Manufacturing method of selective chemical nickel ceramic-based printed circuit board for power module
By employing a double-layer film application and laser windowing method in the selective electroless nickel plating process, the problems of nickel layer yellowing and copper surface oxidation are solved, achieving protection of the nickel layer and improved solderability of the copper surface, making it suitable for high-end applications of ceramic-based printed circuit boards.
Patent Information
- Application Number
- CN202511757808.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-27
- Publication Date
- 2026-03-20
AI Technical Summary
Existing selective electroless nickel plating processes suffer from problems such as nickel layer yellowing and copper surface oxidation. In particular, the nickel layer is prone to oxidation during subsequent acid and alkali treatment, which affects the product's appearance and weldability.
The process employs two protective film applications and two laser windowing techniques. The second film application physically isolates the electroless nickel layer from the acid and alkali solutions, while the precise laser windowing technology ensures that the nickel layer does not come into contact with the acid and alkali solutions during subsequent processing, thus preventing oxidation.
It effectively solves the problem of nickel layer yellowing, ensures the appearance and welding performance of the nickel layer, improves the solderability of the copper surface, and has a simple and efficient process that is suitable for different substrate types and meets the reliability requirements of high-end power modules.
Smart Images

Figure CN121711897A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic-based printed circuit boards for power modules, and specifically to a method for manufacturing a selective nickel-coated ceramic-based printed circuit board for power modules. Background Technology
[0002] Ceramic copper-clad substrates (such as DBC and AMB) are core components of power modules, and their surface treatment processes directly affect the module's reliability and lifespan. Electroless nickel plating is widely used for surface protection of ceramic substrates due to its excellent corrosion resistance and solderability.
[0003] To achieve different functions, selective electroless nickel plating is required on ceramic substrates. Existing technologies include various methods for selective electroplating or electroless plating on substrates. For example, Chinese patent application CN119095271A discloses a "Method for Electroplating Nickel-Gold onto Copper-Clad Ceramic Substrates," which employs a process of electroplating followed by etching: first, a first coating (exposure and development) is performed on a complete copper surface to define the area to be plated; then, electroplating is performed to form a thicker metal coating; next, the coating is removed and a second coating is performed to define the retention area; finally, wet etching is used to form the final circuitry.
[0004] However, this existing technology has the following limitations: First, its core is electroplating, suitable for scenarios requiring thicker plating layers and subsequent etching to form circuits. Second, the purpose of the second coating is to protect the plating layer and part of the copper surface during the etching step, preventing corrosion by the etching solution. This method completely fails to solve a unique and challenging problem faced in electroless nickel plating: after selective electroless nickel plating, the exposed copper surface needs cleaning and anti-oxidation treatment, a process that requires the use of acidic and alkaline solutions. The plated electroless nickel layer is extremely sensitive; once it comes into contact with these acidic and alkaline solutions, the surface will quickly oxidize, yellow, and darken, severely damaging the product's appearance and degrading its solderability. The protective film in CN119095271A is only used to resist the etching solution and does not address, nor can it solve, the problem of the electroless nickel layer yellowing due to contact with acids and alkalis during subsequent copper surface treatment. In addition, existing selective electroless nickel plating processes also generally suffer from the problem of easy oxidation of the copper surface during processing, leading to a decrease in solderability. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art by providing a method for manufacturing a selective electroless nickel ceramic-based printed circuit board for power modules. This method, through a unique process design, fundamentally solves the technical problems of nickel layer yellowing and copper surface oxidation in selective electroless nickel plating.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is: a method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module, comprising the following steps: S1. Provide a ceramic-based copper-clad laminate and fabricate the circuit diagram; S2. A first protective film is attached to the surface of the circuit lines; S3. Perform the first laser windowing to remove the first protective film on the area to be electroless nickel plating, exposing the copper surface in that area. S4. Perform chemical nickel plating on the exposed copper surface to form a nickel layer; S5. After completing the electroless nickel plating, remove the first protective film; S6. A second protective film is applied to the entire surface of the circuit lines; S7. Perform a second laser windowing to remove the second protective film on the copper surface area to be treated, exposing the copper surface in that area, while the nickel layer formed by the chemical nickel plating is completely covered by the second protective film. S8. Perform anti-oxidation treatment on the exposed copper surface in step (S7). This treatment process involves the use of acid and alkali solutions. The nickel layer is covered by a second protective film and does not come into contact with the acid and alkali solutions. S9. Remove the second protective film.
