TiB2 reinforced aluminum-based composite powder, preparation method and application thereof and TiB2 reinforced aluminum-based composite material
By combining EIGA technology with a specific aluminum alloy formulation, uniform dispersion and high cleanliness of TiB2 particles in aluminum-based composite powder are achieved, solving the problem of uneven particle dispersion in TiB2-reinforced aluminum-based composite materials, improving the overall performance of the material, and making it suitable for aerospace and rail transportation fields.
Patent Information
- Application Number
- CN202511382716.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-25
- Publication Date
- 2026-01-06
AI Technical Summary
In existing technologies, the TiB2-reinforced aluminum matrix composite powder has poor dispersion uniformity of TiB2-reinforced particles, making it difficult to prepare TiB2-reinforced aluminum matrix composites with superior mechanical properties.
EIGA technology was used to achieve gas atomization co-deposition of nano-sized TiB2 particles and aluminum alloy droplets at the powder preparation source. By optimizing atomization parameters and feeding methods, uniform particle dispersion and high material purity were ensured. Combined with a specific 7xxx series aluminum alloy formulation and heat treatment process, high-performance TiB2-reinforced aluminum-based composite powder was prepared.
It significantly improves the sphericity and particle uniformity of composite powders, reduces agglomeration and interface defects, and enhances the strength, elastic modulus and plasticity of materials, meeting the high-strength and high-modulus material requirements of aerospace and rail transportation.
Smart Images

Figure CN121272272A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal matrix composites, and more specifically, to a TiB2-reinforced aluminum matrix composite powder, its preparation method and application, and TiB2-reinforced aluminum matrix composites. Background Technology
[0002] Al-Zn-Mg-Cu series (7xxx series) aluminum alloys are characterized by their low density (approximately 2.8 g / cm³). 3 With its high specific strength (tensile strength > 500 MPa) and excellent processing performance, aluminum alloy has become a key structural material in aerospace, rail transportation, and other fields. As high-end equipment demands increasingly lightweight, high-rigidity, and high-load-bearing capacity materials, the elastic modulus of traditional aluminum alloys (approximately 70 GPa) is insufficient to meet the design requirements of next-generation structural components, necessitating breakthroughs in performance bottlenecks through composite strengthening technologies. To compensate for insufficient matrix modulus, introducing high-modulus ceramic particles such as TiB2, SiC, and TiC into aluminum alloys to construct particle-reinforced aluminum matrix composites (AMCs) has become an important path to improve overall performance, significantly increasing modulus while maintaining strength, thus meeting the growing demand for high-strength, high-modulus materials in aerospace and rail transportation.
[0003] Among various reinforcements, TiB2 particles are considered ideal due to their high melting point (>2900℃), high elastic modulus (approximately 400 GPa), and good interfacial compatibility with the aluminum matrix. Stir casting and powder metallurgy are common methods for preparing aluminum matrix composites; however, traditional techniques still have many drawbacks. Stir casting introduces TiB2 particles into the molten aluminum alloy through mechanical stirring, but nano-sized TiB2 particles are prone to agglomeration due to van der Waals forces, and particles in the melt are easily pushed to grain boundaries by the solid-liquid interface front, resulting in uneven distribution. Furthermore, insufficient wettability between the aluminum alloy melt and TiB2 can easily induce interfacial porosity, reducing load transfer efficiency. Powder metallurgy uses mechanical ball milling to mix TiB2 powder with aluminum alloy powder, but high-energy ball milling easily leads to cold welding agglomeration of nano-TiB2 particles, forming microcrack sources during subsequent sintering, restricting the dynamic load-bearing capacity of the material. Moreover, the mixing process easily introduces oxygen impurities, impairing the material's plasticity.
[0004] To overcome the aforementioned problems, gas atomization, due to its rapid solidification characteristics, can refine particles and reduce segregation, producing composite powders with high sphericity and uniform composition, making it the mainstream technology for preparing high-performance composite powders. However, existing processes still have shortcomings. In the VIGA (vacuum induction melting gas atomization) process, particle agglomeration and slagging, as well as sedimentation, can easily occur in the melt transport / nozzle front section, leading to loss and limiting the content of reinforcing agents in the powder. While PREP (plasma rotating electrode atomization) can obtain powders with high sphericity, its yield in the target fine powder range is limited, particle size distribution is affected by process parameters, and it requires the prior preparation of high-quality electrodes, resulting in a long process and high cost. In contrast, EIGA (crucibleless electrode induction melting gas atomization) directly melts a solid electrode inside the induction coil without a crucible. The melt flow is instantaneously broken into droplets by an inert gas flow at the nozzle, resulting in fewer process steps, higher metal cleanliness, and better suppression of reinforcing particle sedimentation and secondary contamination in the composite melt. Therefore, it has attracted attention in the field of composite powder preparation.
[0005] However, although EIGA technology can achieve instant mixing and deposition of particles and melt at the source, nanoscale reinforcing particles can still agglomerate under high-speed gas flow, especially in the early stages of gas atomization. Particle agglomeration can reduce the performance of composite materials because the interfacial effects within the agglomerates weaken the reinforcing effect of the particles. Simultaneously, during co-deposition, poor contact between reinforcing particles and the melt, leading to porosity and interfacial defects, can severely affect load transfer efficiency and the mechanical properties of the material. In EIGA technology, particles and molten droplets meet at high speeds; ensuring good contact conditions between them to promote composite formation is a major challenge in technology optimization.
[0006] Therefore, how to provide a particle-reinforced aluminum-based composite powder based on EIGA technology, so that it has good mechanical properties after sintering and hot pressing, is an important technical problem that needs to be solved in this field. Summary of the Invention
[0007] The main objective of this invention is to provide a TiB2-reinforced aluminum-based composite powder, its preparation method and application, and a TiB2-reinforced aluminum-based composite material, in order to solve the problem that in the existing TiB2-reinforced aluminum-based composite powder, it is difficult to obtain a TiB2-reinforced aluminum-based composite material with superior mechanical properties due to the poor dispersion uniformity of TiB2 reinforcing particles.
[0008] To achieve the above objectives, a first aspect of the present invention provides a method for preparing TiB2-reinforced aluminum-based composite powder, comprising: step S1, preparing a 7xxx series aluminum alloy into a rod-shaped electrode; the 7xxx series aluminum alloy comprises, by weight percentage, 8 wt.% to 10 wt.% Zn, 2.1 wt.% to 2.9 wt.% Mg, 1.5 wt.% to 2.5 wt.% Cu, 0.1 wt.% to 0.2 wt.% Zr, with the balance being Al and unavoidable impurities; step S2, atomizing the rod-shaped electrode into an aluminum-based composite powder using an electrode induction melting gas atomization method. The liquid flow is mixed with TiB2 powder to co-deposit 7xxx series aluminum alloy and TiB2 powder to obtain TiB2-reinforced aluminum-based composite powder; the atomization pressure is 2.0MPa~5.0MPa, the atomization power is 30kW~40kW, the feed rate of the rod electrode is 15mm / min~20mm / min, and the powder feeding rate of TiB2 powder is 10g / min~15g / min; the total feed amount of TiB2 powder is 8%~10% based on the total weight of TiB2-reinforced aluminum-based composite powder as 100%; the particle size of TiB2 powder is in the nanometer range.
