Preparation method of LPSC sulfide solid electrolyte, LPSC sulfide solid electrolyte and application thereof
By introducing Se, Me, and Si elements through a multi-layer coating process, the preparation process of LPSC sulfide solid electrolyte was optimized, solving the problems of air stability and hydrogen sulfide release, and achieving high air stability and high ionic conductivity.
Patent Information
- Application Number
- CN202511413409.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-29
- Publication Date
- 2025-12-23
AI Technical Summary
Existing LPSC sulfide electrolytes have insufficient air stability, especially with low ionic conductivity retention at -40 ℃, and pose a risk of hydrogen sulfide release, affecting safety and processing difficulty.
By employing a multilayer coating process, introducing Se, Me (metal) and Si elements, and optimizing the calcination process through selenium doping and metal oxide coating, LPSC sulfide solid electrolytes were prepared, enhancing the bond energy between elements and suppressing side reactions.
It improves the air stability of LPSC sulfide solid electrolyte, maintaining an ionic conductivity of about 95% at -40 ℃, reducing hydrogen sulfide release, and enhancing safety and processing convenience.
Smart Images

Figure CN121192239A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of all-solid-state batteries, and particularly relates to a preparation method of LPSC sulfide solid electrolyte, the LPSC sulfide solid electrolyte and application thereof. BACKGROUND
[0002] The LPSC sulfide is the main electrolyte of the sulfide solid-state battery. For the sulfide electrolyte, the particle size, the degree of side reaction and the air stability are three core elements. The particle size can be designed to have an ideal size distribution by means of fine grinding and air flow breaking, and the side reaction can be inhibited to different degrees by means of the intervention of metal elements. To some extent, the particle size distribution and the side reaction can be effectively inhibited to achieve a relatively ideal rate and cycle effect, and the air stability problem is delayed. The air stability is related to the relaxation degree of the processing environment, the storage mode of the LPSC sulfide electrolyte, the product timeliness and the economic cost and many other problems. The industry is more focused on the ion conductivity, particle distribution and many other researches of the LPSC sulfide electrolyte, and less on the air stability. The existing technology is more focused on the doping of LiBr, LiI and Br elements and O elements. Although this kind of technical means can improve the air stability to a certain extent, the degree is very limited. Generally, the maintenance of the air stability (the ion conductivity retention rate of the environment exposed to-40 ℃ for 24 h) is in the range of 50-60 %, which is far lower than the expected value of the industry. The reason is that the process is too single. In terms of air stability, there is still a great space. In order to realize the high air stability characteristics that meet the industrial development and market demand, it is necessary to introduce appropriate elements and explore a more complex process. According to the literature, the reaction steps of the LPSC sulfide electrolyte and water are divided into four parts: ① Li2S + H2O → LiSH + LiOH; ② LiSH + H2O → LiOH + H2S; ③ P2S7 4- + H2O → PS3 2- SH + PS3 2- OH; ④ PS3 2- SH + H2O → PS3 2- OH + H2S. The contact of the LPSC sulfide electrolyte and water will produce various side reactions, which will cause obvious destruction of the crystal lattice structure, and then the ion conductivity will be obviously deteriorated. At the same time, the release of hydrogen sulfide will cause irreversible damage to life safety. SUMMARY
[0003] The first object of the application is to provide a preparation method of LPSC sulfide solid electrolyte. The preparation method is simple and easy to operate, and the air stability of the prepared LPSC sulfide solid electrolyte is high.
[0004] A second object of the present application is to provide a LPSC sulfide solid electrolyte prepared according to the aforementioned method.
[0005] A third object of the present application is to provide an application of the aforementioned LPSC sulfide solid electrolyte and the aforementioned solid-state battery in a power automobile.
[0006] To achieve the first object of the present application, the following technical solutions are adopted: A method for preparing a LPSC sulfide solid electrolyte, comprising: (1) adding an additive to a main raw material and performing calcination treatment for selenium doping to obtain a first calcined material; wherein, the main raw material is a first raw material; the first raw material comprises phosphorus pentasulfide, lithium sulfide and lithium chloride; the additive is a first additive; the first additive is selenium dioxide; (2) repeating step (1) by taking a second raw material as the main raw material and taking a second additive as the additive to perform metal element coating to obtain a second calcined material; wherein, the second raw material is the first calcined material obtained in step (1); the second additive is a metal oxide; (3) repeating step (1) by taking a third raw material as the main raw material and taking a third additive as the additive to perform Si element coating to obtain a third calcined material, i.e., a LPSC sulfide solid electrolyte; wherein, the third raw material is the second calcined material obtained in step (2); the third additive is a Si-containing compound.
[0007] Preferably, in step (1), the amount ratio of phosphorus pentasulfide, lithium sulfide and lithium chloride in the first raw material is 1:(3-5.5):(1.5-4) in terms of molar ratio.
[0008] Preferably, in step (1), the amount ratio of the first additive to the first raw material is (0.05-0.08):1 in terms of the molar ratio of Se element in the first additive to P element in the first raw material.
[0009] Preferably, in step (1), the calcination temperature is (380-500)℃, and / or the heating rate is (1.5-3)℃ / min, and / or the calcination time is (2-6)h.
[0010] Preferably, in step (2), the amount ratio of the second additive to the second raw material is 1:(10-15) in terms of weight ratio.
