Pickling passivation method for corrosion-resistant aluminum alloy strip
By using pickling and passivation solutions containing methanesulfonic acid, phytic acid, vanadium oxysulfate, and gallic acid, simultaneous pickling and passivation of aluminum alloy surfaces without fluorine or chromium was achieved. This solved the problems of insufficient bath stability and film performance, improved production efficiency and film performance, and met the conductivity and coating adhesion requirements of electronic appliances.
Patent Information
- Application Number
- CN202610152772.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-03
- Publication Date
- 2026-04-14
AI Technical Summary
In existing aluminum alloy surface treatment processes, zirconium-titanium passivation solutions require the addition of fluorides as etchants, which poses high risks and high costs. At the same time, the separation of traditional pickling and passivation processes leads to poor stability of the bath solution, making it difficult to apply stably in large-scale production. Furthermore, the chromium-free passivation film layer has insufficient corrosion resistance and conductivity.
The pickling and passivation solution, composed of methanesulfonic acid, phytic acid, vanadium sulfate, gallic acid, and glycolic acid, achieves simultaneous pickling and passivation through synergistic effects, forming a dense conversion film. This solves the problems of fluoride ion hazards and bath solution stability, and improves the corrosion resistance and conductivity of the film.
This process achieves fluorine-free and chromium-free pickling and passivation, extending the service life of the bath, improving production efficiency, and forming a self-healing conversion film that meets the conductivity requirements of electronic appliances and enhances the adhesion of the coating.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal surface treatment technology, specifically to a method for pickling and passivating corrosion-resistant aluminum alloy strip. Background Technology
[0002] Aluminum alloys are widely used in building decoration, automobile manufacturing, electronics, and new energy batteries due to their light weight, high specific strength, and excellent processing performance. However, aluminum alloys are chemically reactive and easily oxidize or corrode in air. Therefore, surface passivation treatment is usually required to form a conversion film, thereby improving the corrosion resistance of the substrate and providing good adhesion for subsequent coating processes.
[0003] While traditional chromate passivation processes offer excellent corrosion resistance and self-healing capabilities, hexavalent chromium is highly toxic and carcinogenic, and is subject to strict restrictions under EU RoHS and REACH regulations. Therefore, developing environmentally friendly chromium-free passivation technologies has become an inevitable trend in the industry. Currently, chromium-free passivation technologies on the market mainly include zirconium-titanium, silane, and rare-earth-based technologies. Among these, zirconium-titanium passivation solutions typically require the addition of fluorides (such as hydrofluoric acid and potassium fluorozirconate) as etchants to remove the natural oxide film on the aluminum alloy surface. However, fluoride ions pose a significant hazard, and the treatment of fluoride-containing wastewater is difficult and costly, still presenting certain environmental risks.
[0004] In actual production processes, existing aluminum alloy strip surface treatment typically treats pickling and passivation as two separate steps. This is because in acidic environments, the continuous dissolution of the aluminum substrate during production leads to a rapid increase in the aluminum ion concentration in the bath. In traditional sulfuric acid, phosphoric acid, or weak acid systems, accumulated aluminum ions are highly susceptible to hydrolysis, generating flocculent precipitates or slag, resulting in turbid baths, nozzle blockage, and severely affecting the uniformity of the passivation film. To maintain production, factories must frequently change the bath or discharge some waste liquid, which not only reduces production efficiency but also increases chemical consumption and waste liquid treatment burden. Although there are attempts in the industry to combine pickling and passivation processes, the insufficient tolerance of the bath to aluminum ions has made it difficult to stably apply in continuous large-scale production.
[0005] Furthermore, for aluminum alloys with complex compositions such as the 3-series, 5-series, or 6-series, the presence of alloying elements (such as magnesium, silicon, and copper) leads to uneven surface potential, making conversion film formation difficult or resulting in a loose film structure. While some existing chromium-free passivation films have improved the corrosion resistance of the bare film, they often suffer from excessive thickness or insufficient structural density, resulting in high surface contact resistance and failing to meet the conductivity requirements of electronic and electrical components. Alternatively, the film may lack active functional groups to react with organic coatings, causing reduced adhesion after coating and making it prone to coating peeling or filiform corrosion during use. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a pickling and passivation method for corrosion-resistant aluminum alloy strips. This method solves the problem that zirconium-titanium passivation solutions typically require the addition of fluorides as etchants to remove the natural oxide film on the aluminum alloy surface. However, fluoride ions pose a high risk, and the treatment of fluoride-containing wastewater is difficult and costly.