[0009] Further, step S2 also includes: step S2-1, clamping the rod-shaped electrode onto the electrode fixture, activating induction heating to melt the end of the rod-shaped electrode and form a droplet; under the action of the inert gas jet, the droplet atomizes to form an aluminum matrix liquid flow with a cone-shaped spray direction; step S2-2, simultaneously with the droplet atomization, activating the feeder filled with TiB2 powder, and using a carrier gas to allow the TiB2 powder to contact and mix with the aluminum matrix liquid flow in the form of a TiB2 powder flow, forming a composite liquid flow; step S2-3, the composite liquid flow solidifies to achieve co-deposition, thereby obtaining... The TiB2-reinforced aluminum-based composite powder is fed into the atomization chamber in a radial direction perpendicular to the jet axis of the inert gas, and comes into contact with and mixes with the aluminum matrix liquid flow at the junction point; the vertical distance between the junction point and the axis of the aluminum matrix liquid flow is 10 mm to 15 mm; more preferably, in step S2-1, the feed rate of the rod electrode is 18 ± 1 mm / min, the atomization pressure is 3.5 ± 0.2 MPa, and the atomization power is 35 ± 2 kW; and / or, in step S2-2, the powder feeding rate of TiB2 powder is 12 ± 1 g / min.
[0010] Furthermore, in step S2-1, the flow rate of the inert gas is 1000 m³ / h. 3 / h~1500m 3 / h, preferably 1300±50m 3 / h; and / or, in step S2-2, the particle size of the TiB2 powder is 50nm to 100nm.
[0011] Further, in step S1-1, 7xxx series aluminum alloy is melted at 710-760℃ to obtain a first melt; in step S1-2, the first melt is refined and degassed at 710-730℃ for 0.5 min-1 min to obtain a second melt; in step S1-3, Al-Ti-B refining agent is added to the second melt, and the melt is subjected to stirring and settling treatment in sequence to obtain a third melt; the third melt is cast to obtain a rod-shaped electrode; preferably, the amount of Al-Ti-B refining agent added is 2‰-5‰ based on 100% of the total weight of the first melt; more preferably, in step S1-3, the stirring treatment time is 2 min-5 min.
[0012] A second aspect of the present invention provides a TiB2-reinforced aluminum-based composite powder, which is prepared by the above-described method for preparing TiB2-reinforced aluminum-based composite powder.
[0013] A third aspect of the present invention provides a TiB2-reinforced aluminum matrix composite material, which is obtained by sequentially subjecting the above-mentioned TiB2-reinforced aluminum matrix composite powder to sintering, molding, and heat treatment; the TiB2-reinforced aluminum matrix composite material includes an aluminum alloy matrix and TiB2 particles dispersed in the aluminum alloy matrix; preferably, the content of TiB2 particles is 8wt% to 10wt% based on 100% of the total weight of the TiB2-reinforced aluminum matrix composite material; more preferably, the tensile strength of the TiB2-reinforced aluminum matrix composite material is 740MPa to 810MPa, the yield strength is 670MPa to 740MPa, and the elastic modulus is 86GPa to 90GPa.
[0014] Further, the sintering process includes: placing TiB2-reinforced aluminum-based composite powder in a mold, heating it to a holding temperature, and holding it at the holding temperature to obtain a sintered billet; the holding temperature is 540℃~580℃; the axial pressure of the holding process is 30±2MPa, and the holding time is 60min~150min; preferably, the holding temperature is 560±5℃, and the holding time is 120±10min; more preferably, the heating rate of the heating process is 10±2℃ / min.
[0015] Furthermore, the forming process is carried out by hot extrusion; the extrusion ratio of hot extrusion is (10-20):1, and the hot extrusion is carried out at 430°C-470°C; preferably, the extrusion ratio of hot extrusion is (15-17):1, and the hot extrusion is carried out at 450±5°C; more preferably, the extrusion speed of hot extrusion is 0.5±0.05mm / s.
[0016] Further, the heat treatment includes a solution heat treatment and an aging heat treatment performed sequentially; the solution heat treatment temperature is 460℃~480℃, and the holding time is 1.5h~3h; the aging heat treatment temperature is 110℃~140℃, and the holding time is 18h~30h; preferably, the solution heat treatment temperature is 470±5℃, and the holding time is 2±0.2h; and / or, the aging heat treatment temperature is 120±5℃, and the holding time is 24±2h.
[0017] A fourth aspect of the present invention provides an application of the above-mentioned TiB2 reinforced aluminum-based composite powder as a powder raw material for structural components in the fields of aerospace, rail transportation and electronic devices.
[0018] By applying the technical solution of this invention, based on crucibleless electrode induction melting gas atomization (EIGA), the co-deposition of nano-sized TiB2 particles and aluminum alloy droplets through gas atomization at the powder preparation source achieves the goals of uniform dispersion of the reinforcing phase and high material purity. Simultaneously, it overcomes problems such as particle agglomeration, insufficient interfacial wettability, and melt contamination in traditional preparation methods. By optimizing atomization parameters, a multi-scale synergistic strengthening structure of the η′ / GP region precipitated phase, TiB2 particles, and dislocations is effectively constructed, significantly enhancing the comprehensive performance of the powder material. This results in a synergistic improvement in strength and elastic modulus after subsequent sintering and hot pressing. Attached Figure Description
[0019] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:
[0020] Figure 1 The scanning electron microscope (SEM) characterization results of the TiB2-reinforced aluminum-based composite powder obtained in Example 1 are shown below.
[0021] Figure 2 The image shows the cross-sectional SEM characterization results of the sintered billet of the TiB2-reinforced aluminum matrix composite material obtained in Example 1.
[0022] Figure 3 The image shows the cross-sectional SEM characterization results of the TiB2-reinforced aluminum matrix composite material obtained in Example 1.
[0023] Figure 4 The image shows the tensile stress-strain curve of the TiB2-reinforced aluminum matrix composite material obtained in Example 1. Detailed Implementation
[0024] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.
[0025] As described in the background art, existing technologies for preparing TiB2-reinforced aluminum-based composite powders using methods such as the VIGA method often result in powder products containing nanoparticle agglomeration, inclusions, and microcrack initiation sites. Therefore, it is difficult to obtain TiB2-reinforced aluminum-based composite materials with superior mechanical properties. To address these technical problems, the first aspect of this invention provides a method for preparing TiB2-reinforced aluminum-based composite powder, comprising: step S1, preparing a 7xxx series aluminum alloy into a rod-shaped electrode; the 7xxx series aluminum alloy, by weight percentage, comprises 8 wt.%–10 wt.% Zn, 2.1 wt.%–2.9 wt.% Mg, 1.5 wt.%–2.5 wt.% Cu, 0.1 wt.%–0.2 wt.% Zr, with the balance being Al and unavoidable impurities; step S2, atomizing the rod-shaped electrode into aluminum using an electrode induction melting gas atomization method. The matrix liquid flow is mixed with TiB2 powder to co-deposit 7xxx series aluminum alloy and TiB2 powder to obtain TiB2-reinforced aluminum-based composite powder; the atomization pressure is 2.0MPa~5.0MPa, the atomization power is 30kW~40kW, the feed rate of the rod electrode is 15mm / min~20mm / min, and the powder feeding rate of TiB2 powder is 10g / min~15g / min; the total feed amount of TiB2 powder is 8%~10% based on the total weight of TiB2-reinforced aluminum-based composite powder as 100%; the particle size of TiB2 powder is in the nanometer range.
