High-strength laser pressure welding method

By using a C-shaped welding trajectory linked to a servo clamping mechanism and a laser galvanometer, the problems of gaps and cracks in the welding of high-strength steel materials were solved, achieving high-strength zero-gap welding and improving welding quality and fatigue strength.

CN121289760APending Publication Date: 2026-01-09HAOQIONG (SHANGHAI) CONNECTION NEW TECHNOLOGY DEVELOPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511841848.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-09
Publication Date
2026-01-09

AI Technical Summary

Technical Problem

In existing technologies, the welding of high-strength steel materials suffers from problems such as incomplete welding and welding cracks caused by assembly gaps. Traditional laser welding processes are difficult to effectively eliminate gaps and are prone to stress concentration.

Method used

By linking a servo clamping mechanism with a laser galvanometer, eliminating gaps with a rigid nozzle, and optimizing stress distribution through a C-shaped welding trajectory, combined with real-time monitoring of the servo clamping mechanism and dynamic compensation of the laser focus, zero-gap contact welding is achieved.

Benefits of technology

It effectively eliminates assembly gaps, reduces welding crack sensitivity, and improves the fatigue strength and welding quality of welded joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121289760A_ABST
    Figure CN121289760A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength laser pressure welding method which is executed by a system comprising a servo pressing driving mechanism and a laser galvanometer assembly of which the tail end is integrated with a rigid coaxial pressing nozzle. The method comprises the following steps that (1) a servo pressing driving mechanism is controlled to drive a laser galvanometer assembly to feed downwards in the Z-axis direction till the end face of a rigid coaxial pressing nozzle abuts against the surface of a workpiece; after contact, an axial feeding force is continuously applied to a preset pressure and a stroke threshold value; and (2) the servo pressing driving mechanism is kept in a position locking or torque keeping state so as to maintain constant mechanical pressing force, the laser galvanometer assembly is triggered to emit light, the laser beam is controlled to scan a C-shaped welding track within the range of the inner hole of the nozzle, and the C-shaped welding track is a non-closed curve and is not coincident in head and tail. According to the method, the C-shaped non-closed track is adopted, compared with a traditional O-shaped track, the C-shaped opening provides a stress release channel, closing of circumferential tensile stress is effectively blocked, and the welding crack sensitivity of the high-strength steel is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to welding processing, in particular to a high-strength laser pressure welding method. BACKGROUND

[0002] In the field of automobile manufacturing, aerospace and hardware processing, the splicing of white body and structural parts often involves the lap welding of materials such as high-strength steel and hot-formed steel. Traditional laser welding processes (such as remote scanning welding) usually require a high degree of fit between the plates (the gap is usually required to be less than 10% of the plate thickness). However, in actual industrial production, due to factors such as stamping precision and fixture positioning, there is often an unavoidable assembly gap between the plates to be welded.

[0003] In the prior art, the gap is usually compensated by increasing the laser power or using filler wire welding, but this can easily cause the weld to collapse, undercut or be false. In addition, for high-strength steel materials, the traditional closed circular (O-shaped) welding trajectory is prone to stress concentration at the arc, resulting in crystalline or arc pit cracks in the center of the weld, which seriously affects the fatigue strength of the welded joint.

[0004] Therefore, there is an urgent need for a high-strength laser pressure welding method that can both physically eliminate the gap between the plates and control the welding stress through an optimized light path trajectory. SUMMARY

[0005] The purpose of the present application is to provide a high-strength laser pressure welding method that uses a servo pressing mechanism in conjunction with a laser galvanometer to physically eliminate the welding gap using a rigid nozzle, and cooperates with a specific C-shaped welding trajectory to solve the problems of false welding and high-strength steel welding cracks caused by gaps in the prior art.

[0006] To achieve the above-mentioned purpose, the present application provides the following technical solutions: A high-strength laser pressure welding method is performed using a system comprising a servo pressing drive mechanism and a laser galvanometer assembly with an integrated rigid coaxial pressing nozzle, the method comprising the following steps: 1) Control the servo pressing drive mechanism to drive the laser galvanometer assembly to feed downward along the Z-axis until the rigid coaxial pressing nozzle end face presses against the workpiece surface; after contact, continue to apply axial feed force to a preset pressure threshold, and use mechanical pressure to eliminate the assembly gap between the plate layers; 2) Keep the servo pressing drive mechanism in a position-locked or torque- maintained state to maintain constant mechanical pressing force and displacement, trigger the laser galvanometer assembly to emit light, and control the laser beam to scan a C-shaped welding trajectory within the nozzle inner hole, the C-shaped welding trajectory being a non-closed curve and not coinciding at the beginning and end, and the rigid coaxial pressing nozzle end face forming a closed mechanical pressing area outside the C-shaped welding trajectory to maintain the fit between the plate layers; 3) Determine that the processing is complete; 4) End the processing.