[0011] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (2), the metal oxide comprises ZnO, SnO2, CuO, Al2O3, WO3, ZrO, NbO, Cr2O3, TiO2, V2O3, CaO, MgO, SrO, BaO, Cs 11 O3, Rb2O, ScO, YO, Ta2O5, MoO2, MnO and Sb2O3, or a combination of one or more thereof.
[0012] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (2), the calcination temperature is (300-400) ℃, and / or the heating rate is (1.5-3) ℃ / min, and / or the calcination time is (2-6) h.
[0013] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (3), the ratio of the third additive to the third raw material is 1: (10-20) in terms of weight ratio.
[0014] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (3), the Si-containing compound comprises one or more of CaSiO3, Mg3(Si4O 10 )(OH)2, CaSi, MgSi, Na2SiO3 and K2SiO3.
[0015] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (3), the calcination temperature is (380-500) ℃, and / or the heating rate is (1.5-3) ℃ / min, and / or the calcination time is (2-6) h.
[0016] The preparation method of the LPSC sulfide solid electrolyte, preferably, step (1) comprises: a. proportionally liquid-phase star milling the main raw material and the additive; b. sequentially washing, filtering and drying the material obtained in step a; c. calcining the material obtained in step b. The preparation method of the LPSC sulfide solid electrolyte, preferably, preferably, step (1) further comprises grinding the material obtained in step c; preferably, comprising: d. liquid-phase primary grinding the material obtained in step c; e. liquid-phase secondary grinding the material obtained in step d, and sequentially filtering and drying the obtained material to obtain a calcined material.
[0017] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step a, the liquid phase comprises a combination of any one or more of dimethylbenzene, tetrahydrofuran, dimethyl sulfoxide, ethyl propionate, ethyl acetate and octamethylcyclotetrasiloxane.
[0018] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step d, the grinding is terminated when D50 is less than or equal to 3 microns; and / or, In step e, the grinding is terminated when D50 is less than or equal to 1 micron.
[0019] The preparation method of the LPSC sulfide solid electrolyte, preferably, in step (2), when repeating step d in step (1), the grinding is terminated when D50 is less than or equal to 2 microns; and / or, In step (2), when repeating step e in step (1), the grinding is terminated when D50 is less than or equal to 0.8 micron; and / or, In step (3), when repeating step d in step (1), the grinding is terminated when D50 is less than or equal to 2 microns; and / or, In step (3), when repeating step e in step (1), the grinding is terminated when D50 is less than or equal to 0.8 micron.
[0020] To achieve the second object, the application further provides a LPSC sulfide solid electrolyte prepared by the aforementioned preparation method.
[0021] To achieve the third object, the application further provides an application of the aforementioned LPSC sulfide solid electrolyte in a power automobile.
[0022] The application has the following beneficial effects: The preparation method of the LPSC sulfide solid electrolyte of the application introduces Se, Me (metal) and Si elements through reasonable element doping and multi-layer coating process, which strengthens the bond energy between the introduced elements and S elements, further weakens the reaction between S elements and proton H in H2O, and also weakens the side reaction between S elements and positive and negative electrodes, thereby ensuring more excellent electrochemical performance. The prepared LPSC sulfide solid electrolyte can achieve excellent effects of maintaining the ion conductivity at about 95% after being placed in a dry room at-40℃ for 24 hours, and maintaining the ion conductivity at about 90% after being placed in a dry room at-40℃ for 48 hours. The preparation method of the LPSC sulfide solid electrolyte of the application can improve the air stability of the LPSC sulfide solid electrolyte from 50-60% on the market to 95% under the condition of ensuring a certain ion transmission capacity, reasonable element matching, sintering process matching and multi-layer structure optimization, greatly enriches the exposure time of the solid electrolyte to air, reduces the release of H2S, protects personal safety and reduces the processing difficulty of the material battery cell. BRIEF DESCRIPTION OF DRAWINGS
[0023] Figure 1 Figure 1 is a microstructure diagram of LPSC sulfide solid electrolyte A1 obtained by the method of the present application. DETAILED DESCRIPTION
[0024] The technical solutions of the present application and their effects are further described below in conjunction with specific embodiments. The following embodiments are only used to illustrate the content of the present application, and the present application is not limited to the following embodiments or examples. Simple changes to the present application using the concept of the present application are within the scope of the present application.
[0025] The present application provides a method for preparing a LPSC sulfide solid electrolyte, comprising: (1) adding an additive to a main raw material and performing calcination treatment for selenium doping to obtain a first calcined material; wherein, The main raw material is a first raw material; the first raw material comprises phosphorus pentasulfide, lithium sulfide and lithium chloride; The additive is a first additive; the first additive is selenium dioxide; (2) repeating step (1) with a second raw material as the main raw material and a second additive as the additive to perform metal element coating to obtain a second calcined material; wherein, The second raw material is the first calcined material obtained in step (1); The second additive is a metal oxide (abbreviated as MeO); (3) repeating step (1) with a third raw material as the main raw material and a third additive as the additive to perform Si element coating to obtain a third calcined material, i.e. a LPSC sulfide solid electrolyte; wherein, The third raw material is the second calcined material obtained in step (2); The third additive is a Si-containing compound (abbreviated as SiX).