[0026] Based on the crucibleless electrode induction melting gas atomization (EIGA) method, this invention achieves uniform dispersion of the reinforcing phase and high material purity by realizing the gas atomization co-deposition of nano-sized TiB2 particles and aluminum alloy droplets at the powder preparation source. Specifically, using EIGA technology, a rod-shaped electrode of 7xxx series aluminum alloy is directly melted under an induced magnetic field, and atomization is achieved using a high-speed jet of inert gas, while simultaneously introducing TiB2 nanoparticles. The atomization effect of the high-speed gas flow and the synergy of the synchronous feeding system allow the TiB2 nanoparticles to be instantly coated on the surface of the molten droplets. This process greatly reduces the probability of particle agglomeration under high-temperature conditions, increases the contact area between the particles and the matrix, and thus improves the interfacial bonding strength. The co-deposition mechanism ensures the uniform distribution of particles in the composite powder, which is crucial to the performance of the final material. Through EIGA technology, combined with optimized atomization pressure, atomization power, and particle feed rate, the prepared composite powder exhibits excellent sphericity and a narrow particle size distribution, while significantly reducing so-called "satellite powder" (small particles adhering around large particles). These properties not only increase the bulk density of the powder, making it easier to densify in subsequent sintering processes, but also reduce the probability of defect formation during sintering, such as voids and cracks.
[0027] In the aforementioned atomization process, the appropriate TiB2 content ensures that the reinforcing phase forms an effective stress transfer network in the composite material, while the nanoscale particle size promotes the uniform distribution of the reinforcing phase particles in the matrix, avoiding the interfacial brittleness problem that may be caused by micron-sized particles. The aluminum alloy with the specific formulation used in this invention has high plasticity and a good strength-hardness balance, making it particularly suitable for the preparation of composite materials to achieve high strength and high modulus performance requirements. The age hardening effect of Zn and Mg improves the alloy strength, while the solid solution strengthening and precipitation strengthening of Cu further improve the strength, but their content needs to be controlled to maintain plasticity. The addition of Zr forms an Al3Zr dispersed phase, refining the grains and inhibiting recrystallization, thereby improving high-temperature processing performance and TiB2 interfacial compatibility, giving the matrix both high strength and moderate plasticity.
[0028] In general, by combining EIGA technology with specific 7xxx series aluminum alloy formulations, and by strictly controlling the particle feed rate and particle size, the sphericity, cleanliness, and uniform dispersion of the composite powder have been significantly improved.
[0029] In practical applications, after the composite powder is obtained by atomization deposition, the above preparation method also includes collection and classification: the composite powder obtained by atomization is collected under inert protection or vacuum conditions, and sieved and demagnetized according to the target particle size range to obtain composite powder that meets the requirements of subsequent densification and thermal processing.
[0030] In several typical implementations, to further improve the sphericity and packing density of the obtained composite powder and more significantly reduce the proportion of satellite powder, thereby obtaining a TiB2-reinforced aluminum-based composite powder with superior performance, better processability, and uniform microstructure, step S2 preferably further includes: step S2-1, clamping the rod-shaped electrode onto the electrode fixture, initiating induction heating to melt the end of the rod-shaped electrode and form a droplet; under the action of an inert gas jet, the droplet atomizes to form an aluminum matrix liquid flow with a conical spray direction; step S2-2, simultaneously with the droplet atomization, activating the feeder filled with TiB2 powder, and using a carrier gas to allow the TiB2 powder to contact and mix with the aluminum matrix liquid flow in the form of a TiB2 powder flow, forming a composite liquid flow; step S2-3, the composite liquid flow solidifies to achieve co-deposition, thereby obtaining the TiB2-reinforced aluminum-based composite powder.
[0031] Furthermore, to enhance the mixing uniformity of the aluminum matrix liquid stream and the TiB2 powder stream, preferably: the aluminum matrix liquid stream enters the atomization chamber along its axial direction, and the TiB2 powder stream enters the atomization chamber radially perpendicular to the jet axis of the inert gas, and contacts and mixes with the aluminum matrix liquid stream at the junction point; the vertical distance between the junction point and the axis of the aluminum matrix liquid stream is 10 mm to 15 mm. In practical applications, the carrier gas can be argon.
[0032] To avoid ambiguity, the feeding method for TiB2 powder during the co-deposition process described above employs a closed-loop inert gas-protected powder feeding system. After drying in the feeding hopper (or feeder), the TiB2 powder is conveyed into the pipeline at a precisely controlled rate via a screw feeder, where it mixes with carrier argon gas to form an aerosol-like powder stream. This aerosol stream is radially injected into the atomization chamber through a nozzle, achieving spatial convergence at a distance of 10mm–15mm from the aluminum substrate liquid stream injection axis. During this process, high-temperature aluminum droplets encapsulate the TiB2 particles through surface tension, completing micro-area melting and wetting, and ultimately co-depositing into the cooling and collection device.
[0033] In the above process, to promote the stable formation of the aluminum matrix liquid flow, in step S2-1, the preferred feed rate of the rod electrode is 18±1 mm / min, the atomization pressure is 3.5±0.2 MPa, and the atomization power is 35±2 kW. To ensure that the TiB2 particles can encounter the aluminum matrix liquid flow at a more suitable concentration, in step S2-2, the preferred feed rate of the TiB2 powder is 12±1 g / min. By optimizing the parameters in the above EIGA process, the TiB2 particles can be more uniformly coated by the liquid flow and achieve uniform dispersion in the aluminum matrix, significantly reducing aggregation in the resulting composite powder, and ultimately further improving the particle size uniformity and microstructure uniformity of the resulting composite powder.
[0034] Furthermore, the preferred flow rate of the inert gas in step S2-1 is 1000 m³ / h. 3 / h~1500m 3 / h, more preferably 1300±50m 3 / h, to maintain an inert atmosphere in the atomization zone, reduce melt oxidation, and promote faster breakage and spheroidization of aluminum matrix droplets, further optimizing the sphericity and particle size distribution of the composite powder. In step S2-2, it is preferable that the TiB2 powder has a particle size of 50nm to 100nm, which can promote the reinforcing phase particles to form an interface with the melt more effectively, providing a more uniform reinforcement effect, and also more effectively reducing interface defects and brittleness problems, improving the fracture toughness of the obtained composite powder after sintering and extrusion.
[0035] In step S1, to provide a higher quality aluminum alloy matrix for subsequent EIGA co-deposition, thereby further improving the processing performance of the obtained composite powder, this step preferably further includes: step S1-1, melting 7xxx series aluminum alloy at 710-760°C to obtain a first melt; step S1-2, refining and degassing the first melt at 710-730°C for 0.5 min-1 min to obtain a second melt; step S1-3, adding Al-Ti-B refining agent to the second melt, and sequentially subjecting it to stirring and settling treatment to obtain a third melt; casting the third melt to obtain a rod-shaped electrode; and, to refine the solidification structure of the rod-shaped electrode, thereby optimizing the microstructure of the obtained composite powder and the density of its finished product, the amount of Al-Ti-B refining agent added is preferably 2‰-5‰ based on 100% of the total weight of the first melt; in step S1-3, the stirring treatment time is preferably 2 min-5 min.
[0036] Furthermore, in the preparation process of aluminum-based rod-shaped electrodes, the melt is first cast into a rod blank. Then, the cast rod blank is milled to remove the oxide layer and defect layer, and then machined into a rod-shaped electrode that is easy to clamp. The free end of the electrode is machined with positioning steps to ensure the stability of the material supply, thereby reducing secondary pollution and droplet fluctuations from the source.