[0007] To achieve the above objectives, the present invention provides the following technical solution: Firstly, the present invention provides an acid pickling and passivation solution, employing the following technical solution: The pickling and passivation solution is prepared from the following raw materials in parts by weight: Methylsulfonic acid: 30-100 parts; Phytic acid: 2-15 parts; Vanadium oxysulfate: 5-15 parts; Gallic acid: 1-5 parts; Glycolic acid: 5-30 parts; Wetting agent: 0.5-2 parts; Deionized water: Remaining amount, bring the total to 1000 portions.
[0008] By adopting the above technical solution, this invention utilizes the chemical properties and synergistic effects of each component to achieve simultaneous pickling and passivation in a fluorine-free and chromium-free system. Its specific mechanism of action is as follows: Solubilizing and stabilizing effects of methanesulfonic acid: Methanesulfonic acid provides a strongly acidic environment to remove the natural oxide layer on the surface of aluminum alloys. Compared to sulfuric acid or phosphoric acid, the resulting aluminum methanesulfonate has excellent water solubility. During continuous production with increasing aluminum ion concentration, methanesulfonate ions can inhibit the hydrolysis and precipitation of aluminum salts, maintaining the homogeneous stability of the bath solution, thereby increasing the aluminum capacity and service life of the bath solution.
[0009] Synergistic film formation of phytic acid and vanadium oxysulfate: Phytic acid utilizes the phosphate groups in its molecules to chemically adsorb and chelate with the active sites on the surface of the aluminum substrate, forming an aluminum phytate underlayer; vanadium oxysulfate provides a vanadium source under acidic conditions, and vanadium ions fill the microporous structure of the phytic acid film layer, forming a vanadium-containing oxide barrier with redox activity, giving the film layer self-healing properties.
[0010] Crosslinking and sealing effects of gallic acid: The adjacent phenolic hydroxyl groups in the gallic acid molecule coordinate with vanadium and aluminum ions in the film layer to form an organic and inorganic crosslinked structure. This structure seals the lattice defects and micropores of the inorganic film layer, blocks the penetration of corrosive media, and utilizes organic functional groups to enhance the adhesion between the passivation film and subsequent coatings.
[0011] Glycolic acid reduction and auxiliary regulation: Glycolic acid creates a reducing atmosphere, stabilizes the existence of low-valence vanadium ions in the solution, and prevents them from oxidizing and becoming ineffective; at the same time, as an auxiliary pickling agent, glycolic acid can regulate the interfacial reaction rate and avoid excessive corrosion of aluminum due to excessive local acidity.
[0012] Preferably, the raw materials are in the following weight proportions: methanesulfonic acid: 55-65 parts; phytic acid: 4-6 parts; vanadium sulfate: 9-11 parts; gallic acid: 1.5-2.5 parts; glycolic acid: 12-18 parts; wetting agent: 0.8-1.2 parts; deionized water: balance, to a total of 1000 parts.
[0013] By employing the above technical solution and limiting the concentrations of each component within the aforementioned range, the acid etching rate and film formation rate can be balanced. Under this ratio, methanesulfonic acid rapidly exposes the fresh metal substrate without interfering with the deposition kinetics of phytic acid and vanadium ions, thus achieving optimal overall performance in terms of film weight, corrosion resistance, and conductivity.
[0014] Preferably, the wetting agent is selected from one or more of fatty alcohol polyoxyethylene ether, sodium alkyl sulfonate, or fluorocarbon surfactant.
[0015] By adopting the above technical solution, the wetting agent can reduce the surface tension of the pickling and passivation solution, promote the rapid spread of the solution on the surface of the aluminum alloy strip, avoid pitting or stripe defects caused by uneven wetting, and improve the uniformity of the film layer.
[0016] Preferably, the pH value of the pickling and passivation solution is controlled below 1.
[0017] By adopting the above technical solution, maintaining the pH value below 1 ensures sufficient acid etching kinetics, enabling the rapid removal of oxide scale from the substrate surface; the high acidity environment also inhibits the bulk precipitation of the bath solution itself, promoting the film-forming reaction to mainly occur at the metal or solution interface with a relatively high pH value, thereby obtaining a conversion film with strong adhesion.
[0018] Secondly, this invention provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, employing the following technical solution: A method for pickling and passivating corrosion-resistant aluminum alloy strip includes the following steps: The surface of the aluminum alloy strip is degreased and cleaned to remove surface oil and then washed with water. The aluminum alloy strip that has undergone degreasing and cleaning is brought into contact with the pickling and passivation solution described in the first aspect above to react; Clean the surface of the aluminum alloy strip after it has been treated with pickling and passivation solution by deionized water. The cleaned aluminum alloy strip is then heated and dried.