[0026] The method for preparing a LPSC sulfide solid electrolyte of the present application introduces Se, Me (metal) and Si elements through reasonable element doping and multi-layer coating process, and the introduction of Se, Me and Si elements strengthens the bond energy between the introduced elements and S elements, further weakens the reaction between S elements and proton H in H2O, and also weakens the side reaction between S elements and the positive and negative electrodes, ensuring more excellent electrochemical performance; the prepared LPSC sulfide solid electrolyte can achieve excellent effects of maintaining the ion conductivity at about 95% after being placed in a dry room at -40 ℃ for 24 h, and maintaining the ion conductivity at about 90% after being placed in a dry room at -40 ℃ for 48 h.
[0027] In an embodiment, in step (1), the first raw material, the amount ratio of phosphorus pentasulfide, lithium sulfide and lithium chloride is 1: (3-5.5, such as 3, 3.8, 4.5, 5.0 and 5.5 and any value and value range in the range) : (1.5-4, such as 1.5, 2.2, 3.2 and 4 and any value and value range in the range) in terms of molar ratio, so as to adjust the amount ratio of P element in the one-burned material obtained in step (1), improve the effect of inhibiting side reactions, and help improve the air stability of the final obtained three-burned material (i.e. LPSC sulfide solid electrolyte).
[0028] In an embodiment, in step (1), the amount ratio of the first additive to the first raw material is (0.05-0.08):1 in terms of the molar ratio of Se element in the first additive to P element in the first raw material, such as 0.05:1, 0.06:1, 0.07:1 and 0.08:1 and any value and value range in the range, so as to adjust the amount ratio of Se element and P element in the one-burned material obtained in step (1), further improve the bond energy between Se element and S element, weaken side reactions, and help improve the air stability of the final obtained three-burned material (i.e. LPSC sulfide solid electrolyte).
[0029] In an embodiment, in step (1), the calcination temperature is (380-500) ℃, such as 380 ℃, 400 ℃, 450 ℃ and 500 ℃ and any value and value range in the range; and / or the heating rate is (1.5-3) ℃ / min, such as 1.5 ℃ / min, 2 ℃ / min, 2.5 ℃ / min and 3 ℃ / min and any value and value range in the range; and / or the calcination time is (2-6) h, such as 2 h, 4 h and 6 h and any value and value range in the range.
[0030] In an embodiment, in step (1), the calcination treatment is carried out under an inert protective atmosphere, such as nitrogen.
[0031] The present application further sets the calcination conditions in step (1), which helps to further improve the bond energy between Se element and S element in the one-burned material obtained in step (1), weaken side reactions, and thus improve the air stability of the final obtained three-burned material (i.e. LPSC sulfide solid electrolyte).
[0032] In an embodiment, in step (2), the ratio of the amount of the second additive to the second raw material is 1:(10-15) by weight, such as 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, and any number and range of numbers within this range, so as to adjust the addition ratio of the second additive MeO, increase the bond energy between Me element and S element, weaken the side reaction, and thus improve the air stability of the final obtained triple-fired material (i.e., LPSC sulfide solid electrolyte).
[0033] In an embodiment, in step (2), the metal oxide (MeO) comprises ZnO, SnO2, CuO, Al2O3, WO3, ZrO, NbO, Cr2O3, TiO2, V2O3, CaO, MgO, SrO, BaO, Cs 11 O3, Rb2O, ScO, YO, Ta2O5, MoO2, MnO, and Sb2O3, alone or in combination.
[0034] In an embodiment, in step (2), the calcination temperature is (300-400) °C, such as 300 °C, 350 °C, and 400 °C, and any number and range of numbers within this range; and / or the heating rate is (1.5-3) °C / min, such as 1.5 °C / min, 2 °C / min, 2.5 °C / min, and 3 °C / min, and any number and range of numbers within this range; and / or the calcination time is (2-6) h, such as 2 h, 4 h, and 6 h, and any number and range of numbers within this range.
[0035] The present application helps to improve the air stability of the obtained triple-fired material by further setting the calcination conditions in step (2) when repeating step (1).
[0036] In an embodiment, in step (3), the ratio of the amount of the third additive to the third raw material is 1:(10-20) by weight, such as 1:10, 1:12, 1:14, 1:15, 1:18, and 1:20, and any number and range of numbers within this range, so as to adjust the addition ratio of the third additive SiX (sulfur-containing compound), increase the bond energy between Si element and S element, weaken the side reaction, and thus improve the air stability of the final obtained triple-fired material (i.e., LPSC sulfide solid electrolyte).
[0037] In an embodiment, in step (3), the Si-containing compound (abbreviated as SiX) comprises one or more of CaSiO3, Mg3(Si4O 10 )(OH)2, CaSi, MgSi, Na2SiO3, and K2SiO3.
[0038] In an embodiment, in step (3), the calcination temperature is (380-500) °C, such as 380 °C, 400 °C, 450 °C and 500 °C and any value and range of values within this range; and / or the heating rate is (1.5-3) °C / min, such as 1.5 °C / min, 2 °C / min, 2.5 °C / min and 3 °C / min and any value and range of values within this range; and / or the calcination time is (2-6) h, such as 2 h, 4 h and 6 h and any value and range of values within this range.
