Method for preparing alcohol oxidation coupling hydrogen production catalyst by using waste ternary positive electrode material

By using an electric field-driven method of lithium removal and in-situ growth of iron hydroxide, waste ternary cathode materials are transformed into an alcohol oxidation coupled hydrogen production catalyst. This solves the problems of low added value of waste battery resource recycling and high energy consumption of electrocatalytic hydrogen production, and realizes a high-efficiency and low-cost electrocatalytic alcohol oxidation coupled hydrogen production reaction, while simultaneously preparing high-value-added chemicals.

CN121428603BActive Publication Date: 2026-06-09HEFEI UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202512033469.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-30
Publication Date
2026-06-09
Estimated Expiration
2045-12-30

Smart Images

  • Figure CN121428603B_ABST
    Figure CN121428603B_ABST
Patent Text Reader

Abstract

This invention belongs to the interdisciplinary field of resource recovery from spent lithium-ion batteries and electrocatalytic energy conversion technology, and discloses a method for preparing an alcohol oxidation-coupled hydrogen production catalyst using spent ternary cathode materials. This method employs a synergistic strategy of electric field-driven delithiation and in-situ modification with iron hydroxide: first, the spent cathode material is pretreated, and then delithiation is performed via an electric field to convert it into a Ni-Co-Mn transition metal composite oxide, simultaneously recovering lithium carbonate; then, the transition metal composite oxide is mixed with iron salt, and after ultrasonic reaction, FeOOH grows in situ on the surface of the transition metal composite oxide and is loaded onto a nickel foam substrate to form a composite catalyst. The transition metal and FeOOH exhibit a significant synergistic catalytic effect, greatly enhancing the alcohol oxidation-coupled hydrogen production reaction, reducing the total electrolytic potential of water electrolysis, and improving hydrogen production efficiency. This invention features a simple process, mild reaction conditions, and combines the advantages of high-value resource recovery with low-energy hydrogen production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the interdisciplinary field of resource recycling of waste lithium-ion batteries and electrocatalytic energy conversion technology, specifically involving a method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode materials. Background Technology

[0002] With the energy crisis and environmental problems caused by the overconsumption of fossil fuels becoming increasingly prominent, electrocatalytic water splitting for hydrogen production, as a clean and renewable energy conversion technology, has become a key research focus in the energy field. However, the oxygen evolution reaction (OER) of the traditional water splitting system suffers from drawbacks such as slow kinetics, no added value of the products, and high cost of precious metal catalysts (Ru / Ir-based), which seriously restricts its large-scale application.

[0003] To overcome the aforementioned bottlenecks, researchers have proposed a coupled hydrogen production strategy that replaces the OER with an electrocatalytic alcohol oxidation reaction (AOR). Under this strategy, alcohol substrates (such as benzyl alcohol and ethanol) can be oxidized at the anode into high-value-added carboxylic acids, aldehydes, and ketones, while hydrogen evolution is simultaneously achieved at the cathode with low energy consumption. The overall reaction offers the dual benefits of energy conversion and resource enhancement. A typical benzyl alcohol oxidation coupled hydrogen production reaction is as follows:

[0004] Anode: C7H8O + 4 OH- - → C6H5COOH + 3 H2O + 4 e - ;

[0005] Cathode: 4 H₂O + 4 e⁻ - → 2 H2 + 4 OH - ;

[0006] Overall reaction: C7H8O + H2O → C6H5COOH + 2 H2.

[0007] Current electrocatalytic alcohol oxidation catalysts mostly rely on primary transition metals / oxides such as Ni, Co, and Pd for preparation, which not only consumes limited mineral resources but also drives up catalyst costs. Meanwhile, the rapid development of new energy vehicles and energy storage industries has led to a surge in the number of spent lithium-ion batteries, particularly their ternary cathode materials (LiNi). x Co y Mn 1-x-y O2 is rich in high-valence transition metals such as Ni, Co, and Mn. If only traditional hydrometallurgical / pyrometallurgical processes are used for the extraction of elemental metals, there are problems such as complex processes, high energy consumption, and low product added value.

