A high-damping machine tool moving part and its preparation method
By combining basalt fiber and carbon fiber, along with the synergistic effect of mineral powder, epoxy resin system, and additives, the problems of high inertia and high energy consumption in traditional machine tool moving parts during high-speed motion have been solved. This has resulted in machine tool moving parts with high damping and dimensional stability, suitable for high-speed and high-precision CNC machine tools.
Patent Information
- Application Number
- CN202610701904.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-05-21
AI Technical Summary
Traditional machine tool moving parts suffer from high inertia, high energy consumption, and poor vibration absorption during high-speed movement. Furthermore, carbon fiber composite materials have limited damping properties, making it difficult to balance strength, toughness, rigidity, and damping performance.
By using a blend of basalt fiber and carbon fiber, combined with high-content mineral powder, epoxy resin system and antimony and bismuth additives, and through vacuum kneading, preforming and molding curing processes, a high-damping machine tool moving part is formed, which improves damping performance, dimensional stability and crack resistance.
It achieves high damping, low thermal expansion coefficient, and lightweight machine tool moving parts, which can effectively suppress vibration and thermal deformation, improve machining accuracy and rapid movement capability, reduce energy consumption, and is suitable for high-speed, high-precision CNC machine tools.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of machine tool manufacturing technology, specifically to a high-damping machine tool moving part and its preparation method. Background Technology
[0002] Machine tool moving parts (such as worktables, slides, crossbeams, spindle boxes, tool holders, etc.) need to withstand dynamic loads, vibrations, shocks, and temperature changes during high-speed movement. Traditional moving parts are mostly made of cast iron or steel, which have problems such as high motion inertia, high energy consumption, and poor vibration absorption, which restrict the improvement of machine tool rapid movement capability and machining accuracy.
[0003] In recent years, carbon fiber composites have been increasingly used in machine tool moving parts due to their high specific stiffness and low density. However, carbon fiber is expensive, and the damping performance of single carbon fiber composites remains limited. Furthermore, it is difficult to achieve a balance of strength, toughness, rigidity, and damping performance in a single or limited fiber system. In addition, the quality of the fiber-resin interface, bubble control, and molding precision are also key factors limiting the performance of moving parts. Therefore, developing a composite machine tool moving part that combines high strength, high toughness, high rigidity, high damping, low density, and dimensional stability is of great significance for improving the dynamic performance and machining accuracy of machine tools. Summary of the Invention
[0004] To address the shortcomings of existing machine tool moving parts, this invention provides a high-damping machine tool moving part. Through the synergistic effect of basalt fiber and carbon fiber composite, high-content mineral powder filling, epoxy resin system modification, and antimony and bismuth additives, the moving part's damping performance, dimensional stability, and crack resistance are significantly improved while maintaining high specific stiffness. It has excellent vibration absorption and damping capabilities, low thermal expansion coefficient, and lightweight advantages. It can effectively suppress vibration and thermal deformation of the moving part during high-speed movement, improve the machine tool's rapid movement capability, reduce energy consumption, and ensure the stability of various machine tool data. It is particularly suitable for high-speed, high-precision CNC machine tool moving parts.
[0005] To achieve the above objectives, the present invention provides the following technical solution: a high-damping machine tool moving part, which is formed by vacuum kneading, preforming, and molding curing of a composite material, wherein the composite material comprises, by weight, the following components: 30-35 parts basalt fiber, 2-5 parts carbon fiber, 27-35 parts mineral powder, A mixture of 30-35 parts epoxy resin and phenolic curing agent 0.1-0.2 parts defoamer; The composite material also contains additional antimony and bismuth additives, wherein the mass of the antimony additive is 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent, and the mass of the bismuth additive is 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent.
[0006] Furthermore, the basalt fiber has a length of 5-8 mm; the carbon fiber has a length of 3-8 mm.
[0007] Furthermore, by weight percentage, the mineral powder comprises: 57-59% silicon dioxide, 18-19% aluminum oxide, 8-9% calcium oxide, 5-6% magnesium oxide, 8-9% ferric oxide, and 0.7-1% titanium dioxide.
[0008] Furthermore, in the mixture of epoxy resin and phenolic curing agent, the mass ratio of epoxy resin to phenolic curing agent is 100:(35-45).
[0009] Furthermore, the antimony additive is antimony trioxide or organic antimony, and the bismuth additive is organic bismuth or bismuth oxide.
[0010] Furthermore, the moving parts of the machine tool are a worktable, a slide plate, a crossbeam, a spindle box, or a tool post.
