fan-shaped section drive device 7. The bottom of the tundish 3, the separation ring 4, and the crystallizer 5 form a connected solidification cavity for molten steel at an angle θ to the horizontal plane. Secondary cooling water nozzles 8 are located in the middle of the fan-shaped section 6 for cooling. The billet cutting device 10 is located at the billet outlet end of the fan-shaped section 6 and is used for cutting the hollow tube billets 9. The billet discharge device 12 is located in the billet discharge direction at the billet outlet end of the fan-shaped section 6 and is used for outputting the hollow tube billets 9.
[0043] In practical use, qualified molten steel produced by the steel smelting system flows from ladle 1 through long nozzle 2 into tundish 3. The molten steel flowing into tundish 3 passes through the immersion nozzle at the bottom of tundish 3 and the separation ring 4 into crystallizer 5. Under forced cooling in crystallizer 5, the molten steel near the side wall surface of crystallizer 5 solidifies first, forming a primary solidified shell of a certain thickness. The molten steel at the center of the solidified shell remains molten steel. A separation ring 4 with refractory material can be used to connect tundish 3 and crystallizer 5. When the molten steel enters crystallizer 5, it first contacts the separation ring 4 and solidifies uniformly on the end face of the separation ring 4, which is beneficial for generating a uniform and stable primary solidified shell. The solidified shell exiting crystallizer 5 is continuously pulled out obliquely upwards in a spiral motion under the traction force and radial rotation force of the fan-shaped section 6. Because the molten steel in tundish 3, crystallizer 5, and fan-shaped section 6 are mutually... The interconnected structures, under atmospheric pressure, form a communicating vessel. The molten steel surface inside the initial billet shell and the molten steel surface in the tundish 3 are kept at the same horizontal level. The solidified billet shell is continuously pulled by the fan-shaped section drive device 7 and is pulled obliquely upward out of the crystallizer 5. The initial solidified billet shell exiting the crystallizer 5 is further cooled by the spray of the secondary cooling water nozzles 8 set on the fan-shaped section 6, which further thickens the solidified billet shell. When the solidified billet shell is pulled obliquely upward to a height higher than the molten steel surface inside the tundish 3, only the solidified hollow billet shell with a certain thickness requirement remains inside the tube billet, which forms the hollow tube billet 9. When the hollow tube billet 9 passes through the cutting area where the billet cutting device 10 is located, the billet cutting device 10 cuts the hollow tube billet 9 to the specified length according to the fixed length requirement, and then the hollow tube billet is swung to a horizontal state by the billet exiting device 12 and transported to the rolling mill.
[0044] The hollow tube blank 9 is pulled out obliquely upward by a spiral, which not only allows the blank to be easily demolded from the crystallizer 5 and effectively improves the surface quality of the hollow tube blank 9, but also allows the hollow tube blank 9 to maintain the uniformity of radial thickness.
[0045] This invention eliminates the hot rolling and piercing process from solid billets to hollow billets, significantly simplifying the seamless steel pipe production process. It reduces total energy consumption (from continuous casting) by 25%–40% and increases metal yield by 2%–5% or more. This invention achieves fully sealed casting of hollow billets, effectively reducing secondary oxidation of molten steel and significantly improving billet purity. The hollow billets produced using this invention do not undergo bending and straightening processes, effectively solving the problem of cracks caused by bending and straightening forces in solidified billets produced by arc-shaped continuous casting machines. The central porosity and segregation in the solidification structure of the hollow billets produced using this invention are completely resolved. This invention is relatively simple to implement, requires simple equipment, and has low investment costs, making it highly suitable for industrial production.
[0046] In some embodiments, a core blowing device 11 is also included; the core blowing device 11 is disposed at the billet outlet end of the sector segment 6 and is used to blow inert protective gas into the core of the hollow tube billet 9.
[0047] Furthermore, the core blowing device 11 of the billet includes at least a track, a control device, a nozzle, and an air source; the nozzle is connected to the track; the air source is connected to the nozzle to provide air jet gas to the nozzle; the control device is connected to the nozzle and the air source to control the supply and interruption of the air source, and at the same time control the nozzle to move synchronously with the hollow tube billet 9 on the track.
[0048] In practical use, to improve the smoothness of the inner surface of the hollow tube billet 9 and prevent secondary oxidation of the molten steel inside the hollow tube billet 9, protective gases such as argon or nitrogen can be introduced through the core blowing device 11 at the end of the billet. This will create an inert atmosphere inside the hollow tube billet 9, thereby ensuring uniform solidification of the molten steel inside the hollow tube billet 9. The protective gas is an inert gas, the function of which is to prevent high-temperature oxidation of the tube billet.