[0019] By adopting the above technical solution, the interfacial chemical reaction process in the contact step between the aluminum alloy strip and the pickling and passivation solution is as follows: Interface etching: The pickling and passivation solution comes into contact with the aluminum alloy surface, and the high concentration of hydrogen ions reacts with the surface alumina and the aluminum substrate (2Al + 6H₂O). + →2Al 3+ +3H2), which leads to a local increase in pH value at the metal or solution interface.
[0020] Film deposition: As the pH value at the interface increases, the solubility of phytate ions and vanadium ions in the solution decreases, and they preferentially precipitate at the active sites to form a primary film layer of aluminum phytate and hydrated vanadium oxide.
[0021] Coordination blocking: Gallic acid molecules in the solution are adsorbed on the surface and pores of the primary film layer and undergo coordination reactions with metal ions in the deposit.
[0022] Dynamic equilibrium: Methylsulfonic acid continuously dissolves the detached oxide scale and dissolved aluminum ions, preventing reaction products from accumulating at the interface and maintaining the dynamic equilibrium of etching and film formation.
[0023] Preferably, in the pickling and passivation solution contact, the contact method is spraying or immersion; the temperature of the pickling and passivation solution is 45-60°C; and the contact time is 60-180 seconds.
[0024] By adopting the above technical solution, the temperature is controlled within the range of 45-60℃, providing the activation energy required for the chemical reaction to form a dense film layer, while avoiding the decomposition of organic components such as glycolic acid and gallic acid due to excessively high temperatures. The processing time is controlled within the range of 60-180 seconds, matching the speed of the continuous production line for aluminum alloy strips, ensuring the completion of the entire process from oxide scale removal to passivation film growth, and preventing incomplete film formation due to too short a processing time or excessive corrosion of the substrate due to too long a processing time.
[0025] Preferably, in the deionized water cleaning process, the cleaning time is 10-30 seconds, and the conductivity of the final cleaning water is controlled below 30 μS / cm.
[0026] By employing the above technical solution, controlling the conductivity of the cleaning water can remove residual acidic media and unreacted ionic compounds from the membrane surface. Removing residual acidic substances prevents the formation of hygroscopic salt nuclei after drying, avoids osmotic blistering and filamentous corrosion under the coating, and ensures the long-term stability of the membrane.
[0027] Preferably, in the heating and drying step, the drying method is hot air circulation drying or infrared radiation drying; during the drying process, the surface temperature (PMT) of the aluminum alloy strip is controlled at 80-120℃.
[0028] By adopting the above technical solution, the film undergoes dehydration and cross-linking within the temperature range of 80-120℃, transforming from a loose gel state to a dense solid state; at the same time, the coordination bond between gallic acid and metal ions is strengthened under thermal action, the film shrinks and densifies, and the hardness and wear resistance are improved.
[0029] Preferably, in the degreasing and cleaning step, the degreasing temperature is 50-65℃ and the processing time is 20 seconds to 3 minutes.
[0030] By adopting the above technical solution, the pretreatment parameters ensure that the rolling oil and attached contaminants on the aluminum surface are emulsified and removed, providing a clean, hydrophilic active surface for pickling and film formation.
[0031] Preferably, the aluminum alloy strip is a 3-series, 5-series, or 6-series aluminum alloy; during the pickling and passivation process, a conversion film containing phytic acid-vanadium complex is formed on the surface of the aluminum alloy strip while removing the oxide scale.
[0032] This invention provides a method for pickling and passivating corrosion-resistant aluminum alloy strip. It has the following beneficial effects: 1. This invention uses methanesulfonic acid as an acidic etching and solvent matrix, taking advantage of its extremely high solubility and stability for aluminum salts. This solves the problem of precipitation failure in traditional pickling and passivation solutions at high aluminum ion concentrations. The methanesulfonic acid system can maintain the homogeneity and stability of the bath solution while quickly removing oxide scale and black ash, thus increasing the upper limit of aluminum capacity of the bath solution. This not only combines the pickling and passivation processes, shortening the production process, but also significantly extends the service life and replacement cycle of the bath solution, reducing waste liquid discharge pressure and production costs.
[0033] 2. This invention forms an aluminum phytate underlayer on the surface of an aluminum substrate through the strong chelating ability of phytic acid. Combined with the active vanadium ions provided by vanadium oxysulfate to fill the defects in the film layer, and further cross-linked and sealed by the phenolic hydroxyl groups of gallic acid, the conversion film structure formed by this ternary synergistic effect is dense, effectively blocking the penetration channels of corrosive media, and has a certain redox self-repair function. The film layer shows a better protective effect than traditional single zirconium or titanium passivation films in neutral salt spray tests, solving the problem that chromium-free passivation films are usually loose and have insufficient corrosion resistance.
