Non-oriented silicon steel and manufacturing method thereof
By optimizing the chemical composition and manufacturing process of non-oriented silicon steel, the balance between high strength and electromagnetic properties has been resolved, resulting in non-oriented silicon steel with high strength and excellent magnetic properties, suitable for high-speed motors, and reducing production costs.
Patent Information
- Application Number
- CN202610233329.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-27
- Publication Date
- 2026-05-12
AI Technical Summary
Existing non-oriented silicon steels are difficult to balance between high strength and electromagnetic properties, especially in high-speed motors where their magnetic properties are insufficient, and their production costs are high.
By controlling the chemical composition and process parameters, including the addition of alloying elements and steps such as hot rolling, cold rolling, and annealing, the manufacturing process of non-oriented silicon steel is optimized. In particular, the content of elements such as Si, Mn, Al, and Sn is controlled, and the strength and magnetic properties of the material are improved by precisely controlling the hot rolling, normalizing, cold rolling, and annealing temperatures.
It achieves high strength (tensile strength exceeding 800MPa) and excellent electromagnetic properties (magnetic induction intensity in the range of 1.63-1.67T) in non-oriented silicon steel, meeting the requirements of high-speed motors while reducing production costs.
Smart Images

Figure CN122013022A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical engineering technology and discloses a non-oriented silicon steel and its manufacturing method. Background Technology
[0002] Non-oriented silicon steel is mainly used in various generators, motors, and rotating equipment. It is a major raw material for motor production and an indispensable soft magnetic material in the electronics, motor, and military industries. In recent years, with the tightening of national energy policies, industrial motors, compressors, and new energy drive motors have placed higher demands on the electromagnetic and mechanical properties of non-oriented silicon steel.
[0003] Especially with the accelerated shift of China's automotive industry from traditional fuel vehicles to new energy vehicles, the demand for non-oriented silicon steel for drive motors is gradually increasing. At the same time, higher requirements are being placed on the electromagnetic and mechanical properties of silicon steel. For the rotor core, high speeds cause the rotor to experience extremely high centrifugal forces. Currently, some new energy drive motors in China operate at speeds reaching 22,000 rpm, or even 30,000 rpm. The strength of mainstream silicon steel used in new energy drive motors is generally between 500-600 MPa, which is no longer sufficient to meet the demands of high-speed drive motors. Currently, the mainstream strengthening methods include solid solution strengthening and precipitation strengthening. Chinese patent CN114657461 A discloses a high-strength non-oriented silicon steel based on solid solution strengthening and its preparation method. This patent utilizes solid solution strengthening by adding Si and P elements, and dislocation strengthening through low-temperature annealing. The chemical composition of the non-oriented silicon steel is: Si: 2.8–4.8 wt.%, P: 0–0.2 wt.%, Mn: 0–0.5 wt.%, Al: 0–0.5 wt.%, (C+N+O+S) ≤100 ppm, with the remainder being Fe. The preparation method includes vacuum smelting, casting and forging, hot rolling and normalizing heat treatment, or thin strip continuous casting. The final high-strength non-oriented silicon steel has a strength (Rm) of 620–750 MPa. However, the highest strength of the non-oriented silicon steel produced by this method is only around 750 MPa, which is relatively low.