[0008] Therefore, developing a technology that directly converts waste ternary cathode materials into high-performance electrocatalytic alcohol oxidation coupled hydrogen production catalysts can not only realize the high-value utilization of waste battery resources, but also reduce the overall cost of electrocatalytic hydrogen production systems, which is of great significance for promoting the coordinated development of battery recycling and clean energy. Summary of the Invention

[0009] Addressing the issues of low added value from recycling waste ternary cathode materials, reliance on primary mineral resources for electrocatalytic alcohol oxidation coupled hydrogen production catalysts, and high energy consumption in the anode reaction of water cracking for hydrogen production, this invention provides a method for preparing alcohol oxidation coupled hydrogen production catalysts using waste ternary cathode materials. The aim is to achieve high-value conversion of waste ternary cathode materials based on electric field-driven delithiation and in-situ growth of iron hydroxide, realizing the targeted recovery of lithium elements and functional reuse of transition metal components in waste ternary cathode materials, and constructing an integrated technical path for waste battery resource recycling and low-energy electrocatalytic hydrogen production.

[0010] To achieve the above objectives, the present invention adopts the following technical solution:

[0011] This invention first provides a method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material, comprising the following steps:

[0012] Step 1: Pretreatment of waste ternary cathode materials

[0013] Waste lithium-ion battery ternary cathode sheets are pre-treated by dismantling, peeling, impurity removal, grinding, and drying to obtain waste ternary cathode powder LiNi. x Co y Mn 1-x-y O2 (x>0, y>0, 1-xy>0);

[0014] Among them, waste ternary cathode powder LiNi x Co y Mn 1-x-y O2 includes, but is not limited to, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.88 Co 0.06 Mn 0.06 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 1 / 3Co1 / 3 Mn 1 / 3 At least one of O2, etc.

[0015] Step 2: Preparation of electric field-driven delithiation and transition metal composite oxide powder

[0016] The waste ternary cathode powder and the binder polyvinylidene fluoride (PVDF) were dispersed in the solvent N-methylpyrrolidone (NMP) and stirred continuously at room temperature until a uniform slurry was formed. The slurry was uniformly coated onto the surface of a titanium mesh and dried in a vacuum oven to obtain a titanium mesh coated with cathode powder, which was used as the anode of an electrolytic cell. A blank titanium mesh was used as the cathode, and an electrolyte solution was added to the electrolytic cell to construct a closed electrolytic system. An electric field-driven delithiation reaction was carried out under set process parameters. After the reaction was completed, the anode titanium mesh was placed in deionized water and ultrasonicated. The surface solid powder was collected, filtered, washed, and dried to obtain Ni-Co-Mn transition metal composite oxide powder (denoted as NCM-T).

[0017] The mass ratio of waste ternary cathode powder to binder is 50-80:1.

[0018] Step 3: In-situ preparation of catalyst for alcohol oxidation coupled with hydrogen production

[0019] The nickel foam was placed in ethanol and deionized water for ultrasonic cleaning for 10-20 minutes to remove surface oil and impurities, and then dried for later use.

[0020] The transition metal composite oxide powder obtained in step 2 was dispersed with iron salt in deionized water to prepare a homogeneous mixed solution.

[0021] The cleaned and dried nickel foam is completely immersed in the mixed solution and subjected to ultrasonic reaction, so that iron hydroxide grows in situ on the surface of transition metal composite oxide powder and is loaded onto the nickel foam substrate.

[0022] After the reaction was completed, the nickel foam was removed and naturally dried to obtain the supported composite catalyst, namely the alcohol oxidation coupled hydrogen production catalyst (denoted as FeOOH / NCM-T@NF).

[0023] Step 4: Lithium carbonate recovery

[0024] The remaining electrolyte after electrolysis in step 2 is filtered to remove impurities. The filtrate is evaporated and concentrated, and excess sodium carbonate powder is added and stirred at room temperature until the lithium salt is completely precipitated. The precipitate is collected by filtration, washed, and dried to obtain the lithium carbonate product.

[0025] Further, in step 2, the electrolyte solution is an aqueous solution of one or more of potassium sulfate, potassium carbonate, potassium hydroxide, sodium sulfate, sodium carbonate, sodium bicarbonate, and sodium hydroxide. The concentration of the solute in the electrolyte solution ranges from 0.2 to 4 mol / L.