[0034] 3. This invention, by regulating the film-forming reaction rate using glycolic acid and gallic acid, avoids excessive film accumulation and thickening, maintaining a low surface contact resistance in the passivation film. This meets the conductivity requirements of aluminum alloy components in the electronics industry. Simultaneously, the organic active functional groups introduced into the film can chemically bond with subsequent powder coatings or paints, acting as molecular bridges between the film and the coating layer, enhancing coating adhesion and effectively preventing filiform corrosion and blistering / peeling under the coating. Detailed Implementation
[0035] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.
[0036] The wetting agent is a polyoxyethylene-polyoxypropylene block copolymer, CAS number 9003-11-6. Its structural characteristics are polyoxypropylene-polyoxyethylene block copolymer, with an average molecular weight of 1800-3000 g / mol and a hydrophilic-lipophilic balance (HLB) value range of 8-12. It belongs to nonionic low-foaming surfactant.
[0037] Preparation Examples 1-5: Preparation Example 1: This preparation example provides an acid pickling and passivation solution, the components of which are as follows by weight: 60 parts methanesulfonic acid, 5 parts phytic acid, 10 parts vanadium sulfate, 2 parts gallic acid, 15 parts glycolic acid, 1 part wetting agent, and 907 parts deionized water.
[0038] The preparation method of pickling and passivation solution includes the following steps: Add approximately 60% of the total formula volume of deionized water to the mixing tank and turn on the mechanical stirrer (300 r / min). Slowly add 60 parts by weight of methanesulfonic acid solution and 15 parts by weight of glycolic acid solution corresponding to the active ingredient, stir evenly, and construct a strongly acidic reducing matrix. Add 5 parts by weight of phytic acid solution corresponding to the active ingredient, stir for 5 minutes, then add 10 parts by weight of vanadium oxysulfate solid, and continue stirring until the blue crystals are completely dissolved. Dissolve 2 parts by weight of gallic acid in a small amount of 50°C warm water (taken from the formula water volume) and add it to the main tank. Stir for 20 minutes, and the solution turns into a deep blue-black color. Add 1 part by weight of wetting agent, and finally add deionized water to make the total weight of the composition 1000 parts. Stir well to obtain the pickling and passivation solution.
[0039] Preparation Example 2: This preparation example provides an acid pickling and passivation solution, the components of which are as follows by weight: 30 parts methanesulfonic acid, 2 parts phytic acid, 5 parts vanadium sulfate, 1 part gallic acid, 5 parts glycolic acid, 0.5 parts wetting agent, and 956.5 parts deionized water.
[0040] The preparation method of this pickling and passivation solution includes the following steps: Add approximately 60% of the total formula volume of deionized water to the mixing tank and turn on the mechanical stirrer (300 r / min). Slowly add 30 parts by weight of methanesulfonic acid solution and 5 parts by weight of glycolic acid solution of active ingredient, and stir until homogeneous; Add 2 parts by weight of phytic acid solution corresponding to the active ingredient, stir evenly, then add 5 parts by weight of vanadium oxysulfate solid, and continue stirring until completely dissolved; Add 1 part by weight of gallic acid (add directly or after pre-dissolving), and stir for 20 minutes until the system is clear; Add 0.5 parts by weight of wetting agent, and finally add deionized water to make the total weight of the composition 1000 parts. Stir well to obtain the pickling and passivation solution.
[0041] Preparation Example 3: This preparation example provides an acid pickling and passivation solution, the components of which are as follows by weight: 100 parts of methanesulfonic acid, 15 parts of phytic acid, 15 parts of vanadium sulfate, 5 parts of gallic acid, 30 parts of glycolic acid, 2 parts of wetting agent, and 833 parts of deionized water.
[0042] The preparation method of this pickling and passivation solution includes the following steps: Add approximately 60% of the total formula volume of deionized water to the mixing tank and turn on the mechanical stirrer (400 r / min). Slowly add 100 parts by weight of methanesulfonic acid solution and 30 parts by weight of glycolic acid solution of active ingredient, being careful to control the acid addition rate to prevent local overheating, and stir until homogeneous. Add 15 parts by weight of phytic acid solution corresponding to the active ingredient, stir thoroughly, then add 15 parts by weight of vanadium oxysulfate solid, and stir until the solid is completely dissolved. Add 5 parts by weight of pre-dissolved gallic acid to the main tank and stir for 30 minutes to ensure uniform dispersion of high-concentration organic ligands; Add 2 parts by weight of wetting agent, and finally add deionized water to make the total weight of the composition 1000 parts. Stir well to obtain the pickling and passivation solution.