[0037] A second aspect of the present invention provides a TiB2-reinforced aluminum-based composite powder, which is prepared by the above-described method for preparing TiB2-reinforced aluminum-based composite powder. Thanks to the step design and parameter control of the above-described preparation method, the resulting composite powder exhibits excellent sphericity, narrow particle size distribution, and uniform particle dispersion, thus providing a good powder raw material for the densification treatment and performance improvement of the materials obtained through subsequent sintering and extrusion.
[0038] It should be noted that due to the complex microstructure formation and compositional changes during the preparation process, especially during EIGA co-deposition, and the limitations of the material field and existing testing and characterization methods, it is difficult to perform a comprehensive quantitative characterization of the complex microstructure of the obtained TiB2-reinforced aluminum-based composite powder. However, performance test results show that the TiB2-reinforced aluminum-based composite powder obtained in this invention possesses superior mechanical properties after being used to prepare profiles.
[0039] A third aspect of this invention provides a TiB2-reinforced aluminum-based composite material, which is obtained by sequentially subjecting the aforementioned TiB2-reinforced aluminum-based composite powder to sintering, molding, and heat treatment. The TiB2-reinforced aluminum-based composite material comprises an aluminum alloy matrix and TiB2 particles dispersed within the aluminum alloy matrix. This invention achieves uniform introduction of the reinforcing phase at the powder preparation source through the EIGA method, avoiding crucible contamination and particle sedimentation that may occur with the VIGA method, and also avoiding the problems of nanoparticle agglomeration, inclusions, and microcrack sources caused by mechanical mixing in powder metallurgy, ultimately obtaining a TiB2-reinforced aluminum-based composite powder with superior comprehensive performance. More specifically, the composite powder prepared by the above method has high cleanliness and good sphericity, which reduces defects such as porosity and incomplete fusion during powder bed melting or metal injection molding, thereby significantly improving the quality and strength of the subsequently obtained composite material. Furthermore, the uniform dispersion of TiB2 nanoparticles in the powder achieved through the above method means that this uniformity can be maintained in subsequent finished products, avoiding localized changes in performance and ensuring that the composite material possesses the same mechanical properties and functional characteristics throughout. The composite powder with narrow particle size distribution and high bulk density obtained based on the EIGA method is more easily densified during sintering, reducing density differences in the resulting material and improving its dimensional stability and consistency of mechanical properties.
[0040] In general, the resulting composite powder, combined with an integrated process chain of hot pressing sintering—hot extrusion—heat treatment, can produce a composite material with dense structure, uniformly dispersed reinforcement, and excellent mechanical properties. Further optimization is achieved by using TiB2-reinforced aluminum matrix composites with a TiB2 particle content of 8wt%–10wt% (100% by weight) to maintain good overall material properties and achieve a better balance between strength and plasticity.
[0041] Furthermore, the tensile strength of the TiB2-reinforced aluminum matrix composite material is 740 MPa–810 MPa, the yield strength is 670 MPa–740 MPa, and the elastic modulus is 86 GPa–90 GPa. This means that through precise control of the parameters in the EIGA process, the reinforcing effect of TiB2 particles in the composite material is more significantly enhanced. After further preparation of the TiB2-reinforced aluminum matrix composite material, not only is the load-bearing capacity of the resulting profile significantly increased, but its stiffness is also greatly improved, enabling it to withstand greater stress without deformation.
[0042] For the process of preparing TiB2-reinforced aluminum-based composite powder into aluminum-based composite profiles, the preferred sintering treatment includes: placing the TiB2-reinforced aluminum-based composite powder in a mold, heating it to 540℃~580℃, and then holding it at 540℃~580℃ under an axial pressure of 30±2MPa for 60min~150min to obtain a sintered blank. During the sintering process, by optimizing the above parameters, more effective contact between composite particles can be promoted, atomic diffusion can be accelerated, and porosity can be significantly eliminated at the microscale, forming a defect-free dense structure and improving the performance of the resulting TiB2-reinforced aluminum-based composite material.
[0043] In the above sintering process, a holding temperature of 560±5℃ is further preferred to facilitate more complete diffusion of the aluminum alloy matrix and form a more stable interfacial bond with the TiB2 particles, without causing abnormal grain growth or matrix overheating, ultimately resulting in a TiB2-reinforced aluminum matrix composite material with superior performance. A holding time of 120±10 min is preferred to provide sufficient diffusion time, promoting the uniform densification of the resulting sintered billet. A heating rate of 10±2℃ / min is preferred to more effectively reduce local overheating and thermal stress, improving the microstructure consistency of the resulting sintered billet.
[0044] To further refine the microstructure of the resulting composite material and improve its plasticity and fatigue resistance, hot extrusion is preferred as the forming process, with an extrusion ratio of (10–20):1, and the hot extrusion is carried out at 430°C–470°C. Further, an extrusion ratio of (15–17):1 is preferred to facilitate sufficient plastic deformation, drive dynamic recrystallization, promote grain refinement, and form a more uniform microstructure, thereby significantly improving the strength and plasticity of the resulting composite material. Simultaneously, hot extrusion is preferably carried out at 450±5°C, a temperature that helps maintain the material in a suitable plastic deformation state, balances work hardening and dynamic softening processes, promotes dislocation rearrangement and annihilation, and thus inhibits abnormal grain growth, improving the overall mechanical properties of the resulting TiB2-reinforced aluminum matrix composite. The preferred hot extrusion speed of 0.5±0.05mm / s aims to improve the stability of the extrusion process, reduce the risk of surface tearing caused by excessive speed, and provide the necessary thermodynamic conditions for dynamic recrystallization, which is beneficial to improving the molding accuracy and surface quality of the resulting composite material.
[0045] The heat treatment process preferably includes sequential solution heat treatment and aging heat treatment. Preferably, the solution heat treatment temperature is 460℃~480℃, and the holding time is 1.5h~3h, to further adapt to the microstructure of the obtained TiB2-reinforced aluminum-based composite powder, promote the dissolution and more uniform distribution of alloying elements, and eliminate stress concentration. The aging heat treatment temperature is preferably 110℃~140℃, and the holding time is preferably 18h~30h, which allows for more uniform and finer formation of the precipitated strengthening phase (such as η′ phase) in the aluminum matrix, thereby further improving the load-bearing capacity and dimensional stability of the resulting composite material.
[0046] Furthermore, to form a more uniform solid solution, reduce grain boundary segregation and microscopic inhomogeneity, and significantly refine the grains to improve the mechanical properties of the resulting composite material, the preferred solution heat treatment temperature is 470±5℃, and the holding time is 2±0.2h. To adapt to the microstructure of the TiB2-reinforced aluminum matrix composite powder, promote more uniform precipitation and more stable growth of the precipitated strengthening phase, and ultimately more effectively improve the overall mechanical properties of the resulting TiB2-reinforced aluminum matrix composite material, based on the above solution heat treatment, the preferred aging heat treatment temperature is 120±5℃, and the holding time is 24±2h.
[0047] A fourth aspect of this invention provides an application of the above-mentioned TiB2-reinforced aluminum-based composite powder as a powder raw material for structural components in the aerospace, rail transportation, and electronic device fields. The TiB2-reinforced aluminum-based composite powder prepared by the above method possesses high cleanliness and sphericity, high particle size distribution uniformity, narrow particle size distribution, and high bulk density. It can be used as a powder raw material to achieve higher densification and, through advanced manufacturing technologies such as additive manufacturing, precision injection molding, and metal injection molding, can be transformed into high-performance structural components.
