Wide flange hot rolled h-beam having a thickness of 20~80mm and a production method thereof
By optimizing specific component ratios and processes, the problems of high hydrogen content and high production costs of existing wide-flange hot-rolled H-beams have been solved, and 20-80mm thick hot-rolled H-beams with the requirements of underground engineering and building structures have been produced, achieving cost reduction and performance improvement.
Patent Information
- Application Number
- CN202610410190.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-31
- Publication Date
- 2026-06-23
AI Technical Summary
Existing wide-flange hot-rolled H-beams have high hydrogen content requirements, complex processes, high production costs, and flange thicknesses that do not meet conventional thickness requirements, making them difficult to widely apply in underground engineering and building structures.
We design wide-flange hot-rolled H-beams with a thickness of 20-80mm, containing Fe and trace elements in a specific composition ratio. We employ hot metal pretreatment, converter smelting, argon blowing refining, LF refining, special-shaped billet casting, billet heating, billet rolling, universal finishing rolling, and post-rolling controlled cooling processes to ensure that the product yield strength level meets Q355-Q420 and the impact performance meets B-C level.
Hot-rolled H-beams with flange thickness of 20~80mm and flange width of 400mm~500mm are produced, with yield strength and impact performance meeting the requirements, satisfying the needs of underground engineering and building structures, and reducing production costs and process complexity.
Smart Images

Figure CN122256831A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal material production technology, specifically to a wide-flange hot-rolled H-beam with a thickness of 20-80mm and its production method. Background Technology
[0002] As a core component of steel structure buildings, hot-rolled H-beams demonstrate significant advantages in multiple fields due to their unique cross-sectional design and excellent mechanical properties: in high-rise buildings, their high strength and lightweight characteristics greatly improve the safety and economy of the building; in industrial plant construction, standardized production significantly shortens the construction cycle; in bridge engineering, their excellent bending resistance ensures structural stability; and in rail transit, their durability effectively extends the service life of the facilities.
[0003] In the field of underground engineering construction, ultra-wide H-beams (flange width ≥ 400mm) are gradually becoming the core material of foundation pit support systems. Ultra-wide H-beams, with their ultra-large cross-sectional moment of inertia (up to 2-3 times that of ordinary H-beams), can effectively resist the lateral pressure of deep soil. Furthermore, through innovative "steel-concrete composite support" technology, ultra-wide H-beams achieve a perfect integration of the support structure and the main structure, shortening the construction period and saving concrete usage in engineering applications.
[0004] Due to limitations in equipment capacity, the main specifications and dimensions of wide-flange hot-rolled H-beams in China are currently concentrated in the range of B < 400mm. For projects such as underground water conservancy and foundation pit support, the connection between hot-rolled H-beams and sheet piles effectively achieves functions such as water stopping and protection. However, for large-area foundation pit structures, due to the narrower flange width of hot-rolled H-beams, using 500mm wide hot-rolled H-beams saves approximately 25% of material per meter compared to using 400mm wide ones.
[0005] Chinese patent "A wide-flange heavy hot-rolled H-beam and its production method and application" (publication number CN113604740B) specifies the following steel composition by mass percentage: C: 0.11~0.15%, Si: 0.35~0.45%, Mn: 1.30~1.60%, P: ≤0.015%, S: ≤0.015%, V: 0.03~0.05%, Nb: 0.030~0.050%, H: ≤0.0002%, N: ≤0.008%, Alt: 0.010~0.015%. The remainder consists of Fe and trace residual elements. During the rough rolling stage, the die design was optimized to allow for sufficient web thickness and improve the metal distribution between the flanges and web, providing more metal for the flange width. This results in wide-flange heavy-duty hot-rolled H-beams with a flange width ≥500mm and a flange thickness of 80~140mm. The product meets the load-bearing capacity requirements of hot-rolled H-beams for foundation pit support in high-rise and super high-rise buildings. However, this invention requires extremely low levels of hydrogen, necessitating special refining and degassing processes, such as VD or RH processes.