[0043] Preparation Example 4: This preparation example provides an acid pickling and passivation solution, the components of which are as follows by weight: 80 parts methanesulfonic acid, 10 parts phytic acid, 8 parts vanadium sulfate, 3 parts gallic acid, 20 parts glycolic acid, 1.5 parts wetting agent, and 877.5 parts deionized water.
[0044] The preparation method of pickling and passivation solution includes the following steps: Add approximately 60% of the total formula volume of deionized water to the mixing tank and turn on the mechanical stirrer (300 r / min). Slowly add 80 parts by weight of methanesulfonic acid solution and 20 parts by weight of glycolic acid solution of active ingredient, and stir until homogeneous; Add 10 parts by weight of phytic acid solution corresponding to the active ingredient, stir for 10 minutes to give the system a strong ion shielding ability, and then add 8 parts by weight of vanadium oxysulfate solid to dissolve. Add 3 parts by weight of gallic acid and stir for 20 minutes; Add 1.5 parts by weight of wetting agent, and finally add deionized water to make the total weight of the composition 1000 parts. Stir well to obtain the pickling and passivation solution.
[0045] Preparation Example 5: This preparation example provides an acid pickling and passivation solution, the components of which are as follows by weight: 50 parts methanesulfonic acid, 4 parts phytic acid, 12 parts vanadium sulfate, 2.5 parts gallic acid, 10 parts glycolic acid, 0.8 parts wetting agent, and 920.7 parts deionized water.
[0046] The preparation method of pickling and passivation solution includes the following steps: Add approximately 60% of the total formula volume of deionized water to the mixing tank and turn on the mechanical stirrer (300 r / min). Slowly add 50 parts by weight of methanesulfonic acid solution and 10 parts by weight of glycolic acid solution of active ingredient, and stir until homogeneous; Add 4 parts by weight of phytic acid solution corresponding to the active ingredient, stir well, then add 12 parts by weight of vanadium oxysulfate solid and stir until dissolved. Add 2.5 parts by weight of gallic acid and stir for 20 minutes; Add 0.8 parts by weight of wetting agent, and finally add deionized water to make the total weight of the composition 1000 parts. Stir well to obtain the pickling and passivation solution.
[0047] Examples 1-5: Example 1: This embodiment provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, wherein the substrate being treated is 6061 aluminum alloy sheet, and includes the following steps: Degreasing: The aluminum alloy sheet is placed in a weakly alkaline degreasing solution for spraying treatment. The temperature is controlled at 60℃, the spraying pressure is 0.1MPa, and the treatment time is 20 seconds. Then, it is rinsed twice with countercurrent pure water until a continuous water film is formed on the surface. Pickling and passivation: The aluminum alloy plate after degreasing is completely immersed in the pickling and passivation solution prepared in Example 1. The temperature of the solution is controlled at 50°C and the immersion time is 90 seconds. During this time, the solution is kept circulating and stirred. The acid etching of methanesulfonic acid and the deposition of vanadium phytate induced by the increase of the interface pH are used to simultaneously remove oxide scale and form a film on the aluminum surface. Post-reaction water washing: Remove the treated board and immediately spray it with room temperature deionized water for 15 seconds to thoroughly remove the residual acidic medium and floating reactants on the surface. The conductivity of the final cleaning water should be controlled below 30μS / cm. Drying and curing: The washed board is sent into a hot air circulating oven for drying. The board surface temperature (PMT) is controlled to reach 100℃ and the drying time is 3 minutes. After cooling, the finished product is obtained.
[0048] Example 2: This embodiment provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, wherein the substrate being treated is 3003 aluminum alloy sheet, and includes the following steps: Degreasing: Immerse the aluminum alloy sheet completely in a weak alkaline degreasing solution at a temperature of 50°C for 3 minutes. After immersion, rinse it with water multiple times until it becomes neutral. Pickling and passivation: The aluminum alloy sheet was sprayed with the pickling and passivation solution of Preparation Example 2. The spraying pressure was 0.8 MPa, the solution temperature was controlled at 45°C, and the spraying time was 60 seconds. Post-reaction water washing: Use room temperature deionized water to overflow rinse for 10 seconds to wash away residual drug solution on the surface; Drying and curing: Place the board in an oven and dry for 5 minutes at a board surface temperature (PMT) of 80°C to complete the film curing with low energy consumption.