[0007] Preferably, the ceramic-based copper-clad laminate is a direct copper-clad substrate or an active metal brazing substrate.
[0008] Preferably, when the ceramic-based copper-clad laminate is an active metal brazing substrate, after step S1 and before step S2, the step further includes: using an etching solution to etch the solder layer at the line trench to expose the ceramic.
[0009] Preferably, before step S2, the process further includes degreasing, micro-etching, and a first anti-oxidation treatment of the board on which the circuit lines are fabricated.
[0010] Preferably, the thickness of the nickel layer formed in step S4 is 2.5~6μm.
[0011] Preferably, in step S8, the anti-oxidation treatment includes degreasing, micro-etching, pickling, and anti-oxidation agent treatment performed sequentially; and the second protective film is removed after the pickling step and before the anti-oxidation agent treatment.
[0012] Preferably, both the first protective film and the second protective film are acid and alkali resistant dry films.
[0013] Preferably, after step S9, the product is further subjected to a laser cutting step, with a cutting depth of 30% to 40% of the thickness of the ceramic substrate.
[0014] The key innovation of this invention lies in the synergistic application of two protective film applications and two laser windowing processes, especially the second film application and windowing. Its purpose is not for circuit etching, but specifically to physically isolate the completed and sensitive electroless nickel layer from the acid and alkaline solutions during the specific process of copper surface anti-oxidation treatment. This targeted protective measure is unprecedented in existing technologies and successfully solves the long-standing industry problem of nickel layer yellowing.
[0015] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art: 1. It innovatively solves the problem of nickel layer yellowing: by applying a second film to precisely protect the nickel layer, it is isolated from all subsequent copper surface treatment processes involving acid and alkali solutions, fundamentally eliminating the root cause of nickel layer yellowing and ensuring the appearance and solderability of the nickel layer.
[0016] 2. Effectively ensures the solderability of the copper surface: By applying anti-oxidation treatment to the copper surface before and after nickel plating, combined with local protection of the protective film, the high cleanliness and excellent solderability of the final exposed copper surface are ensured.
[0017] 3. Precise and efficient process: Laser windowing has high precision and good flexibility, making it particularly suitable for selective processing of pre-formed fine lines. Compared with exposure and development processes, the process is simpler, requires no film, and has strong adaptability.
[0018] 4. High compatibility and reliability: This method is applicable to both DBC and AMB substrates, and can perform solder etching on AMB substrates. The final product exhibits corrosion resistance in the nickel areas and good solderability in the copper areas, with overall reliability meeting the requirements of high-end power modules. Attached Figure Description
[0019] The technical solution of the present invention will be further described below with reference to the accompanying drawings: Appendix Figure 1 This is a flowchart of a method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to the present invention; Appendix Figure 2 This is a cross-sectional view of a circuit board manufactured in accordance with the present invention. Appendix Figure 3 This is a cross-sectional view of the circuit board obtained in Embodiment 2 of the present invention; Appendix Figure 4 This is a cross-sectional view of the circuit board obtained by implementing the three-stage process in this invention.
[0020] The components are: 1. Ceramic substrate; 2. Copper; 3. Nickel layer. Detailed Implementation
[0021] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments. Example
[0022] This embodiment uses an AMB silicon nitride ceramic substrate as an example, with selective electroless nickel plating on one side. The fabrication process is as follows: S1. Circuit supply: The ceramic substrate 1 and copper 2 are combined through the AMB process to form a double-sided copper-clad ceramic substrate, and the preset circuit lines are produced by exposure, development and etching.
[0023] S2. Solder Etching: Using a special acidic etching solution, residual solder in the trenches between circuits is etched to expose the ceramic.
[0024] S3. First Anti-oxidation Treatment: The board is degreased, micro-etched, and acid-washed, and then dipped in BTA (benzotriazole) anti-oxidation agent to protect the copper surface.
[0025] S4. First Film Application and Laser Windowing: Apply acid and alkali resistant dry film to both sides of the board as the first protective film. Use an ultraviolet laser to create windows in the areas requiring selective electroless nickel plating on the board, and then peel off the film layer in those areas to expose the copper surface.
[0026] S5. Electroless nickel plating: The plate is immersed in an electroless nickel-phosphorus alloy plating solution, and a nickel layer with a thickness of 4.0±0.5μm is deposited on the copper surface exposed on one side.
[0027] S6. Post-nickelization treatment and film removal: After neutralization with dilute sulfuric acid, washing with water, and drying, the first protective film on both sides is removed.