[0004] Chinese patent CN 120591677 A discloses a high-strength non-oriented silicon steel with a yield strength of 930 MPa and its production method. This patent comprehensively utilizes three strengthening methods: dislocation strengthening, solid solution strengthening, and precipitation strengthening. The chemical composition of the non-oriented silicon steel is designed as follows: Si: 3.0-4.0%, Al: 0.1-2%, Mn: 0.1-1.0%, Nb: 0.0005-0.0010%, Ti: 0.001-0.0030%, V: 0.0010-0.0025%, C: 0.0020-0.0035%, N: 0.0010-0.0025%, and Si+Al+Mn: 4.0-5.4%, Nb+Ti+V: 0.0045-0.0055%, C+N: 0.0035-0.0050%. The production method employs a process route of converter smelting → RH refining → continuous casting → hot rolling → pickling → cold rolling → annealing → coating. By designing the matching relationship between composition, annealing temperature, and annealing speed, and using a hot rolling process of "high-temperature long-time heating, low-temperature final rolling, and high-temperature coiling," excellent properties such as yield strength Rp0.2≥930MPa, iron loss P1.0 / 400≤57W / kg, and magnetic polarization J5000≥1.52T are obtained. Although the high-strength non-oriented silicon steel manufactured by this method has excellent mechanical properties, its electromagnetic properties, especially magnetic polarization, are relatively low. During the operation of the iron core rotor, this may cause the rotor teeth or yoke to prematurely enter a magnetic saturation state, affecting efficiency.
[0005] Japanese Patent JP2011-184787 discloses a method for producing high-strength non-oriented silicon steel. Its chemical composition is as follows: C: 0.003%, Si: 3%, Al: 0.75%, Mn: 0.24-2.18%, Ni: <2.59%, Cr: 2.09-6.14%, P: 0.03%. The annealing process is 750℃×20s, the finished product thickness is 0.2mm, Re: 609-679MPa, Rm: 712-776MPa, A: 29-31%, P15 / 50: 4.3-4.5W / kg, P10 / 1000: 38-44W / kg, B50: 1.58-1.65T.
[0006] Japanese Patent JP2008-261053 discloses a method for producing high-strength non-oriented silicon steel containing Cu. Its chemical composition is: C < 0.003%, Si: 1.1-1.3%, Al < 0.005%, Mn: 0.13-0.44%, P: 0.015-0.021%, S < 0.003%, Cu: 0.93-2.24%. The billet thickness is 250mm, the soaking temperature is 1100℃, the hot-rolled plate thickness is 2mm, the coiling temperature is 500℃, the cold-rolled plate thickness is 0.5mm, and the annealing process involves maintaining the temperature near 500℃ for 100-300s during cooling. The finished product has the following strengths: Re: 448-571MPa, Rm: 573-727MPa, P10 / 400: 34.8-38.4W / kg, B10: 1.57-1.62T.
[0007] Currently, most publicly disclosed high-strength silicon steel patents are from Japan. The solid solution strengthening route requires the addition of alloying elements such as Ni, Cr, and P to improve the mechanical properties of the finished product. However, the high prices of Ni and Cr lead to high production costs, and solid solution strengthening has limited strength-enhancing capabilities. The Cu precipitation route adds Cu and, through optimized heat treatment and aging processes, controls the Cu precipitation size to achieve material strengthening. However, Cu can cause hot brittleness, generally requiring the addition of Ni to suppress it, increasing costs. Furthermore, the Cu precipitation route requires aging treatment to achieve material strengthening, which is time-consuming and reduces production efficiency. In addition, domestic companies such as Shougang and Taiyuan Iron & Steel use dislocation strengthening to produce high-strength non-oriented silicon steel. While its mechanical properties can reach over 900 MPa, its electromagnetic properties are poor, particularly in terms of magnetic induction and magnetic polarization, thus affecting motor operating efficiency. Summary of the Invention
[0008] To address the above problems, this invention provides a method for manufacturing non-oriented silicon steel, comprising the following steps: S1. During the steelmaking process, through decarburization, desulfurization, and the addition of alloying raw materials, the chemical composition of the steel billet, by weight percentage, is as follows: C≤0.003%, Si: 3.2-3.5%, Mn: 0.4-0.6%, Als: 0.5-0.8%, Sn: 0.03-0.05%, S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurities; The roles of each element in steel are as follows: C: Although C can improve mechanical properties, it is a harmful element for non-oriented silicon steel, which will deteriorate the magnetic properties of silicon steel. Preferably, the present invention requires that the C content be controlled below 0.003%.