[0049] Example 3: This embodiment provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, wherein the substrate being treated is 5052 aluminum alloy sheet (high magnesium alloy), and includes the following steps: Degreasing: The aluminum plate is degreased by spraying at 65℃ for 30 seconds, followed by thorough rinsing with water. Pickling and passivation: The aluminum alloy sheet was immersed in the pickling and passivation solution of Preparation Example 3. The temperature of the solution was controlled at 60°C and the immersion time was extended to 180 seconds to ensure the complete removal of the thick oxide scale and the sufficient growth of the passivation film. The pH value of the solution was maintained below 1 during the process. Post-reaction water washing: A two-stage spray water washing process is adopted, with a total water washing time of 30 seconds, to ensure thorough removal of high-viscosity residual liquid; Drying and curing: The board is placed in an oven and the surface temperature (PMT) is controlled to reach 120°C and held for 2 minutes to promote the formation of a highly cross-linked film.
[0050] Example 4: This embodiment provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, wherein the substrate being treated is 6061 aluminum alloy sheet, and includes the following steps: Degreasing: Conventional alkaline degreasing, temperature 55℃, time 25 seconds, then rinse with water; Pickling and passivation: The enhanced pickling and passivation solution of Preparation Example 4 was selected, the bath temperature was controlled at 55℃, the treatment method was immersion, and the time was 120 seconds. Post-reaction water washing: Rinse with deionized water at room temperature for 20 seconds; Drying and curing: Hot air drying is used, with the surface temperature (PMT) controlled at 110℃ and the drying time being 3 minutes.
[0051] Example 5: This embodiment provides a method for pickling and passivating corrosion-resistant aluminum alloy strip, wherein the substrate being treated is 3003 aluminum alloy sheet, and includes the following steps: Degreasing: Conventional spray degreasing, temperature 60℃, time 20 seconds, followed by rinsing with water; Pickling and passivation: The aluminum alloy sheet was sprayed into contact with the pickling and passivation solution prepared in Example 5 at a temperature of 52°C for 100 seconds. Post-reaction water washing: Spray clean with room temperature deionized water for 15 seconds, and squeeze out most of the surface moisture by squeezing rollers; Drying and curing: The board is rapidly cured by passing it through an infrared (IR) heating tunnel. The radiation power is set so that the surface temperature (PMT) of the board reaches 120°C within 15 seconds and is maintained at that temperature for 15 seconds, followed by air cooling to room temperature.
[0052] Comparative Examples 1-6: Comparative Example 1: Compared with Example 1, the difference is that the pickling and passivation solution in the pickling and passivation process is replaced with a commercially available fluorozirconate passivation solution (the main components are fluorozirconic acid 3g / L, hydrofluoric acid 0.2g / L, and pH adjusted to 3.5), the treatment temperature is room temperature, and the time is 3 minutes; the remaining steps (degreasing, washing, and drying) are the same.
[0053] Comparative Example 2: Compared with Example 1, the difference is that phytic acid is not added to the pickling and passivation solution used, the other components and ratios remain unchanged, and the step of adding phytic acid is omitted during preparation; the other process steps are the same.
[0054] Comparative Example 3: Compared with Example 1, the difference is that in the pickling and passivation solution used, methanesulfonic acid (MSA) is replaced with an equimolar amount of sulfuric acid (H2SO4), while the other components and proportions remain unchanged; the other process steps are the same.
[0055] Comparative Example 4: Compared with Example 1, the difference is that gallic acid is not added to the pickling and passivation solution used, the other components and ratios remain unchanged, and the step of adding gallic acid is omitted during preparation; the other process steps are the same.
[0056] Comparative Example 5: Compared with Example 1, the difference is that 1 g / L of sodium persulfate (a strong oxidant) was added to the pickling and passivation solution used, while the other components and proportions remained unchanged; the other process steps were the same.
[0057] Comparative Example 6: Compared with Example 1, the difference is that the post-reaction water washing is omitted, and the aluminum plate after acid pickling and passivation is directly squeezed dry and sent to the oven for drying and curing; all other aspects are the same.
[0058] Test Example 1-2: Test Example 1: Process Adaptability and Stability Test Experimental steps: Take 1000 mL of fresh working solution prepared in each example and comparative example, and seal it in a borosilicate glass container. Place it in an environment of 25±2℃ and 45±2℃ respectively for standing. Visually inspect the solution appearance periodically, recording color changes, layering, flocculation, and crystal precipitation. The failure criterion is the appearance of visible precipitate at the bottom of the solution or irreversible discoloration and turbidity of the entire solution; record the time it remains clear. Take another 500 mL of fresh working solution from each group, heat to 50℃, and add 200-mesh pure aluminum powder (purity ≥99.5%) in batches under magnetic stirring at 300 r / min. Each addition is equivalent to 2 g / L of aluminum content. After the aluminum powder has completely reacted and dissolved, let it stand for 30 minutes. Observe the solution state; if it remains clear, continue adding aluminum powder; if turbidity, gelation, or crystal precipitation occurs, stop adding aluminum powder and record the total concentration of aluminum ions accumulated in the system at this time.