[0039] In an embodiment, step (1) comprises: a. liquid phase star milling the main raw material with the additive in a ratio; b. sequentially washing, filtering and drying the material obtained in step a; c. calcining the material obtained in step b. In an embodiment, step (1) further comprises grinding the material obtained in step c; preferably comprising: d. liquid phase primary grinding of the material obtained in step c; e. liquid phase secondary grinding of the material obtained in step d, and sequentially filtering and drying the material obtained to obtain a calcined material.
[0040] In an embodiment, in step a, the liquid phase comprises any one or more of a combination of xylene, tetrahydrofuran, dimethyl sulfoxide, ethyl propionate, ethyl acetate and octamethylcyclotetrasiloxane.
[0041] In an embodiment, in step d, the grinding is terminated when D50≤3 pm; preferably the grinding time is (1-2) h, such as 1 h, 1.5 h and 2 h and any value and range of values within this range.
[0042] In an embodiment, in step e, the grinding is terminated when D50≤1 pm; preferably the grinding time is (2-4) h, such as 2 h, 2.5 h, 3 h and 4 h and any value and range of values within this range.
[0043] In an embodiment, in step d, the Zr beads used in the grinding have a size of (4-8) mm, such as 4 mm, 6 mm and 8 mm and any value and range of values within this range.
[0044] In an embodiment, in step e, the Zr beads used in the grinding have a size of (1-3) mm, such as 1 mm, 2 mm and 3 mm and any value and range of values within this range.
[0045] In one embodiment, in step (2), the grinding is terminated when D50≤2 μm upon repeating step d in step (1).
[0046] In one embodiment, in step (2), the grinding is terminated when D50≤0.8 μm upon repeating step e in step (1).
[0047] In one embodiment, in step (3), the grinding is terminated when D50≤2 μm upon repeating step d in step (1).
[0048] In one embodiment, in step (3), the grinding is terminated when D50≤0.8 μm upon repeating step e in step (1).
[0049] In the present application, washing, filtering and drying are common means in the art and will not be described here.
[0050] In the present application, the preparation method of the LPSC sulfide solid electrolyte introduces Se, Me and Si elements through reasonable element doping and multi-layer coating process. The introduction of Se, Me and Si elements strengthens the bond energy between the introduced elements and S elements, further weakens the reaction between S elements and proton H in H2O, and also weakens the side reaction between S elements and the positive and negative electrodes, ensuring more excellent electrochemical performance. The prepared LPSC sulfide solid electrolyte can achieve excellent effects of maintaining the ion conductivity at about 95 % after being placed in a dry room at -40 ℃ for 24 h, and maintaining the ion conductivity at about 90 % after being placed in a dry room at -40 ℃ for 48 h. Specifically, By liquid phase star milling, calcining and two-stage grinding (coarse grinding and fine grinding) of the precursors phosphorus pentasulfide, lithium sulfide, lithium chloride and the first additive in a certain proportion, the activity of S elements is weakened by the bond energy between Se elements and S elements, so that a burned material with certain side reaction inhibition effect is obtained. By repeating the calcining and coating MeO treatment, the activity of S elements is further weakened by the bond energy between Me elements and S elements by using the substitution relationship between metal Me elements and P elements, so as to further improve the air stability of the obtained LPSC sulfide solid electrolyte. The two-stage grinding (coarse grinding and fine grinding) process obtains fine powder of 200-300 nm to ensure the uniformity of the positive electrode coating, so as to inhibit polarization to a weak state, so that the obtained LPSC sulfide solid electrolyte has the ability of inhibiting side reaction, inhibiting polarization and high air stability. By repeating the calcining and coating SiX treatment, the activity of S elements is further weakened by the bond energy between Si elements and S elements, so as to further improve the air stability of the obtained LPSC sulfide solid electrolyte.
[0051] The present application also provides a LPSC sulfide solid electrolyte prepared according to the above preparation method.
[0052] The application also provides application of the aforementioned LPSC sulfide solid electrolyte in a power automobile.
[0053] The LPSC sulfide solid electrolyte obtained by the application has low side reactions and good air stability.
[0054] The application is further illustrated below by specific examples and comparative examples.
[0055] The raw materials used in the following examples and comparative examples are as follows: Unless otherwise specified, the raw materials used are all of analytical purity, and the manufacturer is Macklin.
[0056] The test method is as follows.
[0057] 1. Ion conductivity characterization 0.2 g of the LPSC sulfide solid electrolyte sample obtained by the application is placed in a battery mold for cold pressing to obtain an electrolyte sheet, wherein the pressure applied during the cold pressing process is maintained at 320 Mpa; an ion blocking battery is assembled in the order of a stainless steel sheet, an electrolyte sheet, and a stainless steel sheet; the ion conductivity of the LPSC sulfide solid electrolyte sample is evaluated by testing the electrochemical impedance spectrum of the obtained ion blocking battery. The calculation formula of the ion conductivity is as follows: ; wherein, σ represents the ion conductivity of the LPSC sulfide solid electrolyte sample, L is the thickness of the electrolyte sheet, S is the surface area of the electrolyte sheet, and R is the resistance of the electrolyte sheet.