[0009] Si: Si can reduce iron loss, and the solid solution strengthening effect of Si can improve mechanical strength. At the same time, the increase of Si is beneficial to the improvement of electromagnetic energy. In combination with the requirements of ultra-high speed (≥22000 rpm) motor rotor for material mechanical properties, the Si content in this invention is controlled at 3.2%-3.5%.
[0010] Mn: Mn plays a solid solution strengthening role in non-oriented silicon steel, which can improve the product strength and reduce the product iron loss. Mn and S form MnS, which reduces the amount of S dissolved during the heating of the slab and can effectively suppress the hot brittleness phenomenon during the heating process. However, if the Mn content is too high, fine MnS precipitates will be generated during hot rolling, which will prevent grain growth and deteriorate the magnetic properties. Therefore, the Mn content in this invention is controlled at 0.40%-0.60%.
[0011] Als: Al is similar to Si in that it can improve the magnetic properties and mechanical strength of the product. However, Al has a smaller impact on the brittleness of electrical steel than Si. Considering the magnetic performance requirements of the product, the Al content in this invention should be controlled at 0.5%-0.8%.
[0012] Sn: Sn mainly exists in steel in a solid solution state or is segregated at grain boundaries, reducing the formation of coarse grains. Sn can also improve the texture of non-oriented silicon steel, increasing the content of components with favorable textures such as {100} and {110}, thereby improving magnetic flux density. High magnetic flux density reduces the risk of magnetic circuit saturation, decreases excitation requirements, and indirectly reduces copper losses. Especially at high speeds and high loads, it ensures the flux transmission efficiency of the rotor magnetic circuit. However, Sn is expensive, and excessive addition will increase costs. Therefore, in this invention, Sn is controlled at 0.03-0.05%.
[0013] S2. Molten steel is continuously cast into slabs and heated in a heating furnace. It is then hot-rolled in 7 passes to a thickness of 2.0-2.3mm. The final rolling temperature is controlled at 850-870℃, and the slabs are cooled to 600-650℃ and then coiled. Considering that the present invention has a normalizing process, the final rolling temperature is high-temperature final rolling. A high final rolling temperature can optimize the texture and improve the magnetic induction. Therefore, the final rolling temperature is controlled at 850-870℃. Excessive winding temperature will reduce mechanical properties and promote the precipitation of carbides and nitrides, which is detrimental to electromagnetic properties. Therefore, this invention requires the hot rolling winding temperature to be controlled at 600-650℃, and the coiled coil to be naturally cooled to room temperature.
[0014] S3. The coiled strip is heated in a normalizing furnace, with the normalizing temperature controlled between 830-870℃ and the normalizing time between 2-4 minutes. After cooling, it is pickled and then cold rolled to the target thickness in 5-6 passes. To reduce the risk of strip breakage during high-Si non-oriented cold rolling, the normalizing temperature should not be too high. At the same time, to ensure the magnetic properties of the product, the normalizing temperature should not be too low. Taking into account magnetic properties, mechanical strength, and the smoothness requirements of cold working, the normalizing temperature should be controlled between 830-870℃, and the normalizing time should be 2-4 minutes to reduce the internal stress of the strip and allow the grains to fully recover.
[0015] S4. Continuously anneal the cold-rolled sheet, with the annealing temperature controlled between 650-710℃ and the holding time controlled between 60-120s; If the annealing temperature is too high, the yield strength of the product will decrease. In order to ensure the ultra-high strength mechanical properties of the finished product, elements such as Si, Mn, Als, and Sn have been added during refining. These elements are all substitutional solute atoms, which will cause lattice distortion. During the recrystallization process, these lattice distortion regions will have a pinning effect on the grain boundaries, thereby increasing the recrystallization temperature. Therefore, annealing is required.
[0016] S5. After annealing, the sheet is alkali washed and then coated with insulating paint using a coating roller. The insulating paint is cured at 380-650℃ and then cooled to complete the manufacturing of non-oriented silicon steel.