[0026] Furthermore, in step 2, the process conditions for the electric field-driven lithium removal reaction are: applying a DC voltage of 3–15 V, a reaction temperature of 10–50 °C, and a reaction time of 3–12 h.

[0027] Further, in step 3, the iron salt is any one or a mixture of FeCl3·6H2O, Fe(NO3)3·9H2O, FeCl2·4H2O, FeSO4·7H2O, and Fe2(SO4)3.

[0028] Further, in step 3, the concentration of iron salt in the mixed solution is 0.01–0.2 mol / L, and the solid-liquid ratio of transition metal composite oxide powder to deionized water is 10–30 g / L.

[0029] Furthermore, in step 3, the process conditions for the ultrasonic reaction are: a reaction temperature of 20–50°C and a reaction time of 2–4 h.

[0030] Furthermore, in step 4, the evaporation concentration and drying temperatures are both 60–80°C.

[0031] This invention further provides the application of the obtained FeOOH / NCM-T@NF catalyst in the electrocatalytic alcohol oxidation coupled hydrogen production reaction. Specifically, the catalyst can be used as the working electrode, a platinum sheet as the counter electrode, and an Hg / HgO electrode as the reference electrode to construct a three-electrode electrocatalytic system. A KOH aqueous solution with a pH of 10-14 is used as the electrolyte, and a small molecule alcohol substrate with a concentration of ≥50 mmol / L is added to the electrolyte. An electrocatalytic reaction is carried out by applying voltage, thereby realizing the coupling of high-value chemical synthesis of alcohol oxidation at the anode and hydrogen evolution at the cathode.

[0032] Furthermore, the small molecule alcohol substrate is one or more of methanol, ethanol, ethylene glycol, benzyl alcohol, and glycerol.

[0033] Compared with existing technologies, this invention achieves the following significant technical effects through the synergistic design of electric field-driven delithiation and in-situ modification of iron hydroxide:

[0034] 1. Dual benefits of resource recycling and high-value conversion: On the one hand, it enables the targeted recovery of lithium from waste ternary cathode materials. By adding sodium carbonate for precipitation, filtration, washing and drying, high-purity lithium carbonate products can be obtained with a high lithium recovery rate. On the other hand, it converts transition metal components into high-performance electrocatalysts, avoiding the limitations of traditional recycling that only extracts low-value elemental metals. It enables the functional reuse of transition metals such as Ni, Co, and Mn, and significantly reduces dependence on primary mineral resources.

[0035] 2. Significantly Enhanced Catalytic Performance: The delithiation process induces abundant wrinkles and cracks in the transition metal composite oxide, significantly increasing its specific surface area compared to the original material, providing ample active sites for the catalytic reaction. Simultaneously, the Ni in the transition metal composite oxide and the in-situ grown FeOOH form a strong synergistic catalytic effect, significantly improving conductivity and alcohol adsorption activation capacity. The prepared catalyst exhibits excellent performance in the electrocatalytic oxidation of benzyl alcohol at 10 mA cm⁻¹. -2 The potential at the current density is only 1.332 V, which is more than 66 mV lower than that of the traditional oxygen evolution reaction. Moreover, it can be stably electrolyzed for more than 25 hours, and no significant change in the working voltage was found, which shows good stability.

[0036] 3. Synergistic effect of reduced energy consumption and high-value products: Replacing the anodic oxygen evolution reaction of traditional water cracking with electrocatalytic alcohol oxidation not only reduces the total energy consumption of hydrogen production, but also simultaneously produces high-value-added organic chemicals such as benzoic acid and acetic acid. The products have high purity, achieving synergistic benefits of energy conversion and fine chemical product synthesis, and significantly enhancing the economic value of the technology.

[0037] 4. The process is green, efficient, and easy to industrialize: The entire preparation process does not require harsh conditions such as high-temperature calcination or deep leaching with strong acids and alkalis. The reaction temperature is controlled between 10 and 80°C. The process is simple and highly operable. The electrolyte can be recycled, and no toxic or harmful waste is generated, which meets the requirements of green chemical development. The raw materials used are recycled products of waste batteries, which are inexpensive. Moreover, the process parameters of each step are easy to control, which facilitates large-scale production and application. Attached Figure Description

[0038] Figure 1 NCM8866-T (prepared for Example 1 of this invention) Figure 1 a) and FeOOH / NCM8866-T@NF ( Figure 1 b) Scanning electron microscope image of the catalyst;

[0039] Figure 2 Linear potential scans of the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention in KOH electrolyte containing benzyl alcohol and KOH electrolyte without benzyl alcohol.