[0059] Test result data: The test data for each group are summarized in Table 1 below. The maximum aluminum capacity refers to the limit of aluminum ion concentration that the solution can dissolve to maintain a clear and transparent state.
[0060] Table 1. Summary of test data on composition stability and aluminum content (Note: "--" indicates that the test was not performed because the bath solution decomposed and failed, making it impossible to prepare a valid sample.) Results analysis: Based on the experimental data and chemical reaction mechanism analysis in Table 1: Compared with Comparative Example 1 and Comparative Example 3, replacing methanesulfonic acid with sulfuric acid reduced the system's capacity to hold aluminum ions from 28 g / L to 4 g / L. Aluminum sulfate and vanadium oxysulfate have low solubility product constants in acidic environments; as the aluminum ion concentration increases, they rapidly reach supersaturation due to the common ion effect and crystallize out. The methanesulfonic acid system used in Example 1 has high metal salt water solubility, maintaining homogeneity of the bath solution under aluminum ion enrichment.
[0061] Compared with Comparative Example 2, the absence of phytic acid resulted in a decrease in aluminum capacity from 28 g / L to 8 g / L, and a decline in storage stability. The phosphate groups in the phytic acid molecule chelate with aluminum ions, forming a water-soluble phytic acid-aluminum complex. This chelation inhibits the hydrolytic polymerization of aluminum ions to form aluminum hydroxide colloids or aluminum hydroxide, thus delaying precipitation.
[0062] In Comparative Example 5, the addition of sodium persulfate resulted in blackening and degradation within a short period. The gallic acid and phytic acid components in the system decomposed under strong oxidizing conditions. Removing the strong oxidant and utilizing glycolic acid to create a reducing environment maintained the structural integrity of the organic ligands, ensuring the working solution remained stable at 45°C.
[0063] Example 4 showed an aluminum capacity of 35 g / L, higher than the 12 g / L of the fluorozirconic acid system in Comparative Example 1. The methanesulfonic acid-phytic acid system can accommodate higher concentrations of reaction products, extending the service life of the bath.
[0064] Test Example 2: Film Performance Index Test Experimental steps: Aluminum alloy sheet samples treated in Examples 1 to 5 and Comparative Examples 1 to 6 were selected. The film weight test was performed according to the standard GB / T9792-2003, "Determination of the Mass of Conversion Coating per Unit Area on Metallic Materials," using a phosphochromic acid solution to remove the film, and the mass difference before and after removal was measured to calculate the film weight per unit area. The neutral salt spray corrosion resistance test was performed according to the standard GB / T10125-2021, "Artificial Atmosphere Corrosion Test - Salt Spray Test," using a 50±5 g / L NaCl solution continuously sprayed at 35±2℃, and the time to the first visible corrosion point on the surface was recorded. The contact resistance test was performed according to the standard MIL-DTL-81706B, "Cross-cut Test for Paints and Varnishes," using an ST2263 surface resistance tester with a pressure set to 0.2 MPa. Ten points were measured for each sample group, and the average value was calculated. Coating adhesion testing was conducted according to GB / T9286-2021 standard. Polyester powder coating was sprayed onto the passivation film surface and cured. A 1mm interval cross-cut test was performed, and the peeling level was assessed using 3M 600 tape. Electrochemical polarization curve testing employed a three-electrode system, using a saturated calomel electrode as the reference, a platinum sheet as the counter electrode, and a 3.5wt% NaCl solution as the electrolyte. The scan rate was 1mV / s, and the self-corrosion current density was obtained using the Tafel zone extrapolation method.
[0065] The test results for various physical and chemical properties are summarized in Table 2: Table 2. Summary of physicochemical properties and corrosion resistance test data of passivation film. (Note: Comparative Example 5 could not be tested because the solution rapidly decomposed and failed, making it impossible to prepare an effective sample.) Results analysis: Example 1: Membrane weight 185.4 mg / m³ 2 Neutral salt spray corrosion resistance time: 216 hours; self-corrosion current density: 0.45 μA / cm³. 2 Contact resistance 0.8 mΩ·cm 2 In a fluorine-free and chromium-free system, its corrosion resistance and conductivity meet or exceed the passivation level of the traditional fluorine-containing zirconium system in Comparative Example 1, meeting the requirement of a contact resistance of less than 1.5 mΩ·cm in the electronics and electrical appliance industry. 2 Requirements.