[0017] Preferably, the temperature of the heating furnace is controlled at 1100-1250℃, and the heating and holding time is not less than 210 minutes.
[0018] Preferably, after normalization, the temperature is first cooled to 600-700℃ at 5-10℃ / s, and then cooled to below 100℃ at 20-50℃ / s.
[0019] Preferably, pickling is performed using 45-65% hydrochloric acid at a temperature of 60-85℃. Preferably, during continuous annealing, a protective atmosphere is prepared using H2 and N2 in a volume ratio of 3:7.
[0020] This ensures that there are no oxidation defects on the surface.
[0021] Preferably, laminar flow cooling is used before winding, and segmented cooling is used to ensure that the temperature during winding is within a set range.
[0022] Based on the same principle, the present invention also provides a non-oriented silicon steel manufactured using the above method, the chemical composition of which, by weight percentage, is: C≤0.003%, Si: 3.2-3.5%, Mn: 0.4-0.6%, Als: 0.5-0.8%, Sn: 0.03-0.05%, S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurities.
[0023] Compared with existing technologies, the non-oriented silicon steel and its manufacturing method provided by this invention have the following advantages: The production process of non-oriented silicon steel of the present invention is the same as that of conventional high-strength non-oriented silicon steel, but with higher production efficiency and better economic benefits. The non-oriented silicon steel of this invention breaks through the limits of the mechanical properties of conventional solid solution strengthened non-oriented silicon steel, and its tensile strength can exceed 800 MPa. The non-oriented silicon steel of this invention maintains the advantage of ultra-high strength while possessing excellent electromagnetic properties, especially magnetic induction in the range of 1.63-1.67T, which meets the rotor core's requirement for high magnetic induction. Attached Figure Description
[0024] Figure 1 This is the microstructure of Embodiment 1 of the present invention; Figure 2 This is the microstructure of Embodiment 2 of the present invention; Figure 3 This is the microstructure of Embodiment 3 of the present invention. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be described below with reference to the accompanying drawings. The described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without innovative effort are within the scope of protection of the present invention.
[0026] Referring to the accompanying drawings, the present invention provides an embodiment of a method for manufacturing non-oriented silicon steel as follows: Embodiment 1 1) The molten steel refined in the RH furnace (a refining furnace jointly developed by Ruhr Steel and Helas) is continuously cast into slabs with a thickness of 230 mm. The chemical composition of the slabs by weight percentage is as follows: Si: 3.35%; Als: 0.65%; Mn: 0.50%; Sn: 0.05%; S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurity elements.
[0027] 2) The temperature of the slab in the heating furnace is 1120℃, and the heating and holding time is 220min; 3) The material is hot-rolled to a thickness of 2.0 mm in 7 passes, with a final rolling temperature of 860℃ and a coiling temperature of 650℃. 4) The normalizing temperature is controlled at 850℃, the normalizing time is 2.5min, and the thickness is 0.27mm after 6 passes of rolling; 5) Anneal at 670-680℃ for 60 seconds, using a protective atmosphere of H2 and N2 in a 3:7 ratio. 6) After alkaline washing, the insulating coating is applied through a coating roller and cured at 380-650℃.
[0028] The non-oriented electrical steel manufactured using the above process has an iron loss P1.0 / 400 of 41.4 W / kg, a magnetic induction B50 of 1.631 T, an Rm of 880 MPa, and a microstructure as shown below. Figure 1 As shown.
[0029] Example 2 1) The molten steel refined in the RH furnace is continuously cast into slabs with a thickness of 230 mm. The chemical composition of the slabs by weight percentage is as follows: Si: 3.4%; Als: 0.68%; Mn: 0.55%; Sn: 0.04%; S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurity elements.