[0049] The core blowing device 11 of the billet is matched with the pulling speed of the hollow tube billet 9, and the two can move synchronously.
[0050] In some embodiments, the upward directions of the crystallizer 5 and the sector segment 6 are the same as the angles formed by the horizontal line of the output direction of the hollow tube blank 9; the crystallizer 5 is a circular crystallizer.
[0051] Furthermore, the included angle is θ, where 0° < θ < 90°.
[0052] In practical use, in order to improve the surface quality of the hollow tube blank 9, the clamping roller in the fan-shaped section 6 of the present invention not only makes the tube blank continuously pulled out along the angle θ, but also makes the tube blank rotate along the radial direction of the tube blank. That is, the hollow tube blank 9 is pulled out obliquely upward by a spiral. This not only enables the casting blank to be easily demolded from the crystallizer 5, effectively improving the surface quality of the hollow tube blank 9, but also enables the hollow tube blank 9 to maintain the uniformity of radial thickness.
[0053] In this embodiment, the sector segment 6 includes at least a lifting drive roller, a sector segment frame, and a drive cylinder. The lifting drive roller is connected to the sector segment frame, and the drive cylinder is connected to the lifting drive roller. The sector segment drive device 7 includes a coupling, a motor, and a reducer. The motor and reducer are connected by a coupling, which transmits the torque generated by the motor to the reducer. A long coupling is provided between the output end of the reducer and the drive roller of the sector segment 6, which transmits the increased torque from the reducer to the drive roller of the sector segment 6. The lifting drive roller in this embodiment is based on a mature device available in the prior art.
[0054] In application, this invention allows for the adjustment of the angle θ (0° < θ < 90°) between the crystallizer 5 and the sector segment 6 and the horizontal plane to achieve the thickness requirements of different product specifications. The thickness is determined based on the solidification law of metals or alloys, obtaining the length of the crystallizer cooling and spray cooling water zones, and using trigonometric relationships to determine the specific θ value to meet the thickness requirements of the production specifications. During production, the billet thickness can also be changed by detecting the thickness of the hollow tube billet at the molten steel surface, adjusting the amount of cooling water supplied to the crystallizer and the secondary cooling spray water (the specific water volume is calculated based on the solidification law simulation), and altering the solidification rate to change the billet shell thickness, thereby meeting actual production needs.
[0055] In some embodiments, the billet cutting device 10 includes at least a slide rail, a drive device, and a cutting torch; the cutting torch is connected to the slide rail; the drive device is used to drive the cutting torch to move synchronously with the hollow tube billet 9 on the slide rail.
[0056] In actual use, after passing through the billet cutting device 10, the hollow tube billet 9 is cut to the specified length according to the required length. Then, the billet unloading device 12 swings the hollow tube billet 9 to a horizontal state and transports it to the steel rolling workshop. Throughout the cutting process, the billet cutting device 10 and the hollow tube billet 9 move at the same speed and can move synchronously.
[0057] In some embodiments, the separation ring 4 is an annular refractory seal made of zirconium oxide; the separation ring 4 is used for sealing the connection between the tundish 3 and the crystallizer 5.
[0058] In practical use, the separating ring 4 connects the tundish 3 and the crystallizer 5 to achieve sealed casting. Simultaneously, the separating ring 4 is also the starting point for the initial billet shell. When molten steel enters the crystallizer 5, it first contacts the separating ring 4 and solidifies uniformly on the end face of the separating ring 4, which is beneficial for generating a uniform and stable solidified billet shell. As the production process continues, the hollow billet shell is pulled out, and newly added molten steel reforms a new billet shell at the separating ring 4, thus achieving continuous casting of the hollow tube billet 9.
[0059] Example 2:
[0060] according to Figure 1 and Figure 2 Application of a near-net-shape continuous casting system for directly producing hollow tube blanks: This system is applied to the continuous casting of hollow tube blanks of non-ferrous metals or non-ferrous metal alloys or ferrous metals or ferrous metal alloys.
[0061] In practical use, the equipment used in this invention is simple and the investment cost is relatively low, which is very beneficial for its application in the industrial production of continuously cast hollow tube blanks.