[0007] Preferably, in step 1), the feedback torque value and the encoder position value of the servo pressing drive mechanism are monitored in real time; only when the feedback torque value reaches the set pressing force and the Z-axis downward displacement amount is within the preset effective tolerance interval, it is determined that the gap elimination is qualified and step 2) is allowed to enter; if the displacement amount exceeds the tolerance interval, step 4) is entered.

[0008] Preferably, in step 2), the specific path planning of the C-shaped welding trajectory is that the laser beam starts from the opening side of the C-shaped arc, continuously scans along the circular arc path to the other side of the arc, forming a gap; the direction of the gap is preset according to the stress direction or the gravity direction of the workpiece, so as to block the crack propagation path when the weld cools and shrinks.

[0009] Preferably, in step 2), the focal position of the laser beam is dynamically compensated according to the actual downward displacement amount of the servo pressing drive mechanism in step 1); the accurate height of the upper surface of the workpiece is calculated according to the actual Z-axis coordinate after the workpiece is compacted by the rigid pressing nozzle; the laser galvanometer assembly adjusts the focal length in real time according to the height, so as to ensure that the laser focal point is always located at the plate bonding surface or the preset defocusing position when the C-shaped welding trajectory is scanned.

[0010] Preferably, the size of the C-shaped welding trajectory is limited within the inner diameter range of the rigid pressing nozzle.

[0011] The beneficial effects of the present application are: 1. Active gap elimination: by directly pressing the workpiece with the servo-driven rigid nozzle, the "uncontrollable gap" non-contact welding is converted into "zero gap" contact pressure welding, which significantly reduces the precision requirements of the workpiece pre-process.

[0012] 2. Crack suppression: C-shaped non-closed trajectory is adopted, compared with the traditional O-shaped trajectory, the C-shaped opening provides a stress release channel, effectively blocks the closure of the circumferential tensile stress, and greatly reduces the high-strength steel welding crack sensitivity. BRIEF DESCRIPTION OF DRAWINGS

[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the following will briefly introduce the drawings needed to be used in the embodiments or prior art description. Obviously, for those skilled in the art, other drawings can also be obtained without creative labor based on these drawings.

[0014] Figure 1 is a process flow chart of an embodiment of the present application; Figure 2 is a path planning schematic diagram of the C-shaped welding trajectory in an embodiment of the present application. Specific embodiments

[0015] The accompanying drawings are only for illustrative purposes and should not be construed as a limitation to this patent; for better illustration of this embodiment, some components in the drawings are omitted, enlarged or reduced, which do not represent the dimensions of the actual product.

[0016] For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted. The technical solutions of the present invention will be further described below in conjunction with the drawings and embodiments.

[0017] As Figure 1 and Figure 2 shown, this embodiment provides a high-strength laser pressure welding method, which is executed based on a set of laser pressure welding system. The system includes a frame, a servo pressing drive mechanism (such as a servo motor cooperating with a ball screw and a guide rail) installed on the frame, and a laser galvanometer assembly connected to the output end of the drive mechanism. A rigid coaxial pressing nozzle (preferably made of copper alloy or cemented carbide) is integrated at the end of the light outlet of the laser galvanometer assembly, and a through hole is provided in the center of the rigid coaxial pressing nozzle for the laser beam to pass through.

[0018] The pressure welding method of this embodiment specifically includes the following steps: Step 1: Rigid addressing and double-loop detection; Control the servo pressing drive mechanism to drive the entire laser galvanometer assembly and the rigid coaxial pressing nozzle to feed downward along the Z-axis (the direction perpendicular to the workpiece surface). During the feeding process, the system monitors the feedback torque value of the servo motor and the Z-axis position value feedback by the encoder in real time. When the end face of the rigid coaxial pressing nozzle physically contacts the workpiece surface, continue to apply the downward movement, and at this time the torque value will rise rapidly. The system sets a preset pressure threshold (corresponding to the servo torque) and / or an effective tolerance range (corresponding to the Z-axis coordinate, such as the standard workpiece height ± 0.5mm).

[0019] Logical judgment: When the feedback torque value reaches the set pressing force, and the downward displacement of the Z-axis at this time is within the preset effective tolerance range. This means that the workpiece exists and the thickness is normal, and at the same time, the assembly gap between the plates is forcibly eliminated by mechanical pressure. At this time, it is determined to be qualified and allowed to enter step 2.

[0020] If the torque reaches, but the displacement exceeds the tolerance range (for example, too large displacement indicates that the workpiece is missing, too small displacement indicates that there are extra workpieces or foreign objects blocking), or the displacement is in place but the torque is insufficient. At this time, it is determined to be abnormal, and directly jump to step 4, the system alarms and stops, preventing the laser from emitting light accidentally and damaging the equipment or producing defective products.

[0021] Step 2: C-shaped trajectory welding under pressure holding state; After confirming the qualification of the pressing, the servo pressing driving mechanism is kept in the "position locking" or "torque holding" mode. At this time, the rigid coaxial pressing nozzle forms a closed mechanical pressing area around the welding area, maintaining the close contact between the layers of the sheet.