[0006] The aforementioned wide-flange heavy hot-rolled H-beams with flange thicknesses of 80-140mm have the following technical problems: First, from the current market perspective, there are no physical applications yet; Second, the product requires a high hydrogen content, the process is complex, and the production cost is high. Third, the flange thickness is above 80mm, which is mainly used in ultra-large underground engineering projects. The composition control precision is extremely high, which does not meet the application requirements of conventional thickness wide-flange hot-rolled H-beams, and is not conducive to the promotion and application of practical projects. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention proposes a wide-flange hot-rolled H-beam with a thickness of 20-80mm and its production method. This method has no hydrogen content requirements, a simple process, and low production costs. It develops products with flange thicknesses of 20-80mm and flange widths of 400mm-500mm, achieving yield strength levels of Q355-Q420 and impact performance levels of B-C, thus meeting the needs of underground engineering and building structure industries for wide-flange hot-rolled H-beams.
[0008] To achieve the above objectives, this invention designs a wide-flange hot-rolled H-beam with a thickness of 20-80mm, comprising Fe and trace residual elements, and is particularly characterized by further comprising 0.15-0.20 parts of carbon, 0.20-0.40 parts of silicon, 1.20-1.60 parts of manganese, 0-0.025 parts of phosphorus, 0-0.015 parts of sulfur, 0-0.030 parts of niobium, 0.020-0.100 parts of vanadium, and 0.010-0.025 parts of aluminum, in parts by weight. The specifications of the wide-flange hot-rolled H-beams range from 20mm to 80mm in flange thickness, 400mm to 1000mm in web height, 400mm to 500mm in flange width, and a web height / flange width ratio of 1.0 to 2.0. The strength grade of the wide-flange hot-rolled H-beams meets the requirements of Q355~Q420, and the impact performance meets the requirements of B~C.
[0009] Furthermore, for Q355 grade products, the vanadium alloy addition range is 0.020%~0.050% for 20~60mm flange thickness and 0.050%~0.080% for 60~80mm flange thickness. For Q390~Q420 grade products, with a flange thickness of 20~60mm, the vanadium alloy addition range is 0.030%~0.060%, and with a flange thickness of 60~80mm, the vanadium alloy addition range is 0.060%~0.100%.
[0010] Furthermore, for Q355-level products, the vanadium alloy content is 0.030% for 20~60mm flange thickness and 0.060% for 60~80mm flange thickness. For Q390~Q420 grade products, the vanadium alloy addition is 0.050% for 20~60mm flange thickness and 0.080% for 60~80mm flange thickness.
[0011] This invention also provides a method for producing wide-flange hot-rolled H-beams with a thickness of 20-80mm, applicable to the aforementioned wide-flange hot-rolled H-beams with a thickness of 20-80mm, characterized by the following steps: S1) Hot metal pretreatment, converter smelting, argon blowing refining, LF refining; S2) Casting of irregularly shaped billets; S3) Billet heating; S4) Billet rolling; The initial rolling temperature is 1120℃~1160℃, and the final rolling temperature is not lower than 1050℃, ensuring that the temperature before the initial rolling section is higher than the complete recrystallization temperature of austenite. S5) Universal precision rolling; The initial rolling temperature shall not exceed 1050℃, and different universal rolling passes shall be designed for products with different flange thicknesses; details are as follows: For products with a diameter of 20-40mm, the universal rolling process should be no less than 9 passes. For products with a diameter of 40-60mm, the universal rolling process should be completed in no fewer than 7 passes. For products with a diameter of 60-80mm, the universal rolling process should be carried out in no less than 5 passes. S6) For finished products with a thickness of 60mm or more and a steel grade higher than Q390, the post-rolling controlled cooling process is adopted; for other rolled parts, the post-rolling air cooling process control in step S7) is adopted. S7) Air cooling after rolling; S8) Fixed-length straightening.
[0012] Further, in S2), the ratio of the width to the web thickness of the selected irregular billet is 3.8 to 4.0, and the ratio of the billet height to the flange thickness is 6.5 to 7.0; or the ratio of the width to the web thickness of the selected irregular billet is 3.5 to 3.8, and the ratio of the billet height to the flange thickness is 7.0 to 7.5.
[0013] Furthermore, in S3), the heating temperature in the furnace is 1220℃~1280℃, the furnace time is 120 min~180 min, and the temperature of the soaking zone is 35 min~55 min, to ensure that the austenite grain size grade is not lower than 8.5. Furthermore, in S4), if a billet with a width-to-web thickness ratio of 3.8 to 4.0 and a height-to-flange thickness ratio of 6.5 to 7.0 is selected, the entire billet opening stage will achieve a cross-sectional compression ratio of not less than 20%. If the ratio of billet width to web thickness is 3.5 to 3.8 and the ratio of billet height to flange thickness is 7.0 to 7.5, the entire billet opening stage will achieve a cross-sectional compression ratio of no less than 30%.