[0040] Figure 3 Linear potential scans of the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention, and Fe@NF, NCM8866-T@NF, and blank NF as comparisons, in 1 M KOH + 0.1 M benzyl alcohol;

[0041] Figure 4 This is a photograph of the product obtained after the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention has undergone a catalytic reaction.

[0042] Figure 5 The X-ray diffraction pattern of the product obtained after catalysis by the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention;

[0043] Figure 6 The infrared spectrum of the product obtained after the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention is shown.

[0044] Figure 7 The stability test diagram is shown for the FeOOH / NCM8866-T@NF catalyst prepared in Example 1 of this invention.

[0045] Figure 8 Linear potential scans of FeOOH / NCM8866-T@NF prepared in Example 1 of this invention in KOH electrolyte containing ethanol and KOH electrolyte without ethanol;

[0046] Figure 9 Linear potential scans of FeOOH / NCM8866-T@NF prepared in Example 1 of this invention in KOH electrolyte containing ethylene glycol and KOH electrolyte without ethylene glycol. Detailed Implementation

[0047] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments and accompanying drawings, further clarifies the invention. It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0048] Example 1

[0049] In this embodiment, the FeOOH / NCM8866-T@NF catalyst was prepared using the following method:

[0050] Step 1: Pretreatment of waste ternary cathode materials

[0051] Selected ternary cathode sheets (LiNi) from waste lithium-ion batteries 0.88 Co 0.06 Mn 0.06 O2), after being disassembled and stripped to remove the current collector and separator, and after impurities are removed, it is ground in a ball mill for 30 min and dried at 80℃ for 6 h to obtain waste ternary cathode powder LiNi. 0.88 Co 0.06 Mn 0.06 O2 (denoted as NCM8866).

[0052] Step 2: Preparation of electric field-driven delithiation and transition metal composite oxide powder

[0053] First, the polyvinylidene fluoride adhesive is placed in a stirring flask, and NMP solvent is added dropwise and stirred for 30 minutes until it becomes transparent. Then, the ground LiNi is added. 0.88 Co 0.06 Mn 0.06 O2, continue magnetic stirring at room temperature for 12 h to form a homogeneous slurry. LiNi 0.88 Co 0.06 Mn 0.06 The mass ratio of O2 to polyvinylidene fluoride adhesive is 75:1, per 0.6 g LiNi 0.88 Co 0.06 Mn 0.06 O2 was added dropwise with 0.5 mL of NMP solvent; the slurry was then uniformly coated onto the surface of a 6 cm × 8 cm titanium mesh, with a coating area of ​​4 cm × 6 cm. Each titanium mesh sheet contained approximately 0.6 g of LiNi. 0.88 Co 0.06 Mn 0.06 O2 cathode powder was dried in a vacuum oven at 60℃ for 12 h to obtain a titanium mesh (anode) coated with cathode powder; using a blank titanium mesh of the same size as the cathode, 150 mL of 0.2 mol / L K2SO4 aqueous solution was added to the electrolytic cell as the electrolyte solution to construct a closed electrolytic system.

[0054] The electric field-driven delithiation process parameters were set as follows: DC voltage of 5 V, reaction temperature of 25℃, and continuous electrolysis for 3 h. After the electrolysis reaction was completed, the anode titanium mesh was removed and placed in deionized water for sonication for 2 h. The material separated from the titanium mesh was collected, filtered, and washed three times to remove residual salt ions. It was then dried at 80℃ for 12 h to obtain the delithiation product—Ni-Co-Mn transition metal composite oxide powder (denoted as NCM8866-T).

[0055] Step 3: In-situ preparation of composite catalyst

[0056] Take nickel foam (NF, size 1 cm × 1 cm), and ultrasonically clean it for 15 min each in ethanol and deionized water to remove surface oil and impurities. Dry it in an oven at 60℃ for later use. Weigh 90 mg of NCM8866-T powder and 139 mg of FeSO4·7H2O, add them to 5 mL of deionized water, and prepare a homogeneous mixed solution.