[0011] On the other hand, the method for preparing the high-damping machine tool moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber and mineral powder according to the ratio, mix them evenly and heat them to above 120°C to remove moisture, and obtain the mixture. S2: Add antimony additive, bismuth additive, and defoamer to the mixture of epoxy resin and phenolic curing agent, stir evenly, and obtain colloidal modified resin; S3: Place the mixture in a vacuum device, evacuate the vacuum, preheat the colloidal modified resin to 80-100℃, add it to the device under vacuum conditions, and knead and stir it with the mixture and mineral powder for 20-30 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use an extrusion method to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, heat and pressurize it to form a molded product, keep it warm and pressurized, cool and demold it to obtain the finished machine tool moving part.
[0012] Furthermore, in S3, the vacuum level is 10-20 kPa.
[0013] Furthermore, in S4, the molding temperature is 150-180℃, the molding pressure is 10-15MPa, and the heat and pressure holding time is 1-2h.
[0014] The machine tool moving part of the present invention has the following beneficial effects: 1. High damping: The use of fiber-modified resin with antimony and bismuth improves the internal friction energy dissipation capacity of moving parts, and the vibration decay speed is fast, which can effectively suppress vibration and chatter during the processing.
[0015] 2. High strength and high rigidity: Basalt fiber provides the main strength, while carbon fiber improves the rigidity. Together, they enable moving parts to maintain excellent mechanical properties while being lightweight.
[0016] 3. Dimensional stability: The addition of antimony and bismuth additives reduces the coefficient of thermal expansion of the resin, resulting in a high degree of matching with the thermal expansion of the fiber. This leads to minimal deformation during temperature changes, ensuring long-term data stability of the machine tool.
[0017] 4. Lightweight: The density is about 1.98-2.02 g / cm³, which is only about 1 / 4 of that of cast iron. This significantly reduces the inertia of moving parts, which is beneficial for achieving rapid machine tool movement and reducing drive energy consumption.
[0018] 5. High molding precision: The combination of vacuum-assisted kneading and molding processes effectively eliminates air bubbles, ensuring the adhesion of internal materials and surface quality of the product. Detailed Implementation
[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] This invention provides a high-damping machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material comprises, by weight, the following components: 30-35 parts basalt fiber, 2-5 parts carbon fiber, 27-35 parts mineral powder, A mixture of 30-35 parts epoxy resin and phenolic curing agent 0.1-0.2 parts defoamer; The composite material also contains additional antimony and bismuth additives. The antimony additive accounts for 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent by mass, and the bismuth additive accounts for 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent by mass. The antimony and bismuth additives have a regulating effect on the thermal expansion behavior and curing shrinkage of the resin.
[0021] The composite material utilizes a combination of basalt fiber and carbon fiber, along with a mixture of mineral powder, epoxy resin, and phenolic curing agent, forming a multi-scale fiber-reinforced network. Basalt fiber provides high strength and stability, while carbon fiber imparts high rigidity and dimensional stability. This synergistic effect allows the moving parts to achieve both lightweight construction and excellent mechanical properties. The addition of antimony and bismuth additives effectively regulates the resin's thermal expansion behavior, reduces curing shrinkage, and improves dimensional stability. This formulation ensures that the moving parts exhibit comprehensive performance characteristics of high damping, high strength, low thermal expansion, and low density, making it suitable for high-speed, precision machine tool moving components.
[0022] In this invention, an acid anhydride curing agent can also be used as the phenolic curing agent.
[0023] In this invention, the basalt fiber has a length of 5-8 mm, and the carbon fiber has a length of 3-8 mm. This length range ensures good dispersion and wetting of the fiber in the resin, and also allows for the formation of an effective three-dimensional network structure during molding, fully leveraging the reinforcing, toughening, and stiffening effects of the fiber. Simultaneously, it helps improve the internal friction energy dissipation capacity of the composite material and enhances its damping performance.
[0024] In this invention, the mineral powder, by weight percentage, comprises 57-59% silicon dioxide, 18-19% aluminum oxide, 8-9% calcium oxide, 5-6% magnesium oxide, 8-9% ferric oxide, and 0.7-1% titanium dioxide. The mineral powder can uniformly fill the gaps between fibers, increasing the number of internal interfaces in the material, improving internal friction energy dissipation, and further enhancing the damping ratio.