[0028] S7. Second Film Application and Laser Windowing: Apply a second protective film (acid and alkali resistant dry film) to the selectively electroless nickel-plated surface. Use a laser to create windows in the copper areas requiring final treatment and peel off the film to expose the copper surface. At this point, all electroless nickel-plated areas on one side are tightly covered by the second protective film; the other side of the board, lacking the second protective film, directly exposes the entire copper surface.
[0029] S8. Second Anti-oxidation Treatment: The board undergoes degreasing, micro-etching, and dilute sulfuric acid pickling. Key steps: After pickling, the board is first removed and rinsed with water. The second protective film on the selectively electroless nickel plating surface is then removed, and the exposed copper surface is immersed in BTA anti-oxidation solution. This sequence ensures that the nickel layer is completely protected during the pickling stage, with no chemical residue, resulting in a circuit board with the cross-section shown below. Figure 2 As shown.
[0030] S9. Laser Cutting and Inspection: Perform laser cutting to a depth of 35% of the ceramic thickness, followed by final inspection.
[0031] The product prepared by this method has a uniform silver-white electroless nickel layer with no signs of yellowing; the copper surface is bright and has excellent solderability. Example
[0032] The difference from Example 1 is that double-sided selective electroless nickel plating is used, and its fabrication process is as follows: S1. Circuit supply: The ceramic substrate 1 and copper 2 are combined through the AMB process to form a double-sided copper-clad ceramic substrate, and the preset circuit lines are produced by exposure, development and etching.
[0033] S2. Solder Etching: Using a special acidic etching solution, residual solder in the trenches between circuits is etched to expose the ceramic.
[0034] S3. First Anti-oxidation Treatment: The board is degreased, micro-etched, and acid-washed, and then dipped in BTA (benzotriazole) anti-oxidation agent to protect the copper surface.
[0035] S4. First Film Application and Laser Windowing: Apply acid and alkali resistant dry film to both sides of the board as the first protective film. Use an ultraviolet laser to create windows in the areas on both sides where chemical nickel plating is required, and then peel off the film layer in those areas to expose the copper surface.
[0036] S5. Electroless nickel plating: The plate is immersed in an electroless nickel-phosphorus alloy plating solution, and a nickel layer with a thickness of 3.5±0.5μm is deposited on the exposed copper surfaces on both sides.
[0037] S6. Post-nickelization treatment and film removal: After neutralization with dilute sulfuric acid, washing with water, and drying, the first protective film on both sides is removed.
[0038] S7. Second Protective Film Application and Laser Windowing: Apply a second protective film (acid and alkali resistant dry film) to both sides. Use a laser to create windows in the copper surface areas requiring final treatment and peel off the film to expose the copper surface. At this point, all areas of the electroless nickel layer on both sides are completely covered by the second protective film.
[0039] S8. Second Anti-oxidation Treatment: The board undergoes degreasing, micro-etching, and dilute sulfuric acid pickling. Key steps: After pickling, the board is first removed and rinsed with water, then all the second protective films on both sides are peeled off. Next, it is immersed in BTA anti-oxidation solution to treat the exposed copper surface. This sequence ensures that the nickel layer is completely protected during the pickling stage, with no chemical residue, resulting in a circuit board with the cross-section shown below. Figure 3 As shown.
[0040] S9. Laser Cutting and Inspection: Perform laser cutting to a depth of 35% of the ceramic thickness, followed by final inspection.
[0041] The beneficial effects of this embodiment are: it proves that the method of the present invention can efficiently and synchronously process double-sided circuits, and can ensure that the nickel layers on both sides are effectively protected in the copper surface processing process, avoiding cross-contamination and inconsistent quality problems that may occur in double-sided processing. Example
[0042] The difference from Examples 1 and 2 is that the ceramic copper-clad laminate is prepared using the DBC process, with one side being electroless nickel plated on the entire surface and the other side being selectively electroless nickel plated, such as... Figure 1 As shown, its production process is as follows: S1. Circuit supply: The ceramic substrate 1 and copper 2 are combined through the DBC process to form a double-sided copper-clad ceramic substrate, and the preset circuit lines are produced by exposure, development and etching.
[0043] S2. First Film Application and Laser Windowing: Apply an acid- and alkali-resistant dry film as the first protective film to the selective electroless nickel plating surface of the board. Use an ultraviolet laser to create windows in the areas of the selective electroless nickel plating surface that require electroless nickel plating, and peel off the film layer in those areas to expose the copper surface; the other side, since it is fully nickel plated, does not require the first protective film, exposing the entire copper surface.