[0062] Example 3:
[0063] Reference Figure 1 and Figure 2 A casting method for a near-net-shape continuous casting system that directly produces hollow tube blanks includes the following steps:
[0064] Step 1: The steel smelting system produces qualified liquid steel;
[0065] Step 2: Molten steel flows from ladle 1 through long nozzle 2 into tundish 3;
[0066] Step 3: Formation of the initial solidified shell;
[0067] Molten steel flowing into tundish 3 passes through the immersion nozzle and separation ring 4 at the bottom of tundish 3 and flows into crystallizer 5. Under the forced cooling of crystallizer 5, the molten steel near the side wall surface of crystallizer 5 solidifies first to form a primary solidified shell with a certain thickness. The molten steel in the center of the solidified shell is still liquid.
[0068] Step 4: The solidified shell of the crystallizer 5 is continuously pulled out obliquely upwards in a spiral under the traction force and radial rotation of the fan-shaped section 6;
[0069] Step 5: The solidified shell is further cooled;
[0070] The solidified shell of the crystallizer 5 is further cooled by the spray of two cooling water nozzles 8 set on the fan-shaped section 6, which further thickens the solidified shell.
[0071] Step Six: Formation of Hollow Tube Blank 9;
[0072] When the solidified billet shell is pulled upward at an angle θ to a height higher than the molten steel surface in the tundish 3, only a solidified hollow billet shell with a certain thickness requirement remains inside the tube billet, thus forming a hollow tube billet 9.
[0073] Step 7: The billet cutting device 10 cuts the hollow tube billet 9 and outputs it;
[0074] When the hollow tube billet 9 passes through the cutting area where the billet cutting device 10 is located, the billet cutting device 10 cuts the hollow tube billet 9 to the specified length according to the fixed length requirement, and then the billet discharge device 12 swings the hollow tube billet 9 to a horizontal state before transporting it to the steel rolling workshop.
[0075] Furthermore, in step four, the solidified shell is continuously pulled out obliquely upwards at a speed of 0.01 to 10 m / min under the traction force and radial rotation of the fan-shaped segment 6.
[0076] The present invention can eliminate the hot rolling and piercing process from solid billet to hollow billet 9, which will greatly simplify the production process of seamless steel pipes, reduce the total energy consumption of seamless steel pipe production (calculated from continuous casting billet) by 25% to 40%, and increase the metal yield by more than 2% to 5%.
[0077] In practical applications, depending on the composition of the molten steel or the non-ferrous metal alloy, the drawing speed may exceed the range of 0.01 to 10 m / min.
[0078] This invention enables fully sealed casting of hollow tube billets 9, which can effectively reduce secondary oxidation of molten steel and effectively improve the purity of the billet.
[0079] The hollow tube blank 9 produced by the present invention does not undergo bending and straightening processes, effectively solving the problem of cracks caused by bending and straightening forces in solidified casting blanks produced by arc continuous casting machines.
[0080] The central porosity and segregation in the solidification structure of the hollow tube blank 9 produced by the present invention can be effectively improved.
[0081] The production process of seamless steel pipes using this invention is as follows: steelmaking, continuous casting, hollow tube billet, rolling, diameter reduction, straightening and finishing to finished product. Compared with the prior art, this process reduces the number of steps.
[0082] Where there is no conflict, those skilled in the art can combine the relevant technical features in the above examples according to the actual situation to achieve the corresponding technical effects. Specific details of the various combinations will not be elaborated here.
[0083] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative positional relationship and movement of each component in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indication will also change accordingly.
[0084] Furthermore, the use of terms such as "first" and "second" in this invention is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features.
[0085] The above description is merely a preferred embodiment of the present invention. The present invention is not limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein. Any simple modifications, equivalent variations, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the present invention.
Claims
1. A near-net-shape continuous casting system for directly producing hollow tube blanks, characterized in that: The system includes a ladle (1), a long nozzle (2), a tundish (3), a separation ring (4), a crystallizer (5), a fan-shaped section (6), a fan-shaped section drive device (7), a secondary cooling water nozzle (8), a billet cutting device (10), and a billet discharge device (12). The ladle (1) and the tundish (3) are arranged vertically and connected by the long nozzle (2). The bottom of the tundish (3) is connected to the crystallizer (5) with its outlet inclined upwards via the separation ring (4). The outlet end of the crystallizer (5) is inclinedly connected to the fan-shaped section (6). The shaped section (6) is connected to the fan-shaped section drive device (7). The bottom of the tundish (3), the separation ring (4), and the crystallizer (5) form a connected solidification cavity for molten steel at an angle θ to the horizontal plane. The middle part of the fan-shaped section (6) is provided with a secondary cooling water nozzle (8) for cooling. The billet cutting device (10) is set at the billet outlet end of the fan-shaped section (6) for cutting the hollow tube billet (9). The billet discharge device (12) is set in the billet discharge direction at the billet outlet end of the fan-shaped section (6) for outputting the hollow tube billet (9).