[0025] In this invention, the mass ratio of epoxy resin to phenolic curing agent in the mixture is 100:(35-45). Epoxy resin is the base resin, possessing good fiber wettability and low curing shrinkage, making it suitable for use in conjunction with antimony and bismuth additives. This further improves the resin's thermal and dimensional stability, meeting the heat resistance and deformation resistance requirements of machine tool moving parts during high-speed operation.
[0026] In this invention, the antimony additive is antimony trioxide or organic antimony, and the bismuth additive is organic bismuth or bismuth oxide. Antimony trioxide, organic antimony, organic bismuth, or bismuth oxide are all additives that are easily and uniformly dispersed in the resin. Furthermore, the synergistic effect of antimony and bismuth can significantly reduce the coefficient of thermal expansion and curing shrinkage of the resin, ensuring the composite material maintains dimensional stability under temperature changes, preventing deformation of moving parts due to thermal expansion and contraction, and guaranteeing the data stability of the machine tool during long-term operation.
[0027] In this invention, the moving parts of the machine tool are worktables, slides, crossbeams, spindle boxes or tool holders. These parts bear dynamic loads and vibrations during machine tool operation. When made of the high-damping composite material of this invention, vibration transmission can be effectively suppressed, machining accuracy can be improved, and the weight of moving parts can be reduced, achieving rapid movement and energy saving.
[0028] In this invention, the method for preparing the high-damping machine tool moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber and mineral powder according to the ratio, mix them evenly and heat them to above 120°C to remove moisture, and obtain the mixture. S2: Add antimony additive, bismuth additive, and defoamer to the mixture of epoxy resin and phenolic curing agent, stir evenly, and obtain colloidal modified resin; S3: Place the mixture in a vacuum device, evacuate the vacuum, preheat the colloidal modified resin to 80-100℃, add it to the device under vacuum conditions, and knead and stir it with the mixture and mineral powder for 20-30 minutes to ensure that the resin fully impregnates the mixture and mineral powder and removes air bubbles; then extrude the kneaded material into a columnar preform; kneading under vacuum conditions can ensure that the resin uniformly impregnates the fibers and mineral powder, improving the adhesion between composite materials; preforming into a columnar shape can further remove air bubbles and facilitate subsequent molding operations; S4: Place the columnar preform into the mold, close the mold, heat and pressurize it for molding, maintain the temperature and pressure, cool and demold to obtain the finished machine tool moving part. Molding allows the material to fully solidify and cross-link under high temperature and high pressure, resulting in a high-density, high-strength moving part.
[0029] Preferably, in S3, the vacuum level is 10-20 kPa. This vacuum level can effectively eliminate air bubbles during the mixing process of fibers and resin, while avoiding excessive evaporation or curing of the resin, ensuring that the composite material is free of pores and has good interfacial bonding, thereby improving the mechanical and damping properties of the moving parts.
[0030] Preferably, in step S4, the molding temperature is 150-180℃, the molding pressure is 10-15MPa, and the holding time is 1-2 hours. These process conditions allow the epoxy resin system to fully cure and cross-link, forming a stable three-dimensional network structure, while ensuring high interfacial bonding strength between the fiber and resin and low internal residual stress. The resulting moving part exhibits high flexural strength, high elastic modulus, low linear expansion coefficient, and excellent dimensional stability, meeting the stringent requirements of high-end precision machine tools for moving parts.