[0057] The cleaned and dried nickel foam was completely immersed in the above mixed solution and placed in a constant temperature water bath at 30°C for ultrasonic reaction for 2 h. After the reaction was completed, the nickel foam was removed and allowed to dry naturally at room temperature for 48 h to obtain the FeOOH / NCM8866-T@NF composite catalyst.

[0058] Step 4: Lithium carbonate recovery

[0059] The remaining electrolyte after electrolysis is filtered to remove impurities. The filtrate is evaporated and concentrated to 1 / 3 of its original volume at 60°C. Excess sodium carbonate powder is slowly added and stirred at room temperature to allow the lithium salt to precipitate completely. The precipitate is collected by filtration, washed with deionized water, and dried at 60°C to obtain the lithium carbonate product.

[0060] The catalyst obtained in this embodiment was subjected to the following performance tests and characterization:

[0061] (1) Morphological and structural characterization

[0062] The NCM8866-T and FeOOH / NCM8866-T@NF were characterized using scanning electron microscopy (SEM), and the results are as follows: Figure 1 As shown:

[0063] Figure 1 The results show that the structure of the waste NCM8866 material undergoes significant changes after electrolytic delithiation: a large number of cracks and wrinkles appear on the surface, and the specific surface area is greatly increased, providing sufficient surface space and active sites for the subsequent in-situ growth of FeOOH.

[0064] Figure 1 b shows that FeOOH is grown in situ on the surface of NCM8866-T, forming a uniformly distributed layered or lamellar structure with slight warping or bending between the layers, resulting in a compact and interwoven structure. These lamellar structures have smooth and uniform surfaces, exhibiting micron-scale lamellar stacking, which enhances the specific surface area of ​​the material and creates more active sites and reaction interfaces. Through this layered structure, FeOOH not only improves the efficiency of the catalytic reaction but also optimizes conductivity and reactant diffusion channels. This structure significantly improves the contact between the material and the electrolyte, enhancing reaction kinetics. Particularly in the electrocatalytic oxidation of benzyl alcohol, the FeOOH / NCM8866-T@NF composite catalyst exhibits excellent electrocatalytic performance, providing crucial support for efficient electrochemical conversion.

[0065] (2) Electrocatalytic performance test of benzyl alcohol

[0066] A three-electrode electrocatalytic system was constructed using FeOOH / NCM8866-T@NF as the working electrode, a platinum sheet as the counter electrode, and Hg / HgO as the reference electrode. The electrolyte was a 1 M (1 mol / L) KOH aqueous solution, and two electrolyte solutions were prepared: one without benzyl alcohol and the other containing 0.1 M benzyl alcohol. Before electrochemical testing, saturated nitrogen gas was introduced to remove oxygen from the solution, and linear scan voltammetry (LSV) was performed at room temperature at a scan rate of 5 mV / s. The results are as follows: Figure 2As shown: Without benzyl alcohol, the catalyst reaches 10 mA cm⁻¹. -2 The potential required for the current density is 1.398 V (corresponding to the oxygen evolution reaction, OER). After adding 0.1 M benzyl alcohol, the potential to achieve the same current density drops to 1.332 V, which is 66 mV lower than the OER potential, proving that the electrocatalytic oxidation of benzyl alcohol significantly reduces the energy consumption of the hydrogen production system.

[0067] To verify the superiority of the catalyst, the LSV performance of FeOOH / NCM8866-T@NF was compared with that of Fe@NF (nickel foam with only iron hydroxide loading), NCM8866-T@NF (transition metal composite oxide without iron hydroxide loading), and blank NF in a 1 M KOH + 0.1 M benzyl alcohol solution. The results are as follows: Figure 3 As shown: at 100 mA cm -2 At the current density, the potential of FeOOH / NCM8866-T@NF is only 1.410 V, which is much lower than that of Fe@NF (1.512 V), NCM8866-T@NF (1.564 V) and blank NF (1.627 V), demonstrating the synergistic catalytic effect of Ni-Co-Mn transition metal composite oxide and FeOOH.

[0068] The preparation methods for Fe@NF and NCM8866-T@NF are the same as those for FeOOH / NCM8866-T@NF, except that the amounts of NCM8866-T powder and FeSO4·7H2O in step 3 are adjusted to 0.