[0048] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0049] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0050] Example 1
[0051] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0052] (S1-1) The matrix is a 7xxx series aluminum alloy, with the following mass percentages: Zn: 10 wt.%, Mg: 2.5 wt.%, Cu: 2.5 wt.%, Zr: 0.1 wt.%, and the balance being Al and unavoidable impurities. The smelting raw materials include pure Al, pure Zn, pure Mg, pure Cu, and an Al-Zr master alloy. The 7xxx series aluminum alloy is prepared according to the above ranges, smelted at 730°C, and thoroughly stirred to dissolve and homogenize the alloying elements, yielding the first melt.
[0053] (S1-2) High-purity argon gas is used to degas the bottom of the melt for 1 minute to reduce inclusions and hydrogen content, thereby obtaining a clean and homogeneous second melt.
[0054] (S1-3) Add 5‰ of the Al-Ti-B refining agent by mass of the melt at 730℃ and stir thoroughly for 5 minutes to obtain a third melt with fine grains. Copper mold casting and solidification: Pour the obtained purified melt into a copper mold at 710℃ and solidify with water to obtain a square ingot with uniform composition and structure.
[0055] (S2) Peeling and Electrode Preparation. The ingot is milled to remove the oxide layer and defect layer, and then machined into a rod-shaped electrode for easy clamping. The free end of the electrode is machined with positioning steps to ensure the stability of the material supply, thereby reducing secondary pollution and droplet fluctuations from the source.
[0056] (S3-1) Clamping and Feeding Settings: Insert the rod-shaped electrode into the electrode clamp of the EIGA device; simultaneously add nano-TiB2 particles (particle size 50nm~100nm) into the feeding chamber. Use a closed-loop mass flow rate control method to match the feeding rate with the electrode melting mass flow rate, so that the actual TiB2 content in the composite powder and the final product is stabilized at about 9wt.%. This setting ensures that the particles are introduced synchronously in the atomization core area and make full contact with the aluminum droplets formed by atomization.
[0057] (S3-2) EIGA gas atomization "co-deposition" powder preparation: The feed rate of the rod-shaped electrode is controlled at 18 mm / min. Induction heating is activated to locally melt the free end of the electrode to form droplets. Under the action of a high-speed inert gas jet, the droplets undergo instantaneous breakup, spheroidization, and rapid solidification to form an aluminum matrix liquid flow. The feed rate of nano-TiB2 particles is controlled at 12 g / min, and feeding is activated simultaneously. This allows the TiB2 nanoparticles to meet, be coated, and co-solidify with the aluminum matrix liquid flow at the intersection point in the spray core area, where the powder flow (carrier gas is argon). The vertical distance between the intersection point and the axis of the aluminum matrix liquid flow is 10 mm to 15 mm, thereby obtaining a composite powder with uniformly dispersed reinforcement, clean surface, and high sphericity. The process parameters in this embodiment of EIGA are: atomization pressure 3.5 MPa, argon flow rate 1300 m³ / min. 3 / h, induction power 35kW.
[0058] (S3-3) Powder collection and pretreatment. The atomized powder is collected under an inert or vacuum protective atmosphere, then sieved and demagnetized to obtain composite powder within the target particle size range. Vacuum low-temperature drying and pre-degassing are then performed to remove adsorbed water and residual gas. This pretreatment further improves the cleanliness and flowability of the powder, ensuring densification and consistent forming.
[0059] The SEM characterization results of the obtained TiB2-reinforced aluminum-based composite powder are shown in the figure. Figure 1 .
[0060] A method for preparing TiB2-reinforced aluminum matrix composites:
[0061] (R1) Vacuum hot pressing sintering: The composite material powder obtained above is loaded into a graphite mold and heated to 560°C in a vacuum hot pressing sintering furnace at a heating rate of 10°C / min. The mixture is then held under an axial pressure of 30 MPa for 120 min to complete densification and form a compact. Under appropriate loading pressure, pore closure can be ensured while suppressing excessive plastic flow and interface damage, resulting in a sintered compact with low porosity, clean interfaces, and uniform microstructure.
[0062] The cross-sectional SEM characterization results of the obtained sintered billet are shown in the figure. Figure 2 .
[0063] (R2) Hot extrusion forming: After heating and holding the sintered billet, it is hot extruded on an extruder at an extrusion temperature of 450℃, an extrusion speed of 0.5mm / s, and an extrusion ratio of 16:1 to obtain a rod-shaped extruded material with a dense structure and uniform distribution of the second phase and particles. This step achieves grain refinement and defect healing, providing a favorable dislocation and substructure basis for age strengthening.
[0064] (R3) Solution and aging heat treatment. The extruded material was solution treated, held at 470℃ for 2 hours, then water-quenched, and finally artificially aged at 120℃ for 24 hours. After solution and aging heat treatment, TiB2-reinforced aluminum matrix composite material was finally obtained, forming a multi-scale synergistic strengthening structure of η′ / GP zone precipitates, TiB2 particles, and dislocations, achieving simultaneous improvement in strength and elastic modulus while taking into account necessary plasticity.
[0065] The cross-sectional SEM characterization results of the obtained TiB2 reinforced aluminum matrix composite are shown in the figure. Figure 3 .
[0066] Example 2
[0067] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0068] (S1-1) The matrix is a 7xxx series aluminum alloy with the following mass percentages: Zn: 8 wt.%, Mg: 2.9 wt.%, Cu: 1.5 wt.%, Zr: 0.2 wt.%, and the balance being Al and unavoidable impurities. The smelting raw materials include pure Al, pure Zn, pure Mg, pure Cu, and an Al-Zr master alloy. The 7xxx series aluminum alloy is prepared according to the above ranges, smelted at 710°C, and thoroughly stirred to dissolve and homogenize the alloying elements, yielding the first melt.
[0069] (S1-2) High-purity argon gas is used to degas the bottom of the melt for 0.5 min to reduce inclusions and hydrogen content, thereby obtaining a clean and homogeneous second melt.
[0070] (S1-3) Add 2‰ of the melt mass of Al-Ti-B refining agent at 710℃ and stir thoroughly for 2 minutes to obtain a third melt with fine grains. Copper mold casting and solidification: Pour the obtained purified melt into a copper mold at 710℃ and solidify with water to obtain a square ingot with uniform composition and structure.
[0071] (S2) is consistent with Example 1.
[0072] (S3-1) Clamping and Feeding Settings: Insert the rod-shaped electrode into the electrode clamp of the EIGA device; simultaneously add nano-TiB2 particles (50nm in diameter) into the feeding chamber. Use a closed-loop mass flow rate control method to match the feeding rate with the electrode melting mass flow rate, so that the actual TiB2 content in the composite powder and the final product is stabilized at about 8wt.%. This setting ensures that the particles are introduced synchronously in the atomization core area and make full contact with the aluminum droplets formed by atomization.
[0073] (S3-2) EIGA gas atomization "co-deposition" powder preparation: The feed rate of the rod-shaped electrode is controlled at 18 mm / min. Induction heating is activated to locally melt the free end of the electrode to form droplets. Under the action of a high-speed inert gas jet, the droplets undergo instantaneous breakup, spheroidization, and rapid solidification to form an aluminum matrix liquid flow. The feed rate of nano-TiB2 particles is controlled at 12 g / min, and feeding is activated simultaneously. This allows the TiB2 nanoparticles to meet, be coated, and co-solidify with the aluminum matrix liquid flow at the intersection point in the spray core area, where the powder flow (carrier gas is argon). The vertical distance between the intersection point and the axis of the aluminum matrix liquid flow is 10 mm to 15 mm, thereby obtaining a composite powder with uniformly dispersed reinforcement, clean surface, and high sphericity. The process parameters in this embodiment of EIGA are: atomization pressure 2 MPa, argon flow rate 1000 m³ / min. 3 / h, induction power 20kW.