[0058] 2. Young's modulus test 0.5 g of the LPSC sulfide solid electrolyte sample obtained by the application is pressed into a regular sheet, and the geometric parameters of the obtained sample sheet, including length, cross-sectional size, and mass, are measured. The sample sheet is made to produce longitudinal resonance by vibration excitation. Resonance frequency data are collected, and the geometric parameters and density of the sample sheet are combined to calculate the Young's modulus using the following formula: ; wherein, L is the length, d is the diameter, p is the density, f is the resonance frequency, and m and n are vibration modal coefficients.
[0059] 3. Ion conductivity retention performance test The LPSC sulfide solid electrolyte sample (powder) obtained by the application is laid flat and placed in a sealed cover for exposure, and its ion conductivity is tested at two time nodes of 24 h and 48 h, respectively, so as to calculate its retention rate.
[0060] 4. H2S gas release detection The LPSC sulfide solid electrolyte sample (powder) obtained in the application is laid in a sealed cover for exposure, and the H2S gas content in the cover is detected and the value is read at two time nodes of 24 h and 48 h respectively by using a H2S gas detector.
[0061] Example 1 (S1) LPSC sulfide solid electrolyte A1 is prepared according to the preparation method of the LPSC sulfide solid electrolyte in the application; the preparation method comprises: (1) a, liquid phase star milling of the main raw material and the additive according to the proportion; wherein, the main raw material is the first raw material; the first raw material comprises phosphorus pentasulfide, lithium sulfide and lithium chloride; the additive is the first additive; the first additive is selenium dioxide; the liquid phase is ethyl acetate; In the first raw material, the amount ratio of phosphorus pentasulfide, lithium sulfide and lithium chloride is 1:5:2 according to the molar ratio; The amount ratio of the first additive to the first raw material is 0.05:1 according to the molar ratio of Se element in the first additive to P element in the first raw material; b, the material obtained in step a is sequentially washed, filtered and dried; c, the material obtained in step b is calcined under inert protective atmosphere; wherein, the inert protective gas is nitrogen; the calcination temperature is 500 ℃, the heating rate is 2 ℃ / min, and the calcination time is 5 h; d, the material obtained in step c is subjected to liquid phase primary grinding, and the grinding is terminated when D50≤3 μm; e, the material obtained in step d is subjected to liquid phase secondary grinding, and the grinding is terminated when D50≤1 μm, and the obtained material is sequentially filtered and dried to obtain a calcined material; (2) repeating steps a-e in step (1) by taking the second raw material as the main raw material and the second additive as the additive, and sequentially filtering and drying the obtained material to obtain a second calcined material; wherein, the second raw material is the first calcined material obtained in step (1); the second additive is MeO, and the MeO is ZnO; The amount ratio of the second additive to the second raw material is 1:10 according to the weight ratio; the calcination temperature is 350 ℃, the heating rate is 2 ℃ / min, and the calcination time is 5 h; When step d in step (1) is repeated, the grinding is terminated when D50≤2 μm; When repeating step e in step (1), the grinding is terminated when D50≤0.8 μm; (3), repeating steps a-e with the third raw material as the main raw material and the third additive as the additive, and sequentially filtering and drying the obtained material to obtain a third-burned material, i.e., an LPSC sulfide solid-state electrolyte; wherein, the third raw material is the second-burned material obtained in step (2); the third additive is SiX, and the SiX is CaSiO3; the ratio by weight of the third additive to the third raw material is 1:10; When repeating step d in step (1), the grinding is terminated when D50≤2 μm; When repeating step e in step (1), the grinding is terminated when D50≤0.8 μm.
[0062] The microstructure of the obtained LPSC sulfide solid-state electrolyte A1 is shown in Figure 1 .
[0063] Example 2 (S2) The LPSC sulfide solid-state electrolyte A2 is prepared according to the preparation method of Example 1; the only difference between the two is that: in step (1), the ratio by mole of Se in the first additive to P in the first raw material is 0.08:1; the calcination temperature is 450 ℃; in step (2), the second additive is MeO, and the MeO is Cr2O3; the ratio by weight of the second additive to the second raw material is 1:15; the calcination temperature is 380 ℃; in step (3), the third additive is SiX, and the SiX is Mg3(Si4O 10 )(OH)2; the ratio by weight of the third additive to the third raw material is 1:15.
[0064] Example 3 (S3) The LPSC sulfide solid-state electrolyte A3 is prepared according to the preparation method of Example 1; the only difference between the two is that: in step (1), the ratio by mole of Se in the first additive to P in the first raw material is 0.06:1; the calcination temperature is 460 ℃; In step (2), The second additive is MeO, and the MeO is Al2O3; The ratio by weight of the second additive to the second raw material is 1:12; The calcination temperature is 330 °C; In step (3), The third additive is SiX, and the SiX is CaSi; The ratio by weight of the third additive to the third raw material is 1:17.
[0065] Example 4 (S4) LPSC sulfide solid electrolyte A4 is prepared according to the preparation method of Example 1; the only difference between Example 4 and Example 1 is that: In step (1), The ratio by weight of the first additive to the first raw material is 0.07:1 in terms of the molar ratio of Se in the first additive to P in the first raw material; The calcination temperature is 480 °C; In step (2), The second additive is MeO, and the MeO is TiO2; The calcination temperature is 380 °C; In step (3), The third additive is SiX, and the SiX is K2SiO3; The ratio by weight of the third additive to the third raw material is 1:18.