2. The near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 1, characterized in that: It also includes a billet core blowing device (11); the billet core blowing device (11) is set at the billet outlet end of the fan-shaped section (6) and is used to blow inert protective gas into the core of the hollow tube billet (9).
3. The near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 2, characterized in that: The core blowing device (11) of the billet includes at least a track, a control device, a nozzle and an air source; the nozzle is connected to the track; the air source is connected to the nozzle for providing air to the nozzle; the control device is connected to the nozzle and the air source for controlling the supply and interruption of the air source, and simultaneously controlling the nozzle and the hollow tube billet (9) to move synchronously.
4. A near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 1 or 2, characterized in that: The upward direction of the crystallizer (5) and the fan-shaped section (6) are the same as the angle formed by the horizontal line of the output direction of the hollow tube blank (9); the crystallizer (5) is a circular crystallizer.
5. A near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 4, characterized in that: The included angle is θ, where 0° < θ < 90°.
6. The near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 1, characterized in that: The billet cutting device (10) includes at least a slide rail, a drive device and a cutting torch; the cutting torch is connected to the slide rail; the drive device is used to drive the cutting torch to move synchronously with the hollow tube billet (9) on the slide rail.
7. The near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 1, characterized in that: The separation ring (4) is an annular refractory seal made of zirconium oxide; the separation ring (4) is used for the sealing connection between the tundish (3) and the crystallizer (5).
8. An application of a near-net-shape continuous casting system for directly producing hollow tube blanks, characterized in that: The near-net-shape continuous casting system for directly producing hollow tube blanks as described in any one of claims 1-7 is applied to the continuous casting of hollow tube blanks of all non-ferrous metals or non-ferrous metal alloys or ferrous metals or ferrous metal alloys.
9. A casting method for a near-net-shape continuous casting system that directly produces hollow tube blanks, characterized in that: Includes the following steps, Step 1: The steel smelting system produces qualified liquid steel; Step 2: Liquid steel flows from the ladle (1) through the long nozzle (2) into the tundish (3); Step 3: Formation of the initial solidified shell; Molten steel flowing into the tundish (3) flows into the crystallizer (5) through the immersion port and separation ring (4) at the bottom of the tundish (3); under the forced cooling of the crystallizer (5), the molten steel near the side wall surface of the crystallizer (5) first solidifies to form a primary solidified shell with a certain thickness, and the molten steel in the center of the solidified shell is still liquid molten steel. Step 4: The solidified shell exiting the crystallizer (5) is continuously pulled out obliquely upward spirally under the traction force and radial rotation force of the fan-shaped section (6); Step 5: The solidified shell is further cooled; The solidified shell of the crystallizer (5) is further cooled by the spraying of two cooling water nozzles (8) set on the fan-shaped section (6), which further thickens the solidified shell. Step 6: Formation of hollow tube blank (9); When the solidified billet shell is pulled out obliquely upward at an angle θ to a height higher than the molten steel surface in the tundish (3), only a hollow billet shell that has solidified and has a certain thickness requirement remains in the tube blank, thus forming a hollow tube blank (9). Step 7: The billet cutting device (10) cuts and outputs the hollow tube billet (9); When the hollow tube blank (9) passes through the cutting area where the billet cutting device (10) is located, the billet cutting device (10) cuts the hollow tube blank (9) to the specified length according to the fixed length requirement, and then the billet exiting device (12) swings the hollow tube blank (9) to a horizontal state and transports it to the steel rolling workshop.
10. The casting method of a near-net-shape continuous casting system for directly producing hollow tube blanks as described in claim 9, characterized in that: The solidified shell in step four is pulled out obliquely upwards at a speed of 0.01 to 10 m / min under the traction force and radial rotation of the fan-shaped section (6).
Citation Information
Patent Citations
Vertical jointless steel tube hollow tube blank continuous casting machine
CN2887490Y
Method for manufacturing hollow steel slab for pipe
JP2013000785A