[0074] (S3-3) is consistent with Example 1.
[0075] A method for preparing TiB2-reinforced aluminum matrix composites:
[0076] (R1) Vacuum hot pressing sintering: The composite material powder obtained above is loaded into a graphite mold, heated to 560°C in a vacuum hot pressing sintering furnace at a heating rate of 10°C / min, and held under an axial pressure of 30MPa for 60min to complete densification and form a sintered blank.
[0077] (R2) Hot extrusion forming: After heating and holding the sintered billet, it is hot extruded on an extruder at an extrusion temperature of 430℃, an extrusion speed of 0.5mm / s, and an extrusion ratio of 10:1 to obtain a rod-shaped extruded material with a dense structure and uniform distribution of the second phase and particles.
[0078] (R3) Solution and aging heat treatment. The extruded material was solution treated, held at 460℃ for 3 hours, then water-quenched, and finally artificially aged at 140℃ for 18 hours. After solution and aging heat treatment, TiB2 reinforced aluminum matrix composite material was finally obtained.
[0079] Example 3
[0080] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0081] (S1-1) The matrix is a 7xxx series aluminum alloy with the following mass percentages: Zn: 10 wt.%, Mg: 2.1 wt.%, Cu: 2.5 wt.%, Zr: 0.1 wt.%, and the balance being Al and unavoidable impurities. The smelting raw materials include pure Al, pure Zn, pure Mg, pure Cu, and an Al-Zr master alloy. The 7xxx series aluminum alloy is prepared according to the above ranges, smelted at 760°C, and thoroughly stirred to dissolve and homogenize the alloying elements, yielding the first melt.
[0082] (S1-2) High-purity argon gas is used to degas the bottom of the melt for 0.5 min to reduce inclusions and hydrogen content, thereby obtaining a clean and homogeneous second melt.
[0083] (S1-3) Add 5‰ of the Al-Ti-B refining agent by mass of the melt at 730℃ and stir thoroughly for 2 minutes to obtain a third melt with fine grains. Copper mold casting and solidification: Pour the obtained purified melt into a copper mold at 730℃ and solidify with water to obtain a square ingot with uniform composition and structure.
[0084] (S2) is consistent with Example 1.
[0085] (S3-1) Clamping and Feeding Settings: Insert the rod-shaped electrode into the electrode clamp of the EIGA device; simultaneously add nano-TiB2 particles (100nm in diameter) into the feeding chamber. Use a closed-loop mass flow rate control method to match the feeding rate with the electrode melting mass flow rate, so that the actual TiB2 content in the composite powder and the final product is stabilized at around 10wt.%. This setting ensures that the particles are introduced synchronously in the atomization core area and make full contact with the aluminum droplets formed by atomization.
[0086] (S3-2) EIGA gas atomization "co-deposition" powder preparation: The feed rate of the rod-shaped electrode is controlled at 18 mm / min. Induction heating is activated to locally melt the free end of the electrode to form droplets. Under the action of a high-speed inert gas jet, the droplets undergo instantaneous breakup, spheroidization, and rapid solidification to form an aluminum matrix liquid flow. The feed rate of nano-TiB2 particles is controlled at 12 g / min. Simultaneous feeding is activated so that the TiB2 nanoparticles in the spray core area meet, are coated, and co-solidify with the aluminum matrix liquid flow at the intersection point of the powder flow (carrier gas is argon). The vertical distance between the intersection point and the axis of the aluminum matrix liquid flow is 10 mm to 15 mm, thereby obtaining a composite powder with uniformly dispersed reinforcement, clean surface, and high sphericity. The process parameters in the EIGA process of this embodiment are: atomization pressure 3.5 MPa, argon flow rate 1500 m³ / min. 3 / h, induction power 40kW.
[0087] (S3-3) is consistent with Example 1.
[0088] A method for preparing TiB2-reinforced aluminum matrix composites:
[0089] (R1) Vacuum hot pressing sintering: The composite material powder obtained above is loaded into a graphite mold, heated to 560°C in a vacuum hot pressing sintering furnace at a heating rate of 10°C / min, and held under an axial pressure of 30MPa for 150min to complete densification and form a sintered blank.
[0090] (R2) Hot extrusion forming: After heating and holding the sintered billet at a temperature of 470℃, the extrusion speed is 0.5mm / s and the extrusion ratio is 20:1.
[0091] (R3) Solution and aging heat treatment. The extruded material was solution treated, held at 480℃ for 1.5h, then water-quenched, and finally artificially aged at 110℃ for 30h. After solution and aging heat treatment, TiB2 reinforced aluminum matrix composite material was finally obtained.
[0092] Example 4
[0093] A method for preparing TiB2-reinforced aluminum-based composite powder: consistent with Example 1.
[0094] A method for preparing TiB2-reinforced aluminum matrix composites:
[0095] The only difference between this embodiment and Embodiment 1 is that in step (R1), the holding temperature during the holding process is changed to 540°C.
[0096] Example 5
[0097] A method for preparing TiB2-reinforced aluminum-based composite powder: consistent with Example 1.
[0098] A method for preparing TiB2-reinforced aluminum matrix composites:
[0099] The only difference between this embodiment and Embodiment 1 is that, in step (R1), the holding temperature during the holding process is changed to 580°C.
[0100] Example 6
[0101] A method for preparing TiB2-reinforced aluminum-based composite powder: consistent with Example 1.
[0102] A method for preparing TiB2-reinforced aluminum matrix composites:
[0103] The only difference between this embodiment and Embodiment 1 is that in step (R1), the holding temperature during the holding process is changed to 500°C.
[0104] Example 7
[0105] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0106] The only difference between this embodiment and Embodiment 1 is that in step (S3-2), the feeding rate of the rod electrode is changed to 15 mm / min; and the powder feeding rate of the nano TiB2 particles is changed to 10 g / min.
[0107] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0108] Example 8
[0109] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0110] The only difference between this embodiment and Embodiment 1 is that in step (S3-2), the feed rate of the rod electrode is changed to 20 mm / min; and the powder feeding rate of the nano TiB2 particles is changed to 15 g / min.
[0111] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0112] Example 9
[0113] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0114] The difference between this embodiment and Embodiment 1 lies only in step (S1), specifically:
[0115] (S1-1) Prepare 7xxx series aluminum alloy according to the alloy composition range of Example 1, melt it at 700°C and stir it thoroughly to dissolve and homogenize the alloy elements to obtain the first melt.
[0116] (S1-2) High-purity argon gas is used to degas the bottom of the melt for 1 minute to reduce inclusions and hydrogen content, thereby obtaining a clean and homogeneous second melt.
[0117] (S1-3) Add 5‰ of the melt mass of Al-Ti-B refining agent at 700℃ and stir thoroughly for 5 minutes to obtain a third melt with fine grains.
[0118] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0119] Example 10
[0120] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0121] The difference between this embodiment and Embodiment 1 lies only in step (S1), specifically:
[0122] (S1-1) Prepare 7xxx series aluminum alloy according to the alloy composition range of Example 1, melt it at 770°C and stir it thoroughly to dissolve and homogenize the alloy elements to obtain the first melt.