[0066] Example 5 (S5) LPSC sulfide solid electrolyte A5 is prepared according to the preparation method of Example 1; the only difference between Example 5 and Example 1 is that: In step (1), the ratio by weight of the first additive to the first raw material is 0.08:1 in terms of the molar ratio of Se in the first additive to P in the first raw material; In step (2), The second additive is MeO, and the MeO includes CaO and MgO, and the mass ratio of CaO to MgO is 1:1; The calcination temperature is 400 °C; In step (3), The third additive is SiX, and the SiX includes CaSiO3 and Na2SiO3, and the mass ratio of CaSiO3 to Na2SiO3 is 1:1; The ratio by weight of the third additive to the third raw material is 1:12.
[0067] Example 6 (S6) The LPSC sulfide solid electrolyte A6 was prepared according to the preparation method of Example 1; the only difference between the two is that: In step (1), the calcination temperature was 460 ℃; In step (2), The second additive was MeO, which included SnO2 and V2O3, and the mass ratio of SnO2 and V2O3 was 1:1; The ratio of the amount of the second additive to the second raw material was 1:13 by weight; The calcination temperature was 360 ℃; In step (3), The third additive was SiX, which included CaSi and MgSi, and the mass ratio of CaSi and MgSi was 1:1; The ratio of the amount of the third additive to the third raw material was 1:15 by weight.
[0068] Example 7 (S7) The LPSC sulfide solid electrolyte A7 was prepared according to the preparation method of Example 1; the only difference between the two is that: In step (1), The ratio of the amount of the first additive to the first raw material was 0.08:1 by molar ratio of Se in the first additive to P in the first raw material; The calcination temperature was 420 ℃; In step (2), The second additive was MeO, which included TiO2, YO and Ta2O5, and the mass ratio of TiO2, YO and Ta2O5 was 1:1:1; The calcination temperature was 400 ℃; In step (3), The third additive was SiX, which included CaSiO3, CaSi and MgSi, and the mass ratio of CaSiO3, CaSi and MgSi was 1:1:1.
[0069] Example 8 (S8) The LPSC sulfide solid electrolyte A8 was prepared according to the preparation method of Example 1; the only difference between the two is that: In step (1), The ratio of the amount of the first additive to the first raw material was 0.08:1 by molar ratio of Se in the first additive to P in the first raw material; The calcination temperature was 470 ℃; In step (2), The second additive is MeO, the MeO includes ZnO, SnO2, CuO and Al2O3, and the mass ratio of ZnO, SnO2, CuO and Al2O3 is 1:1:1:1; The calcination temperature is 390 ℃; In step (3), The third additive is SiX, the SiX includes CaSiO3, CaSi, MgSi and Na2SiO3, and the mass ratio of CaSiO3, CaSi, MgSi and Na2SiO3 is 1:1:1.
[0070] Example 9 (S9) The LPSC sulfide solid electrolyte A9 is prepared according to the preparation method of Example 1; the difference between Example 1 and Example 9 is only that: In step (1), The dosage ratio of the first additive to the first raw material is 0.08:1 according to the molar ratio of Se element in the first additive to P element in the first raw material; The calcination temperature is 460 ℃; In step (2), The second additive is MeO, the MeO is Al2O3; The dosage ratio of the second additive to the second raw material is 1:15 according to the weight ratio; The calcination temperature is 380 ℃; In step (3), The third raw material is the second calcined material obtained in step (2); The third additive is SiX, the SiX is CaSi; The dosage ratio of the third additive to the third raw material is 1:15 according to the weight ratio.
[0071] Example 10 (S10) The LPSC sulfide solid electrolyte A10 is prepared according to the preparation method of Example 1; the difference between Example 1 and Example 10 is only that: In step (1), The dosage ratio of the first additive to the first raw material is 0.08:1 according to the molar ratio of Se element in the first additive to P element in the first raw material; The calcination temperature is 400 ℃; In step (2), The second additive is MeO, the MeO includes CaO and MgO, and the mass ratio of CaO and MgO is 1:1; The calcination temperature is 360 ℃; In step (3), The dosage ratio of the third additive to the third raw material is 1:12 according to the weight ratio.
[0072] Example 11 (S11) The LPSC sulfide solid electrolyte A11 was prepared according to the preparation method of Example 1; the only difference between Example 1 and Example 11 is that: In step (1), The ratio of the amount of the first additive to the amount of the first raw material is 0.08:1 according to the molar ratio of Se element in the first additive to P element in the first raw material; The calcination temperature is 420 ℃; In step (2), The second additive is MeO, the MeO includes TiO2, Cr2O3 and SnO2, and the mass ratio of TiO2, Cr2O3 and SnO2 is 1:1:1; The calcination temperature is 400 ℃; In step (3), The third additive is SiX, the SiX includes CaSiO3, Na2SiO3 and K2SiO3, and the mass ratio of CaSiO3, Na2SiO3 and K2SiO3 is 1:1:1.