[0066] Data from Example 1 and Comparative Example 2 showed that the absence of phytic acid led to a decrease in membrane weight to 45.7 mg / m³. 2, The salt spray lifespan is only 24 hours, and the self-corrosion current density increases significantly. The coordination deposition of phytic acid and vanadium ions is the key to the film formation process. Without phytic acid, it is difficult to form a dense conversion film on the aluminum surface, and the natural oxide layer of the substrate cannot provide long-term protection.
[0067] Data from Example 1 and Comparative Example 4 show that the salt spray time of the sample without gallic acid was reduced to 72 hours, while the corrosion current density increased. Gallic acid, as an organic ligand, participates in the sealing of micropores in the membrane layer. The organic-inorganic hybrid structure reduces the porosity of the membrane layer and blocks the penetration channels of corrosive media.
[0068] Comparative Example 6, after washing with water following the cancellation of the reaction, showed a membrane weight of 192.8 mg / m³. 2 However, the contact resistance rose to 3.45 mΩ·cm. 2 The adhesion test result was grade 4 (severe peeling). Residual methanesulfonate and unreacted substances on the surface are hygroscopic, causing osmotic pressure blistering beneath the coating and damaging the bond between the coating and the substrate. A water washing step is necessary to ensure coating compatibility and electrical stability.
[0069] Example 3 showed the thickest film layer (243.1 mg / m³) under high-temperature, long-term treatment conditions. 2 It has the longest corrosion resistance time (248 hours), but the contact resistance rises to 1.94 mΩ·cm. 2 The adhesion dropped to level 1. Process parameter adjustments need to balance corrosion resistance, conductivity, and adhesion. Example 2 verified the effect at a low film weight (92.6 mg / m³). 2 It can provide 96 hours of basic protection and is suitable for low-cost, medium-corrosion-resistance applications.
Claims
1. A method for pickling and passivating corrosion-resistant aluminum alloy strip, characterized in that, Includes the following steps: The surface of the aluminum alloy strip is degreased and cleaned to remove surface oil and then washed with water to obtain the aluminum alloy after degreasing and cleaning treatment. The aluminum alloy strip, after degreasing and cleaning, is brought into contact with an acid pickling and passivation solution to react. Clean the surface of the aluminum alloy strip after it has been treated with pickling and passivation solution by deionized water. The cleaned aluminum alloy strip is then heated and dried.
2. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, The pickling and passivation solution is prepared from the following raw materials in parts by weight: Methylsulfonic acid: 30-100 parts; Phytic acid: 2-15 parts; Vanadium oxysulfate: 5-15 parts; Gallic acid: 1-5 parts; Glycolic acid: 5-30 parts; Wetting agent: 0.5-2 parts; Deionized water: Remaining amount, bring the total to 1000 portions.
3. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 2, characterized in that, The weight parts of the raw materials are: Methylsulfonic acid: 55-65 parts; Phytic acid: 4-6 parts; Vanadium oxysulfate: 9-11 parts; Gallic acid: 1.5-2.5 parts; Glycolic acid: 12-18 parts; Wetting agent: 0.8-1.2 parts; Deionized water: Remaining amount, bring the total to 1000 portions.
4. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 2, characterized in that, The wetting agent is selected from one or more of fatty alcohol polyoxyethylene ether, sodium alkyl sulfonate, or fluorocarbon surfactant.
5. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 2, characterized in that, The pH value of the pickling and passivation solution is controlled below 1.
6. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, In the step of contacting the aluminum alloy strip after degreasing and cleaning with the pickling and passivation solution, the contact method is either spraying or immersion. The temperature of the pickling and passivation solution is 45-60℃; The contact time is 60-180 seconds.
7. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, In the step of cleaning the surface of the aluminum alloy strip after the pickling and passivation solution contact reaction treatment with deionized water, the cleaning time of the deionized water is 10-30 seconds, and the conductivity of the last cleaning water after cleaning is controlled below 30μS / cm.
8. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, In the step of heating and drying the cleaned aluminum alloy strip, the drying method is hot air circulation drying or infrared radiation drying. During the drying process, the surface temperature of the aluminum alloy strip is controlled at 80-120℃.
9. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, In the process of contacting the degreasing and cleaning aluminum alloy strip with the pickling and passivation solution, the degreasing temperature is 50-65℃ and the processing time is 20 seconds to 3 minutes.
10. The pickling and passivation method for corrosion-resistant aluminum alloy strip according to claim 1, characterized in that, The aluminum alloy strip is a 3-series, 5-series, or 6-series aluminum alloy.