[0044] S3, Electroless Nickel Plating: The plate is immersed in an electroless nickel-phosphorus alloy plating solution, and a nickel layer with a thickness of 4.5±0.5μm is deposited on the exposed copper surfaces on both sides.
[0045] S4. Post-nickel plating treatment and film removal: After neutralization with dilute sulfuric acid, washing with water, and drying, the first protective film on the selective electroless nickel plating surface is removed.
[0046] S5. Second Film Application and Laser Windowing: Apply a second protective film (acid and alkali resistant dry film) to both sides. For the selective electroless nickel plating surface, use a laser to create windows in the copper areas requiring final treatment and peel off the film, exposing the copper surface. At this point, all electroless nickel plating areas on both sides are completely covered by the second protective film.
[0047] S6. Second Anti-oxidation Treatment: The board undergoes degreasing, micro-etching, and dilute sulfuric acid pickling. Key steps: After pickling, the board is first removed and rinsed with water, the double-sided second protective film is peeled off, and then it is immersed in BTA anti-oxidation solution to treat the exposed copper surface. This sequence ensures that the nickel layer is completely protected during the pickling stage, with no chemical residue, resulting in a circuit board with a cross-section as shown. Figure 4 As shown.
[0048] S7. Laser Cutting and Inspection: Perform laser cutting to a depth of 35% of the ceramic thickness, followed by final inspection.
[0049] The beneficial effects of this embodiment are: it demonstrates the excellent flexibility of the method of the present invention, and can cope with complex situations where different surface treatment requirements exist on the front and back sides of the same substrate. Through precise control of double film application and laser windowing, the process of "full treatment on one side and selective treatment on the other side" is perfectly realized, meeting the diverse needs when the substrate is connected to different components (such as chips and casings) in the power module.
[0050] The above are merely specific application examples of the present invention and do not constitute any limitation on the scope of protection of the present invention. All technical solutions formed by equivalent transformations or substitutions fall within the scope of protection of the present invention.
Claims
1. A method for fabricating a power module using a selective electroless nickel ceramic-based printed circuit board, characterized in that: Includes the following steps: S1. Provide a ceramic-based copper-clad laminate and fabricate the circuit diagram; S2. A first protective film is attached to the surface of the circuit lines; S3. Perform the first laser windowing to remove the first protective film on the area to be electroless nickel plating, exposing the copper surface in that area. S4. Perform chemical nickel plating on the exposed copper surface to form a nickel layer; S5. After completing the electroless nickel plating, remove the first protective film; S6. A second protective film is applied to the entire surface of the circuit lines; S7. Perform a second laser windowing to remove the second protective film on the copper surface area to be treated, exposing the copper surface in that area, while the nickel layer formed by the chemical nickel plating is completely covered by the second protective film. S8. Perform anti-oxidation treatment on the exposed copper surface in step (S7). This treatment process involves the use of acid and alkali solutions. The nickel layer is covered by a second protective film and does not come into contact with the acid and alkali solutions. S9. Remove the second protective film.
2. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 1, characterized in that: The ceramic-based copper-clad laminate is either a direct copper-clad substrate or an active metal brazing substrate.
3. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 2, characterized in that: When the ceramic-based copper-clad laminate is an active metal brazing substrate, after step S1 and before step S2, the step further includes: using an etching solution to etch the solder layer at the line trench to expose the ceramic.
4. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 3, characterized in that: Before step S2, the process also includes steps of degreasing, micro-etching, and first anti-oxidation treatment of the board on which the circuit lines are fabricated.
5. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 1, characterized in that: The thickness of the nickel layer formed in step S4 is 2.5~6μm.
6. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 1, characterized in that: In step S8, the anti-oxidation treatment includes degreasing, micro-etching, pickling, and anti-oxidation agent treatment performed sequentially; and after the pickling step and before the anti-oxidation agent treatment, the second protective film is removed first.
7. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 1, characterized in that: Both the first protective film and the second protective film are acid and alkali resistant dry films.
8. The method for manufacturing a selective electroless nickel ceramic-based printed circuit board for a power module according to claim 1, characterized in that: After step S9, the product is further subjected to laser cutting, with a cutting depth of 30% to 40% of the thickness of the ceramic substrate.
Citation Information
Patent Citations