[0031] The beneficial technical effects of the high-damping machine tool moving parts of the present invention will be described below through several embodiments and comparative examples. The mineral powder (58.05% silica, 18.07% alumina, 8.76% calcium oxide, 5.48% magnesium oxide, 8.76% ferric oxide, 0.88% titanium dioxide) formulation used in all the following embodiments and comparative examples is the same. Example
[0032] This example provides a composite material machine tool moving part for a CNC machine tool worktable. The part is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 32 parts basalt fiber, 4 parts carbon fiber, 30 parts mineral powder, 32 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), 0.1 parts defoamer, 0.08 parts antimony trioxide, and 0.08 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part. Example
[0033] This example provides a composite material machine tool moving part for a CNC machine tool worktable. The part is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 35 parts basalt fiber, 2 parts carbon fiber, 28 parts mineral powder, 34 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:35), 0.1 parts defoamer, 0.07 parts antimony trioxide, and 0.07 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part. Example
[0034] This example provides a composite material machine tool moving part for a CNC machine tool worktable. The part is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 30 parts basalt fiber, 5 parts carbon fiber, 35 parts mineral powder, 30 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:45), 0.15 parts defoamer, 0.09 parts antimony trioxide, and 0.09 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part. Example
[0035] This example provides a composite material machine tool moving part for a CNC machine tool worktable. The part is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 33 parts basalt fiber, 3 parts carbon fiber, 32 parts mineral powder, 33 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:42), 0.12 parts defoamer, 0.09 parts antimony trioxide, and 0.09 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0036] Comparative Example 1 This example provides a machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 32 parts basalt fiber, 4 parts carbon fiber, 30 parts mineral powder, 32 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), and 0.1 parts defoamer. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0037] Comparative Example 2 This example provides a machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 65 parts carbon fiber, 35 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), and 0.15 parts defoamer. The preparation method of the moving part includes the following steps: S1: Weigh the carbon fiber according to the ratio and dry it in an oven at 120℃ for 2 hours; S2: Add defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal resin; S3: Place the carbon fiber in a vacuum kneader and evacuate it to 15 kPa. Preheat the colloidal modified resin to 90°C and add it to the equipment under vacuum. Knead and stir it with the carbon fiber for 25 minutes to allow the resin to fully impregnate the fiber and remove air bubbles. Then, use an extrusion method to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0038] Comparative Example 3 This example provides a machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 32 parts basalt fiber, 4 parts carbon fiber, 32 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), 0.1 parts defoamer, 0.08 parts antimony trioxide, and 0.08 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber and carbon fiber according to the ratio, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture for 25 minutes to allow the resin to fully impregnate the mixture and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0039] Comparative Example 4 This example provides a machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 65 parts basalt fiber, 35 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), and 0.15 parts defoamer. The preparation method of the moving part includes the following steps: S1: Weigh the basalt fiber according to the ratio and dry it in an oven at 120℃ for 2 hours; S2: Add defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal resin; S3: Place the basalt fiber in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the basalt fiber for 25 minutes to allow the resin to fully impregnate the mixture and remove air bubbles; then use an extrusion method to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0040] Comparative Example 5 This example provides a machine tool moving part, which is made of composite material through vacuum kneading, preforming, and compression molding. The composite material, by weight, comprises: 20 parts basalt fiber, 15 parts carbon fiber, 30 parts mineral powder, 32 parts a mixture of epoxy resin and phenolic curing agent (weight ratio 100:40), 0.15 parts defoamer, 0.08 parts antimony trioxide, and 0.08 parts organic bismuth. The preparation method of the moving part includes the following steps: S1: Weigh basalt fiber, carbon fiber, and mineral powder according to the formula, mix them evenly, and dry them in an oven at 120℃ for 2 hours; S2: Add antimony trioxide, organic bismuth, and defoamer to the mixture of epoxy resin and phenolic curing agent, and stir for 10 minutes to obtain colloidal modified resin; S3: Place the mixture in a vacuum kneader, evacuate to 15 kPa, preheat the colloidal modified resin to 90°C, add it to the equipment under vacuum, and knead and stir it with the mixture and mineral powder for 25 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use extrusion to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, and mold it at 160℃ and 12MPa pressure for 1.5h. After heat preservation and pressure maintenance, cool to room temperature and demold to obtain the finished machine tool moving part.
[0041] Table 1. Performance comparison of machine tool moving parts in Examples 1-4 and Comparative Examples 1-5
[0042] Specific stiffness = elastic modulus / density: It represents the resistance to deformation that a material can provide under the same weight. Under the same weight, materials with higher specific stiffness are less likely to deform; a higher specific stiffness means that the same rigidity can be achieved with lighter materials. Damping ratio is determined using the free beam vibration attenuation method.
[0043] According to Table 1: 1. The damping ratios (0.030-0.035) of Examples 1-4 are significantly higher than those of all comparative examples, indicating that the present invention significantly improves the vibration absorption and damping capacity of moving parts through the synergistic effect of high content mineral powder, epoxy resin system and antimony and bismuth modification.
[0044] 2. Comparing Example 1 and Comparative Example 1, the addition of antimony and bismuth increased the damping ratio by approximately 45%, while the linear expansion coefficient decreased from 20 × 10⁻⁶. -6 / K decreased to 14×10 -6 K indicates that antimony and bismuth additives effectively reduced the thermal expansion and contraction rate of the resin and improved its dimensional stability.
[0045] 3. Comparing Example 1 and Comparative Example 3, the addition of mineral powder increased the damping ratio by about 60% and the elastic modulus by 60%, indicating that the filling of mineral powder increased the energy dissipation of interfacial friction within the material and played a reinforcing role.