[0073] Example 12 (S12) The LPSC sulfide solid electrolyte A12 was prepared according to the preparation method of Example 1; the only difference between Example 1 and Example 12 is that: In step (1), In the first raw material, the ratio of the amount of phosphorus pentasulfide, lithium sulfide and lithium chloride is 1:3:4 according to the molar ratio; the liquid phase is tetrahydrofuran; The calcination temperature is 500 ℃, the heating rate is 1.5 ℃ / min, and the calcination time is 6 h; In step (2), The second additive is MeO, the MeO includes Cs 11 O3 and Rb2O, and the mass ratio of Cs 11 O3 and Rb2O is 1:2; In step (3), The third additive is SiX, the SiX includes K2SiO3 and CaSi, and the mass ratio of K2SiO3 and CaSi is 2:1; The ratio of the amount of the third additive to the amount of the third raw material is 1:20 according to the weight ratio.
[0074] Example 13 (S13) The LPSC sulfide solid electrolyte A13 was prepared according to the preparation method of Example 1; the only difference between Example 1 and Example 13 is that: In step (1), the amount ratio of phosphorus pentasulfide, lithium sulfide and lithium chloride in the first raw material is 1:5.5:1.5 in terms of molar ratio; the liquid phase is octamethylcyclotetrasiloxane; In step (1), the calcination temperature is 500 ℃, the heating rate is 3 ℃ / min, and the calcination time is 2 h.
[0075] Comparative Example 1 (D1) LPSC sulfide solid electrolyte A1’ was prepared according to the preparation method of Example 1; the only difference between it and Example 1 is that: Only step (1) was performed, and steps (2) and (3) were not performed; and in step e of step (1), the grinding was terminated when D50≤0.8 μm; The obtained calcined material is LPSC sulfide solid electrolyte A1’.
[0076] Comparative Example 2 (D2) LPSC sulfide solid electrolyte A2’ was prepared according to the preparation method of Example 1; the only difference between it and Example 1 is that: Only steps (1) and (2) were performed, and step (3) was not performed; The obtained two calcined materials are LPSC sulfide solid electrolyte A2’.
[0077] Comparative Example 3 (D3) LPSC sulfide solid electrolyte A3’ was prepared according to the preparation method of Example 1; the only difference between it and Example 1 is that: In step (1), the calcination temperature is 460 ℃; In step (2), The second additive is SiX, the SiX includes CaSi and MgSi, and the mass ratio of CaSi and MgSi is 1:1; The amount ratio of the second additive to the second raw material is 1:13 in terms of weight ratio; The calcination temperature is 360 ℃; In step g, The third raw material is the two calcined materials obtained in step (2); The third additive is MeO, the MeO includes SnO2 and V2O3, and the mass ratio of SnO2 and V2O3 is 1:1; The amount ratio of the third additive to the third raw material is 1:15 in terms of weight ratio.
[0078] The performance test is as follows.
[0079] 1、According to the ion conductivity characterization method and Young's modulus test method, the initial ion conductivity and Young's modulus of the LPSC sulfide solid electrolyte A1-13 and A1'-3' obtained from Examples 1-13 and Comparative Examples 1-3 are tested, and the results are shown in Table 1.
[0080] Table 1: Test results of related properties of LPSC sulfide solid electrolyte A1-13 and A1'-3'
[0081] 2、According to the ion conductivity retention performance test method, the ion conductivity of the LPSC sulfide solid electrolyte A1-13 and A1'-3' obtained from Examples 1-13 and Comparative Examples 1-3 at the time nodes of 24 h and 48 h in the sealed cover is tested, and the retention rate is calculated, and the results are shown in Table 2.
[0082] Table 2: Ion conductivity retention rate of LPSC sulfide solid electrolyte A1-13 and A1'-3'
[0083] 3、According to the H2S gas release detection method, the release amount of H2S gas in the sealed cover of the LPSC sulfide solid electrolyte A1-13 and A1'-3' obtained from Examples 1-13 and Comparative Examples 1-3 at the time nodes of 24 h and 48 h in the sealed cover is detected, and the results are shown in Table 3.
[0084] Table 3: H2S release detection results of LPSC sulfide solid electrolyte A1-13 and A1'-3'
[0085] According to the comparison of Examples 1-13 and Comparative Examples 1-2 and Tables 1-3, the preparation method of the application can obtain LPSC sulfide solid electrolyte with high ion conductivity and high stability by doping Se, Me and Si elements and setting different coating processes, and the ion conductivity retention rate is high.
[0086] According to the comparison of Examples 1-13 and Comparative Examples 1-2 and Tables 1-3, the one-shot doped Se element obtained from one-shot material (LPSC sulfide solid electrolyte A1') has an ion conductivity retention rate of 68% and 55% after exposure for 24 h and 48 h, respectively, and the release amount of H2S gas is 0.79 g / cm 3 and 1.32 g / cm 3; the ion conductivity retention rate of the second-burned doped metal element material (LPSC sulfide solid-state electrolyte A2') exposed for 24 h and 48 h was increased to 80% and 63%, respectively, and the H2S gas release amount was 0.67 g / cm 3 and 1.10 g / cm 3 , respectively. The importance of the second burn coating was obvious. The ion conductivity retention rate of the third-burned doped Si element material (LPSC sulfide solid-state electrolyte A1) exposed for 24 h and 48 h was increased to 94% and 92%, respectively, and the H2S gas release amount was 0.28 g / cm3 and 0.33 g / cm3, respectively. The importance of the third burn coating was obvious.