[0030] 2) The temperature of the slab in the heating furnace is 1120℃, and the heating and holding time is 220min; 3) The material is hot-rolled to a thickness of 2.0 mm in 7 passes, with a final rolling temperature of 860℃ and a coiling temperature of 650℃. 4) The normalizing temperature is controlled at 850℃, the normalizing time is 2.5min, and the thickness is 0.27mm after 6 passes of rolling; 5) Anneal at 680-690℃ for 80 seconds, using a protective atmosphere of H2 and N2 in a 3:7 ratio. 6) After alkaline washing, the insulating coating is applied through a coating roller and cured at 380-650℃.
[0031] The non-oriented electrical steel manufactured using the above process has an iron loss P1.0 / 400 of 35.2 W / kg, a magnetic induction B50 of 1.646 T, an Rm of 790 MPa, and a microstructure as shown below. Figure 2 As shown.
[0032] Example 3 1) The molten steel refined in the RH furnace is continuously cast into slabs with a thickness of 230 mm. The chemical composition of the slabs by weight percentage is as follows: Si: 3.4%; Als: 0.68%; Mn: 0.55%; Sn: 0.04%; S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurity elements.
[0033] 2) The temperature of the slab in the heating furnace is 1120℃, and the heating and holding time is 220min; 3) The material is hot-rolled to a thickness of 2.0 mm in 7 passes, with a final rolling temperature of 860℃ and a coiling temperature of 650℃. 4) The normalizing temperature is controlled at 850℃, the normalizing time is 2.5min, and the thickness is 0.27mm after 6 passes of rolling; 5) Anneal at 680-690℃ for 100 seconds, using a protective atmosphere of H2 and N2 in a 3:7 ratio. 6) After alkaline washing, the insulating coating is applied through a coating roller and cured at 380-650℃.
[0034] The non-oriented electrical steel manufactured using the above process has an iron loss P1.0 / 400 of 30.01 W / kg, a magnetic induction B50 of 1.661 T, an Rm of 730 MPa, and a microstructure as shown below. Figure 3 As shown.
[0035] An embodiment of a non-oriented silicon steel is manufactured by the above method, and its chemical composition by weight percentage is: C≤0.003%, Si: 3.2-3.5%, Mn: 0.4-0.6%, Als: 0.5-0.8%, Sn: 0.03-0.05%, S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurities.
[0036] Comparative Example 1 1) The molten steel refined in the RH furnace is continuously cast into slabs with a thickness of 230mm. The chemical composition of the slabs by weight percentage is as follows: Si: 3.0%; Als: 0.50%; Mn: 0.55%; S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurity elements.
[0037] 2) The temperature of the slab in the heating furnace is 1120℃, and the heating and holding time is 220min; 3) The material is hot-rolled to a thickness of 2.0 mm in 7 passes, with a final rolling temperature of 860℃ and a coiling temperature of 650℃. 4) The normalizing temperature is controlled at 850℃, the normalizing time is 2.5min, and the thickness is 0.27mm after 6 passes of rolling; 5) Anneal at 620-640℃ for 80 seconds, using a protective atmosphere of H2 and N2 in a 3:7 ratio. 6) After alkaline washing, the insulating coating is applied through a coating roller and cured at 380-650℃.
[0038] The non-oriented electrical steel manufactured using the above process has an iron loss P1.0 / 400 of 45W / Kg, a magnetic induction B50 of 1.583T, and an Rm of 721Mpa.
[0039] Comparative Example 2 1) The molten steel refined in the RH furnace is continuously cast into slabs with a thickness of 230 mm. The chemical composition of the slabs by weight percentage is as follows: Si: 3.35%; Als: 0.65%; Mn: 0.50%; Sn: 0.05%; S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurity elements.
[0040] 2) The temperature of the slab in the heating furnace is 1120℃, and the heating and holding time is 220min; 3) The material is hot-rolled to a thickness of 2.0 mm in 7 passes, with a final rolling temperature of 860℃ and a coiling temperature of 650℃. 4) The normalizing temperature is controlled at 850℃, the normalizing time is 2.5min, and the thickness is 0.27mm after 6 passes of rolling; 5) Anneal at 800-820℃ for 60 seconds, using a protective atmosphere of H2 and N2 in a 3:7 ratio. 6) After alkaline washing, the insulating coating is applied through a coating roller and cured at 380-650℃.