[0046] 4. Comparative Example 2 uses pure carbon fiber, which has the highest specific stiffness but the worst damping and high cost; Comparative Example 4 uses pure basalt fiber, which has good damping but low strength and modulus. Examples 1-4, through reasonable fiber ratio and high mineral powder content, achieved damping performance far superior to Comparative Examples 2 and 5 while ensuring specific stiffness (17.9-19.8), resulting in the best overall performance.
[0047] 5. The densities of Examples 1-4 are 1.95-2.02 g / cm³, which are much lower than those of traditional cast iron (about 7.2 g / cm³). Their specific stiffness is close to or better than that of Comparative Example 3, and better than that of Comparative Example 4, which is beneficial for achieving rapid movement of machine tools and reducing energy consumption.
[0048] 6. Example 2 has the highest damping ratio (0.035), making it suitable for applications with extremely high vibration reduction requirements; Example 3 has the highest specific stiffness (19.8), making it suitable for moving parts with higher rigidity requirements.
[0049] In summary, embodiments 1-4 of the present invention significantly improve damping performance and dimensional stability while maintaining sufficient mechanical properties and specific stiffness. Their overall performance is superior to that of the comparative embodiments, and they are particularly suitable for moving parts of high-speed, high-precision CNC machine tools.
[0050] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A high-damping machine tool moving component, characterized in that: The composite material is formed by vacuum kneading, preforming, and compression molding, and the composite material comprises, by weight, the following components: 30-35 parts basalt fiber 2-5 parts carbon fiber 27-35 parts of mineral powder 30-35 parts of a mixture of epoxy resin and phenolic curing agent 0.1-0.2 parts of defoamer; The composite material also contains additional antimony and bismuth additives, wherein the mass of the antimony additive is 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent, and the mass of the bismuth additive is 0.2-0.3% of the mixture of epoxy resin and phenolic curing agent.
2. The high-damping machine tool moving part according to claim 1, characterized in that: The basalt fiber has a length of 5-8 mm; the carbon fiber has a length of 3-8 mm.
3. The high-damping machine tool moving part according to claim 1, characterized in that: The mineral powder comprises, by weight percentage: 57-59% silicon dioxide, 18-19% aluminum oxide, 8-9% calcium oxide, 5-6% magnesium oxide, 8-9% ferric oxide, and 0.7-1% titanium dioxide.
4. The high-damping machine tool moving part according to claim 1, characterized in that: In the mixture of epoxy resin and phenolic curing agent, the mass ratio of epoxy resin to phenolic curing agent is 100:(35-45).
5. The high-damping machine tool moving part according to claim 1, characterized in that: The antimony additive is antimony trioxide or organic antimony, and the bismuth additive is organic bismuth or bismuth oxide.
6. The high-damping machine tool moving part according to any one of claims 1 to 5, characterized in that: The moving parts of the machine tool are the worktable, slide plate, crossbeam, spindle box or tool post.
7. A method for preparing a high-damping machine tool moving part according to any one of claims 1-5, characterized in that: Includes the following steps: S1: Weigh basalt fiber, carbon fiber and mineral powder according to the ratio, mix them evenly and heat them to above 120°C to remove moisture, and obtain the mixture. S2: Add antimony additive, bismuth additive, and defoamer to the mixture of epoxy resin and phenolic curing agent, stir evenly, and obtain colloidal modified resin; S3: Place the mixture in a vacuum device, evacuate the vacuum, preheat the colloidal modified resin to 80-100℃, add it to the device under vacuum conditions, and knead and stir it with the mixture and mineral powder for 20-30 minutes to allow the resin to fully impregnate the mixture and mineral powder and remove air bubbles; then use an extrusion method to form the kneaded material into a columnar preform. S4: Place the columnar preform into the mold, close the mold, heat and pressurize it to form a molded product, keep it warm and pressurized, cool and demold it to obtain the finished machine tool moving part.
8. The preparation method according to claim 7, characterized in that: In S3, the vacuum level is 10-20 kPa.
9. The preparation method according to claim 7, characterized in that: In S4, the molding temperature is 150-180℃, the molding pressure is 10-15MPa, and the heat and pressure holding time is 1-2h.
Citation Information
Patent Citations
Halogen-free flame retardant basalt fiber reinforced unsaturated polyester resin composite material and preparation method thereof
CN104629238A
Automobile parts and preparation method thereof
CN109486117A