[0123] (S1-2) High-purity argon gas is used to degas the bottom of the melt for 1 minute to reduce inclusions and hydrogen content, thereby obtaining a clean and homogeneous second melt.
[0124] (S1-3) Add 1‰ of Al-Ti-B refining agent by mass of the melt at 770℃ and stir thoroughly for 2 minutes to obtain a third melt with fine grains.
[0125] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0126] Example 11
[0127] A method for preparing TiB2-reinforced aluminum-based composite powder: consistent with Example 1.
[0128] A method for preparing TiB2-reinforced aluminum matrix composites:
[0129] The only difference between this embodiment and Embodiment 1 is that the extrusion speed of the hot extrusion in step (R2) is changed to 0.1 mm / s.
[0130] Example 12
[0131] A method for preparing TiB2-reinforced aluminum-based composite powder: consistent with Example 1.
[0132] A method for preparing TiB2-reinforced aluminum matrix composites:
[0133] The only difference between this embodiment and Embodiment 1 is that the extrusion speed of the hot extrusion in step (R2) is changed to 1 mm / s.
[0134] Comparative Example 1
[0135] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0136] The only difference between this comparative example and Example 1 is that the TiB2 particles added in step (S3) are changed to micron-sized particles with a particle size of <50μm.
[0137] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0138] Comparative Example 2
[0139] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0140] The only difference between this comparative example and Example 1 is that the total amount of nano-TiB2 particles added in step (S3) is changed so that the TiB2 content in the composite powder is 5 wt.%.
[0141] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0142] Comparative Example 3
[0143] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0144] The only difference between this comparative example and Example 1 is that in step (S3-2), the atomization pressure is changed to 6 MPa.
[0145] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0146] Comparative Example 4
[0147] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0148] The only difference between this comparative example and Example 1 is that in step (S3-2), the feed rate of the rod electrode is changed to 10 mm / min; and the powder feeding rate of the nano TiB2 particles is changed to 5 g / min.
[0149] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0150] Comparative Example 5
[0151] A method for preparing TiB2-reinforced aluminum-based composite powder:
[0152] The only difference between this comparative example and Example 1 is that in step (S3-2), the feed rate of the rod electrode is changed to 25 mm / min; and the powder feeding rate of the nano TiB2 particles is changed to 20 g / min.
[0153] A method for preparing a TiB2-reinforced aluminum matrix composite material: consistent with Example 1.
[0154] Test methods
[0155] Tensile strength and yield strength: obtained according to the national standard GB / T 228.1—2021 Metallic materials, tensile testing—Part 1: Test method at room temperature.
[0156] Elastic modulus: obtained by pulse excitation method.
[0157] For example, the tensile stress-strain curve of the TiB2-reinforced aluminum matrix composite obtained in Example 1 is shown in the figure. Figure 4 .
[0158] The aluminum-based composite materials obtained in each embodiment and comparative example were subjected to the above tests, and the results are shown in Table 1.
[0159] Table 1
[0160]
[0161]
[0162] As can be seen from the above description, the embodiments of the present invention have achieved the preparation of TiB2-reinforced aluminum-based composite powder with advantages such as excellent sphericity, narrow particle size distribution, and uniform particle dispersion. The obtained composite powder can provide a good powder raw material for the densification treatment and performance improvement of the material obtained by subsequent sintering and extrusion, and the TiB2-reinforced aluminum-based composite material prepared thereby exhibits particularly superior mechanical properties.
[0163] In each embodiment, the parameter combination of Embodiment 1 is the preferred scheme, suitable for scale-up application as the preferred process window under engineering conditions. For other embodiments and comparative examples:
[0164] The comparison results of Examples 1 to 6 and Comparative Examples 1 to 3 show that, under the premise of consistent hot extrusion process and heat treatment regime, atomization pressure and sintering temperature are the key variables determining the performance of the final material sample. When the atomization pressure is increased from 2.0 MPa (Example 2) to 3.5 MPa (Example 1), the powder particle size distribution converges, sphericity and bulk density increase, hot pressing densification is more complete, and the strength and elastic modulus of the material are improved. Further increasing to 5.0 MPa (Example 3) results in a decrease in strength and yield due to the increased proportion of "satellite powder," poorer packing fluidity, and increased surface oxygen. Although the modulus is close to, it is slightly lower than that of Example 1 (but still better than the comparative examples). In Comparative Example 3, this unfavorable trend intensifies, with more obvious satellite powder and packing degradation, leading to a significant overall decrease in performance compared to the examples.
[0165] Regarding sintering temperature, 540℃ (Example 4) resulted in lower density and weaker interfacial bonding due to insufficient diffusion, leading to a slight decrease in performance. 580℃ (Example 5) exhibited a slight interfacial reaction or a tendency for abnormal grain growth, and its overall performance was also slightly lower than that of Example 1. In Example 6, the sintering temperature was low, resulting in weaker densification and a further decrease in strength / yield strength. The overall performance was slightly limited by residual porosity and interfacial weakening, but the elastic modulus remained relatively superior. Therefore, Example 1 showed the best performance in terms of strength-modulus synergy, while the other examples exhibited varying degrees of performance reduction when deviating from the optimal window. In other words, after obtaining TiB2-reinforced aluminum-based composite powder, optimizing the holding temperature during hot pressing to obtain the composite material promotes more complete diffusion of the aluminum alloy matrix, forming a more stable interfacial bond with the TiB2 particles, without causing abnormal grain growth or matrix overheating, ultimately resulting in a TiB2-reinforced aluminum-based composite material with superior performance.
[0166] Regarding the hot extrusion step in the process of preparing composite materials, by comparing Examples 11 and 12 with Example 1, it can be seen that the preferred hot extrusion speed can improve the stability of the extrusion process, reduce the risk of surface tearing caused by excessive speed, and provide the necessary thermodynamic conditions for dynamic recrystallization, which is beneficial to improving the molding accuracy and surface quality of the obtained composite material, and ultimately making the obtained composite material exhibit superior mechanical properties.
[0167] Besides the process window, the particle size and content of the reinforcing phase also have a substantial impact on the results. In Comparative Example 1, the particle size was adjusted to the micrometer level (<5 μm). At a similar content, the overall performance deteriorated significantly due to the significant reduction in interfacial unit area, the worsening of Orowan pinning and load transfer efficiency, and the fact that micrometer particles are more likely to become crack initiators. In Comparative Example 2, when the actual TiB2 content was reduced to about 5 wt.%, the volume fraction of the reinforcing phase was insufficient to form an effective load-bearing skeleton and modulus-enhancing channels. The elastic modulus decreased significantly, and the strength / yield strength also decreased simultaneously. This indicates that at the nanoscale, a reasonable volume fraction still needs to be maintained to achieve a balance between strength and modulus.
[0168] By comparing Examples 7 and 8 and Comparative Examples 4 and 5 with Example 1, it can be seen that in the process of preparing TiB2-reinforced aluminum-based composite powder, by synergistically optimizing the feeding rate of the rod-shaped electrode and the powder feeding rate of the nano-TiB2 particles, the TiB2 particles can be more uniformly coated by the liquid flow and uniformly dispersed in the aluminum matrix, significantly reducing the aggregation phenomenon in the obtained composite powder, and ultimately further improving the particle size uniformity and microstructure uniformity of the obtained composite powder.