[0041] The non-oriented electrical steel manufactured using the above process has an iron loss P1.0 / 400 of 28.11 W / Kg, a magnetic induction B50 of 1.671 T, and an Rm of 632 MPa.
[0042] Those skilled in the art will understand that embodiments of the present invention can be provided as methods, systems, or computer program products. Therefore, the present invention can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, the present invention can take the form of a computer program product embodied on one or more computers or available storage media (including, but not limited to, disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0043] This invention is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of the invention. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded processor, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart illustrations and / or block diagrams. Figure 1 One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.
[0044] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.
[0045] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.
[0046] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for manufacturing non-oriented silicon steel, characterized in that, Includes the following steps: S1. During the steelmaking process, through decarburization, desulfurization, and the addition of alloying raw materials, the chemical composition of the steel billet, by weight percentage, is as follows: C≤0.003%, Si: 3.2-3.5%, Mn: 0.4-0.6%, Als: 0.5-0.8%, Sn: 0.03-0.05%, S≤0.005%, N≤0.005%, Ti≤0.005%, with the remainder being Fe and unavoidable impurities; S2. Molten steel is continuously cast into slabs and heated in a heating furnace. It is then hot-rolled in 7 passes to a thickness of 2.0-2.3mm. The final rolling temperature is controlled at 850-870℃, and the slabs are cooled to 600-650℃ and then coiled. S3. The coiled strip is heated in a normalizing furnace, with the normalizing temperature controlled between 830-870℃ and the normalizing time between 2-4 minutes. After cooling, it is pickled and then cold rolled to the target thickness in 5-6 passes. S4. Continuously anneal the cold-rolled sheet, with the annealing temperature controlled between 650-710℃ and the holding time controlled between 60-120s; S5. After annealing, the sheet is alkali washed and then coated with insulating paint using a coating roller. The insulating paint is cured at 380-650℃ and then cooled to complete the manufacturing of non-oriented silicon steel.
2. The method for manufacturing non-oriented silicon steel according to claim 1, characterized in that, The temperature of the heating furnace is controlled at 1100-1250℃, and the heating and holding time is not less than 210 minutes.
3. The method for manufacturing non-oriented silicon steel according to claim 2, characterized in that, After normalization, cool to 600-700℃ at 5-10℃ / s, then cool to below 100℃ at 20-50℃ / s.
4. The method for manufacturing non-oriented silicon steel according to claim 3, characterized in that, Pickling is performed using 45-65% hydrochloric acid at a temperature of 60-85℃.
5. The method for manufacturing non-oriented silicon steel according to claim 4, characterized in that, During continuous annealing, a protective atmosphere of H2 and N2 in a volume ratio of 3:7 is used.
6. The method for manufacturing non-oriented silicon steel according to claim 5, characterized in that, Laminar flow cooling is used before winding, and segmented cooling ensures that the temperature during winding is within the set range.
7. A non-oriented silicon steel, manufactured using the non-oriented silicon steel manufacturing method according to any one of claims 1-6, wherein its chemical composition by weight percentage is: C ≤ 0.003%, Si: 3.2-3.5%, Mn: 0.4-0.6%, Als: 0.5-0.8%, Sn: 0.03-0.05%, S ≤ 0.005%, N ≤ 0.005%, Ti ≤ 0.005%, with the remainder being Fe and unavoidable impurities.
Citation Information
Patent Citations
High-strength non-oriented silicon steel based on solution strengthening and preparation method thereof
CN114657461A
High-strength non-oriented silicon steel with yield strength of 930 MPa and production method thereof
CN120591677A
Electromagnetic steel sheet and manufacturing method thereof
JP2008261053A
High tensile strength non-oriented electromagnetic steel sheet having excellent high frequency iron loss
JP2011184787A