[0087] According to the comparison of Example 6 and Comparative Example 3 and Tables 1-3, when the processing sequence of MeO (SnO2, V2O3) and SiX (CaSi, MgSi) was reversed, the air stability changed greatly. When the metal oxide MeO was used as the second additive in the second burn, the ion conductivity of the product was large. When the Si-containing compound SiX was used as the second additive in the second burn, the air stability was more excellent.
[0088] According to the comparison of Example 7 and Example 11 and Tables 1-3, when a plurality of different compounds were used as additives, the product had very excellent air stability.
[0089] Compared with Comparative Examples 1 and 2, the H2S gas release amount of the LPSC sulfide solid-state electrolyte product prepared in Examples 1-13 was significantly reduced, the ion conductivity retention rate was greatly improved, and the air stability was excellent, which provided a new way for industrial development.
[0090] Although the content of the present application has been described in detail, it should be recognized that the above description should not be considered as limiting the present application. Those skilled in the art can understand that, under the guidance of the present application, some modifications and adjustments can be made to the present application. These modifications and adjustments should also be within the scope defined by the claims of the present application.
Claims
1. A method for preparing an LPSC sulfide solid electrolyte, characterized in that, The manufacturing method includes: (1) Adding additives to the main raw material and calcining it to dope it with selenium, thereby obtaining a calcined material; wherein, The main raw material is the first raw material; the first raw material includes phosphorus pentasulfide, lithium sulfide and lithium chloride; The additive is a first additive; the first additive is selenium dioxide; (2) Using the second raw material as the main raw material and the second additive as the additive, step (1) is repeated to coat the metal elements, thereby obtaining a second sintered material; wherein, The second raw material is the sintering material obtained in step (1); The second additive is a metal oxide; (3) Using the third raw material as the main raw material and the third additive as the additive, step (1) is repeated to coat Si element to obtain a three-stage sintered material, namely LPSC sulfide solid electrolyte; wherein, The third raw material is the second batch of sintered material obtained in step (2); The third additive is a Si-containing compound.
2. The manufacturing method according to claim 1, characterized in that, In step (1), the molar ratio of phosphorus pentasulfide, lithium sulfide, and lithium chloride in the first raw material is 1:(3-5.5):(1.5-4); and / or, In step (1), the ratio of the first additive to the first raw material is calculated as (0.05-0.08):1 based on the molar ratio of Se element in the first additive to P element in the first raw material; and / or, In step (1), the calcination temperature is (380-500)℃, and / or the heating rate is (1.5-3)℃ / min, and / or the calcination time is (2-6)h.
3. The manufacturing method according to claim 1 or 2, characterized in that, In step (2), the ratio of the second additive to the second raw material is 1:(10-15) by weight; and / or, In step (2), the metal oxides include ZnO, SnO2, CuO, Al2O3, WO3, ZrO, NbO, Cr2O3, TiO2, V2O3, CaO, MgO, SrO, BaO, and Cs. 11 Any one or more combinations of O3, Rb2O, ScO, YO, Ta2O5, MoO2, MnO and Sb2O3; In step (2), the calcination temperature is (300-400)℃, and / or the heating rate is (1.5-3)℃ / min, and / or the calcination time is (2-6)h.
4. The manufacturing method according to any one of claims 1-3, characterized in that, In step (3), the ratio of the third additive to the third raw material is 1:(10-20) by weight; and / or, In step (3), the Si-containing compound includes CaSiO3 and Mg3(Si4O3). 10 (OH)2, CaSi, MgSi, Na2SiO3, and K2SiO3, or one or more of these; and / or, In step (3), the calcination temperature is (380-500)℃, and / or the heating rate is (1.5-3)℃ / min, and / or the calcination time is (2-6)h.
5. The manufacturing method according to any one of claims 1-4, characterized in that, Step (1) includes: a. The main raw materials and additives are subjected to liquid-phase star ball milling in proportion; b. The material obtained in step a is washed, filtered and dried in sequence; c. Calcine the material obtained in step b. Preferably, step (1) further includes grinding the material obtained in step c; preferably, it includes: d. Perform liquid-phase primary grinding on the material obtained in step c; e. The material obtained in step d is subjected to liquid phase two-stage grinding, and the resulting material is filtered and dried in sequence to obtain a burnt material.
6. The manufacturing method according to claim 5, characterized in that, In step a, the liquid phase includes any one or a combination of xylene, tetrahydrofuran, dimethyl sulfoxide, ethyl propionate, ethyl acetate, and octamethylcyclotetrasiloxane.
7. The manufacturing method according to claim 5 or 6, characterized in that, In step d, grinding is terminated when D50 ≤ 3 μm; and / or, In step e, grinding is terminated when D50 ≤ 1 μm.
8. The manufacturing method according to any one of claims 5-7, characterized in that, In step (2), when repeating step d in step (1), grinding is terminated when D50 ≤ 2 μm; and / or, In step (2), when repeating step e in step (1), grinding is terminated when D50 ≤ 0.8 μm; and / or, In step (3), when repeating step d in step (1), grinding is terminated when D50 ≤ 2 μm; and / or, In step (3), when step e in step (1) is repeated, grinding is terminated when D50 ≤ 0.8 μm.
9. An LPSC sulfide solid electrolyte prepared by any one of claims 1-8.
10. The application of the LPSC sulfide solid electrolyte according to claim 9 in a powered vehicle.