[0169] By comparing Examples 9 and 10 with Example 1, it can be seen that by optimizing the conditions in the process of casting the electrode sample from 7xxx series aluminum alloy, a higher quality aluminum alloy matrix can be provided for subsequent EIGA co-deposition, thereby further improving the processing performance of the obtained composite powder and obtaining a TiB2 particle-reinforced aluminum matrix composite material with better mechanical properties.
[0170] In other words, this invention obtains aluminum-based composite powder with high sphericity, narrow particle size, low satellite powder content, and uniform dispersion of reinforcing phase through crucible-free co-deposition using EIGA. High density and clean interface are achieved through vacuum hot pressing sintering. Subsequently, combined with hot extrusion and solution aging heat treatment, a stable and effective load transfer-Orowan pinning-precipitation strengthening network is constructed, ultimately obtaining TiB2 particle-reinforced aluminum-based composite material with synergistic improvement in strength and modulus.
[0171] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those described herein.
[0172] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for producing a TiB2 reinforced aluminum matrix composite powder, characterized by, The method comprises the following steps: S1, preparing a 7xxx series aluminum alloy into a rod-shaped electrode; The 7xxx series aluminum alloy comprises 8wt.%-10wt.% of Zn, 2.1wt.%-2.9wt.% of Mg, 1.5wt.%-2.5wt.% of Cu, 0.1wt.%-0.2wt.% of Zr, and the balance of Al and inevitable impurities, in terms of weight percentage; S2, atomizing the rod-shaped electrode into an aluminum matrix liquid stream by using an electrode induction melting gas atomization method, and adding TiB2 powder to co-deposit the 7xxx series aluminum alloy and the TiB2 powder to obtain the TiB2 reinforced aluminum matrix composite powder; The atomization pressure is 2.0-5.0 MPa, the atomization power is 30-40 kW, the feeding rate of the rod-shaped electrode is 15-20 mm / min, and the powder feeding rate of the TiB2 powder is 10-15 g / min; The total feeding amount of the TiB2 powder is 8%-10% based on the total weight of the TiB2 reinforced aluminum matrix composite powder; The particle size of the TiB2 powder is nanoscale.
2. The method for preparing TiB2-reinforced aluminum-based composite powder according to claim 1, characterized in that, The step S2 further comprises: S2-1, clamping the rod-shaped electrode to an electrode clamp, and starting induction heating to melt the end of the rod-shaped electrode and form a molten drop; under the action of a jet of inert gas, the molten drop is atomized to form the aluminum matrix liquid stream with a conical distribution of jet directions; S2-2, while the molten drop is being atomized, starting a feeder filled with the TiB2 powder, and making the TiB2 powder contact and mix with the aluminum matrix liquid stream in the form of a TiB2 powder stream through a carrier gas to form a composite liquid stream; S2-3, the composite liquid stream is solidified to achieve the co-deposition, thereby obtaining the TiB2 reinforced aluminum matrix composite powder; Preferably, the TiB2 powder stream enters the atomization chamber along a radial direction perpendicular to the jet axis of the inert gas, and contacts and mixes with the aluminum matrix liquid stream at an intersection point; the vertical distance between the intersection point and the axis of the aluminum matrix liquid stream is 10-15 mm; More preferably, in the step S2-1, the feeding rate of the rod-shaped electrode is 18±1 mm / min, the atomization pressure is 3.5±0.2 MPa, and the atomization power is 35±2 kW; and / or, in the step S2-2, the powder feeding rate of the TiB2 powder is 12±1 g / min.
3. The method for preparing the TiB2 reinforced aluminum matrix composite powder according to claim 1 or 2, wherein the particle size of the TiB2 powder in the step S2-2 is 50-100 nm. The flow rate of the inert gas in the step S2-1 is 1000 m 3 / h~1500 m 3 / h, preferably 1300±50 m 3 / h; and / or, The step S1 further comprises:
4. The method of producing a TiB2 reinforced aluminum matrix composite powder according to any one of claims 1 to 3, characterized in that, S1-1, melting the 7xxx series aluminum alloy at 710-760 ℃ to obtain a first melt; S1-2, refining and degassing the first melt at 710-730 ℃ for 0.5-1 min to obtain a second melt; Step S1-3, adding an Al-Ti-B refiner into the second melt, and then sequentially performing stirring treatment and standing treatment to obtain a third melt; and the third melt is cast to obtain the rod-shaped electrode; Preferably, the Al-Ti-B refiner is added in an amount of 2‰-5‰, based on 100% of the total weight of the first melt; More preferably, in the step S1-3, the stirring treatment is performed for 2-5 min.
5. A TiB2 reinforced aluminum matrix composite powder, characterized in that, The TiB2 reinforced aluminum matrix composite powder is prepared by the method for preparing the TiB2 reinforced aluminum matrix composite powder according to any one of claims 1-4.
6. A TiB2 reinforced aluminum matrix composite, characterized in that, The TiB2 reinforced aluminum matrix composite material is obtained by sequentially performing sintering treatment, forming treatment and heat treatment on the TiB2 reinforced aluminum matrix composite powder according to claim 5; and the TiB2 reinforced aluminum matrix composite material comprises an aluminum alloy matrix and TiB2 particles dispersed in the aluminum alloy matrix; Preferably, the content of the TiB2 particles is 8wt%-10wt%, based on 100% of the total weight of the TiB2 reinforced aluminum matrix composite material; More preferably, the TiB2 reinforced aluminum matrix composite material has a tensile strength of 740-810 MPa, a yield strength of 670-740 MPa and an elastic modulus of 86-90 GPa.
7. The TiB2 reinforced aluminum matrix composite of claim 6, wherein, The sintering treatment comprises: placing the TiB2 reinforced aluminum matrix composite powder in a mold, performing temperature rising treatment to reach a holding temperature, and performing holding pressure treatment at the holding temperature to obtain a sintered blank. The holding temperature is 540-580℃; The axial pressure of the holding pressure treatment is 30±2 MPa, and the holding pressure time is 60-150 min; Preferably, the holding temperature is 560±5℃, and the holding pressure time is 120±10 min; More preferably, the temperature rising rate of the temperature rising treatment is 10±2℃ / min.
8. The TiB2 reinforced aluminum matrix composite of claim 6 or 7, wherein, The forming treatment is performed in the form of hot extrusion; the extrusion ratio of the hot extrusion is (10-20):1, and the hot extrusion is performed at 430-470℃; Preferably, the extrusion ratio of the hot extrusion is (15-17):1, and the hot extrusion is performed at 450±5℃; More preferably, the extrusion speed of the hot extrusion is 0.5±0.05 mm / s.
9. The TiB2 reinforced aluminum matrix composite of any one of claims 6-8, wherein, The heat treatment comprises sequentially performing solid solution heat treatment and aging heat treatment; The temperature of the solid solution heat treatment is 460-480℃, and the holding time is 1.5-3 h; The temperature of the aging heat treatment is 110-140℃, and the holding time is 18-30 h; Preferably, the temperature of the solid solution heat treatment is 470±5℃, and the holding time is 2±0.2 h; and / or, the temperature of the aging heat treatment is 120±5℃, and the holding time is 24±2 h.
10. Application of the TiB2 reinforced aluminum matrix composite powder according to claim 5 as a powder raw material of a structural part in the fields of aerospace, rail transportation and electronic devices.
Citation Information
Cited By
Titanium alloy coarse particle powder recovery EIGA atomization method
CN121928036A