[0022] The system triggers the laser galvanometer assembly to emit light. In this process, the system accurately calculates the height of the upper surface of the workpiece according to the actual Z-axis coordinate at which the rigid pressing nozzle finally stops after compacting the workpiece in step 1. The dynamic focusing unit (Z-axis galvanometer) inside the laser galvanometer assembly adjusts the focal length in real time according to the height data, ensuring that the laser focal point always accurately falls on the sheet bonding surface or the preset defocusing position required by the process, avoiding the drift of the focal point caused by the deformation of the workpiece.

[0023] The size of the C-shaped welding trajectory is strictly limited within the inner diameter of the nozzle (for example, the inner diameter of the nozzle is 10 mm, and the outer diameter of the C-shaped trajectory is 8 mm), ensuring that the laser does not hit the nozzle wall.

[0024] The specific path planning is as follows: the laser beam starts from one side of the opening of the C-shaped arc, continuously scans along the circular arc path, and ends at the other side, forming a physical gap in the middle. The C-shaped arc is a non-closed curve, and the beginning and end do not coincide.

[0025] The direction of the gap is set according to the stress direction or gravity direction of the workpiece in service. For example, if the main stress direction is horizontally to the right, the gap can be set at the back of the stress to block the closing of the circumferential tensile stress generated when the weld cools and shrinks, cutting off the crack propagation path.

[0026] Step 3: Determine if the processing is complete; After the laser scanning is completed, the system receives the completion signal of the laser galvanometer assembly, confirming the end of the welding process.

[0027] Step 4: End processing; The servo pressing driving mechanism drives the laser galvanometer assembly to reverse and retreat (the Z-axis is lifted upwards), and the rigid coaxial pressing nozzle leaves the workpiece surface, releasing the workpiece, completing a single pressing and welding cycle.

[0028] Through the above steps, the present application is suitable for lap welding of high-strength steel body parts, effectively solving the problems of defects and cracks caused by gaps.

[0029] Obviously, the above embodiments of the present application are only examples for clearly illustrating the present application, and are not intended to limit the embodiments of the present application. Based on the above description, other different forms of changes or variations can be made by those skilled in the art. Here, it is not necessary or possible to exhaust all embodiments. Any modification, equivalent replacement and improvement made within the spirit and principles of the present application shall be included in the protection scope of the claims of the present application.

Claims

1. A high-intensity laser pressure welding method, characterized in that, The method, performed using a system comprising a servo-driven clamping mechanism and an integrated rigid coaxial clamping nozzle at the end, includes the following steps: 1) Control the servo clamping drive mechanism to drive the laser galvanometer assembly to feed downward along the Z-axis until the end face of the rigid coaxial clamping nozzle presses against the workpiece surface; after contact, continue to apply axial feed force to the preset pressure threshold, and use mechanical pressure to eliminate the assembly gap between the sheet metal layers; 2) Keep the servo clamping drive mechanism in position lock or torque holding state to maintain constant mechanical clamping force and displacement, trigger the laser galvanometer assembly to emit light, and control the laser beam to scan a C-shaped welding trajectory within the nozzle inner hole. The C-shaped welding trajectory is a non-closed curve and the beginning and end do not coincide. The rigid coaxial clamping nozzle end face forms a closed mechanical clamping area around the C-shaped welding trajectory to maintain the interlayer bonding of the sheet metal. 3) Confirm that the processing is complete; 4) End processing.

2. The high-intensity laser pressure welding method according to claim 1, characterized in that, In step 1, the feedback torque value and encoder position value of the servo clamping drive mechanism are monitored in real time; only when the feedback torque value reaches the set clamping force and the Z-axis downward displacement is within the preset effective tolerance range, the gap elimination is deemed qualified and allowed to proceed to step 2); if the displacement exceeds the tolerance range, proceed to step 4).

3. The high-intensity laser pressure welding method according to claim 1, characterized in that, In step 2), the specific path planning for the C-shaped welding trajectory is as follows: The laser beam starts from one side of the C-shaped opening, scans continuously along the arc path to the other side, and forms a notch; The direction of the notch is preset according to the force direction or gravity direction of the workpiece, so as to block the crack propagation path when the weld cools and shrinks.

4. The high-intensity laser pressure welding method according to claim 1, characterized in that, In step 2), the focal position of the laser beam is dynamically compensated based on the actual downward displacement fed back by the servo clamping drive mechanism in step S2. Calculate the precise height of the upper surface of the workpiece based on the actual Z-axis coordinates after the workpiece is compacted by the rigid clamping nozzle; The laser galvanometer assembly adjusts the focal length in real time according to this height to ensure that the laser focus is always located at the joint surface of the plate or the preset defocus position when scanning the C-shaped welding trajectory.

5. The high-intensity laser pressure welding method according to claim 1, characterized in that, The dimensions of the C-shaped welding trajectory are limited to the inner diameter range of the rigid clamping nozzle.