[0069] (3) Product and stability verification

[0070] The electrolyte following the FeOOH / NCM8866-T@NF electrocatalytic reaction was acidified with excess concentrated hydrochloric acid, recrystallized at room temperature, purified by filtration, and dried under vacuum at 60°C for 8 h to obtain a white solid product. Its appearance, XRD, and FTIR characteristics were then analyzed, and the results are as follows: Figure 4 , Figure 5 , Figure 6 As shown: In the XRD pattern, the diffraction peaks of the product perfectly match those of the standard XRD card for benzoic acid (JCPDS No. 12-0853), with no extraneous peaks appearing; in the FTIR pattern, at 1676 cm⁻¹... -1 1323 cm -1 A characteristic peak of C=O stretching vibration appears at 2882 cm⁻¹. -1 2833 cm -1 2710 cm -1 2671 cm -1 2610 cm -1 2557 cm-1 The characteristic peak of OH stretching vibration appears at 3650–3590 cm⁻¹. -1 The absence of characteristic absorption peaks of alcohol hydroxyl groups in the range is consistent with the standard infrared spectrum of benzoic acid, proving that the anode product is high-purity benzoic acid.

[0071] Using FeOOH / NCM8866-T@NF as the working electrode, in a 1 M KOH + 0.1 M benzyl alcohol electrolyte, at a current density j = 10 mA cm⁻¹ -2 The timing potential test was performed, and the results are as follows: Figure 7 As shown, the catalyst operated stably for more than 25 hours without significant changes in the operating voltage, demonstrating excellent electrochemical stability.

[0072] (4) Electrocatalytic performance testing of ethanol and ethylene glycol

[0073] A three-electrode electrocatalytic system was constructed using FeOOH / NCM8866-T@NF as the working electrode, a platinum sheet as the counter electrode, and Hg / HgO as the reference electrode. Before electrochemical testing, saturated nitrogen gas was introduced to remove oxygen from the solution, and linear scan voltammetry was performed at a scan rate of 5 mV / s at room temperature.

[0074] The electrolyte was a 1 M KOH aqueous solution. Two electrolyte solutions were prepared, one without ethanol and the other containing 1 M ethanol. The test results are as follows. Figure 8 As shown: Without ethanol, the catalyst reaches 100 mA cm⁻¹. -2 The potential required for the current density was 1.464 V; after adding 1M ethanol, the potential to achieve the same current density dropped to 1.380 V, which is 84 mV lower than the OER potential, proving that the electrocatalytic ethanol oxidation reaction effectively reduced the energy required for hydrogen production by water electrolysis and optimized the overall energy efficiency.

[0075] The electrolyte was a 1 M KOH aqueous solution. Two electrolyte solutions were prepared: one without ethylene glycol and the other containing 0.5 M ethylene glycol. The test results are as follows. Figure 9 As shown: Without ethylene glycol, the catalyst reaches 100 mA cm⁻¹. -2 The potential required for the current density was 1.464 V; after adding 0.5 M ethylene glycol, the potential to achieve the same current density dropped to 1.389 V, which is 75 mV lower than the OER potential. This proves that the electrocatalytic oxidation of ethylene glycol significantly improves the energy efficiency of the water electrolysis hydrogen production system and reduces the required voltage.

[0076] The above results show that the FeOOH / NCM8866-T@NF catalyst also exhibits excellent oxidation performance for alcohols such as ethanol and ethylene glycol, further demonstrating its wide applicability in various alcohol oxidation reactions, and can significantly reduce energy consumption and improve reaction efficiency in hydrogen production processes.

[0077] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material, characterized in that, Includes the following steps: Step 1: Pretreatment of waste ternary cathode materials Waste lithium-ion battery ternary cathode sheets are pretreated to obtain waste ternary cathode powder LiNi. x Co y Mn 1-x-y O2, where x>0, y>0, 1-xy>0; Step 2: Preparation of electric field-driven delithiation and transition metal composite oxide powder The waste ternary cathode powder and the binder polyvinylidene fluoride were dispersed in the solvent N-methylpyrrolidone and stirred continuously at room temperature until a uniform slurry was formed. The slurry was uniformly coated onto the surface of a titanium mesh and dried in a vacuum oven to obtain a titanium mesh coated with cathode powder, which was used as the anode of the electrolytic cell. A blank titanium mesh was used as the cathode. An electrolyte solution was added to the electrolytic cell to construct a closed electrolytic system and carry out an electric field-driven delithiation reaction. After the reaction, the anode titanium mesh was placed in deionized water and ultrasonicated. The surface solid powder was collected, filtered, washed, and dried to obtain Ni-Co-Mn transition metal composite oxide powder, denoted as NCM-T. The electrolyte solution was an aqueous solution of one or more of potassium sulfate, potassium carbonate, potassium hydroxide, sodium sulfate, sodium carbonate, sodium bicarbonate, and sodium hydroxide, with the concentration of solute in the electrolyte solution ranging from 0.2 to 4 mol / L. The process conditions for the electric field-driven delithiation reaction were: applied DC voltage of 3 to 15 V, reaction temperature of 10 to 50 °C, and reaction time of 3 to 12 h. Step 3: In-situ preparation of catalyst for alcohol oxidation coupled with hydrogen production The nickel foam was ultrasonically cleaned in ethanol and deionized water in sequence to remove surface oil and impurities, and then dried for later use. The transition metal composite oxide powder obtained in step 2 was dispersed with iron salt in deionized water to prepare a homogeneous mixed solution. The cleaned and dried nickel foam is completely immersed in the mixed solution and subjected to ultrasonic reaction, so that iron hydroxide grows in situ on the surface of transition metal composite oxide powder and is loaded onto the nickel foam substrate. After the reaction was completed, the nickel foam was removed and naturally dried to obtain the supported composite catalyst, namely the alcohol oxidation coupled hydrogen production catalyst, denoted as FeOOH / NCM-T@NF; Step 4: Lithium carbonate recovery The remaining electrolyte after electrolysis in step 2 is filtered to remove impurities. The filtrate is evaporated and concentrated, and excess sodium carbonate powder is added and stirred at room temperature until the lithium salt is completely precipitated. The precipitate is collected by filtration, washed, and dried to obtain the lithium carbonate product.

2. The method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material according to claim 1, characterized in that, In step 1, the waste ternary cathode powder LiNi x Co y Mn 1-x-y O2 is LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.88 Co 0.06 Mn 0.06 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 1 / 3Co 1 / 3 Mn 1 / 3 At least one of O2.

3. The method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material according to claim 1, characterized in that, In step 3, the iron salt is any one or a mixture of FeCl3·6H2O, Fe(NO3)3·9H2O, FeCl2·4H2O, FeSO4·7H2O, and Fe2(SO4)3.

4. The method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material according to claim 1, characterized in that, In step 3, the concentration of iron salt in the mixed solution is 0.01–0.2 mol / L, and the solid-liquid ratio of transition metal composite oxide powder to deionized water is 10–30 g / L.

5. The method for preparing an alcohol oxidation coupled hydrogen production catalyst using waste ternary cathode material according to claim 1, characterized in that, In step 3, the process conditions for the ultrasonic reaction are: reaction temperature of 20-50℃ and reaction time of 2-4h.

6. A FeOOH / NCM-T@NF catalyst prepared by the method according to any one of claims 1 to 5.

7. The application of the FeOOH / NCM-T@NF catalyst according to claim 6 in the electrocatalytic alcohol oxidation coupled hydrogen production reaction.

8. The application according to claim 7, characterized in that: Using the catalyst as the working electrode, a platinum sheet as the counter electrode, and an Hg / HgO electrode as the reference electrode, a three-electrode electrocatalytic system was constructed. A KOH aqueous solution with a pH of 10–14 was used as the electrolyte, and a small molecule alcohol substrate with a concentration ≥50 mmol / L was added to the electrolyte. An electrocatalytic reaction was carried out by applying voltage, thereby achieving the coupling of high-value chemical synthesis through anodic alcohol oxidation and cathodic hydrogen evolution.

Citation Information

Patent Citations

  • Method for comprehensive recovery and reutilization of waste ternary electrode material

    CN108808150A

  • Method combining waste ternary positive electrode material recovery and electrochemical hydrogen production

    CN112680596A