[0014] Furthermore, in S5), for products with a specification of 20~40mm, low-speed, light-reduction rolling is used in the first 20% of universal rolling passes, with the cumulative flange reduction not exceeding 25% and the rolling speed not exceeding 3.0m / s; high-speed, high-reduction rolling is used in the first 20%~70% of universal rolling passes, with the rolling temperature not exceeding 970℃, the rolling speed not less than 3.5m / s, the cumulative flange reduction not less than 50%, and the single-pass reduction rate of flange reduction and web reduction not exceeding 10%; light-reduction rolling is used in the last 20% of universal rolling passes, with the cumulative flange reduction not exceeding 20%. For products with a diameter of 40-60mm, the first 20% of universal rolling passes shall use low-speed, light-reduction rolling, with a cumulative flange reduction not exceeding 25% and a rolling speed not exceeding 3.0m / s; the first 20% to 70% of universal rolling passes shall use high-speed, high-reduction rolling, with a rolling temperature not exceeding 970℃, a rolling speed not less than 3.5m / s, a cumulative flange reduction not less than 50%, and a single-pass reduction rate for both flanges and web not exceeding 10%; the last 20% of universal rolling passes shall use light-reduction rolling, with a cumulative flange reduction not less than 15%. For products with a diameter of 60-80mm, low-speed, light-reduction rolling is used in the first 20% of universal rolling passes, with the cumulative reduction of the flanges not exceeding 20% and the rolling speed not exceeding 3.0m / s; high-speed, high-reduction rolling is used in the first 20% to 70% of universal rolling passes, with the rolling temperature not exceeding 970℃, the rolling speed not less than 3.5m / s, the cumulative reduction of the flanges not less than 40%, and the single-pass reduction rate of the flanges and web not exceeding 10%; light-reduction rolling is used in the last 20% of universal rolling passes, with the cumulative reduction of the flanges not less than 10%.
[0015] Furthermore, in S6), the post-rolling controlled cooling process includes: the cooling time at the same rolling position does not exceed 15s, and the surface temperature of the rolled piece after cooling does not exceed 700℃.
[0016] The advantages of this invention are: 1. This invention designs a production process for hot-rolled H-beams with flange thickness of 20mm~80mm and flange width of 400mm~500mm. The yield strength of the product meets the requirements of Q355~Q420, and the impact performance meets the requirements of B~C level. 2. The wide-flange hot-rolled H-beam produced by this invention breaks through the existing shape control technology for rolling wide-flange hot-rolled H-beams. The product has high precision and a wider flange width, meeting the needs of underground engineering and building structure industries.
[0017] This invention relates to a wide-flange hot-rolled H-beam with a thickness of 20-80mm and its production method. Based on existing production equipment and combined with actual production conditions, it develops a product with a flange thickness of 20-80mm and a flange width of 400mm-500mm. The product's yield strength level meets the Q355-Q420 level, and its impact performance meets the B-C level, thus meeting the needs of the underground engineering and building structure industries for wide-flange hot-rolled H-beams. Attached Figure Description
[0018] Figure 1 The blank structure is labeled in the embodiments of the present invention; Figure 2 This is a process flow diagram of the production method of wide-flange hot-rolled H-beams with a thickness of 20~80mm according to the present invention. Detailed Implementation
[0019] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0020] This invention discloses a wide-flange hot-rolled H-beam with a thickness of 20-80 mm, comprising Fe and trace residual elements, and further comprising 0.15-0.20 parts of C, 0.20-0.40 parts of Si, 1.20-1.60 parts of Mn, 0-0.025 parts of P, 0-0.015 parts of S, 0-0.030 parts of Nb, 0.020-0.100 parts of V, and 0.010-0.025 parts of Al, in parts by weight.
[0021] The specifications of the hot-rolled H-beams are as follows: flange thickness 20mm~80mm, web height H (model) 400mm~1000mm, flange width B (model) 400mm~500mm, and web height H / flange width B ratio 1.0~2.0. The billet structure in this embodiment is shown in the attached figure. Figure 1 As shown.
[0022] The strength grade of the hot-rolled H-beams meets the requirements of Q355~Q420, and the impact performance meets the requirements of B~C. Among them, the longitudinal impact energy value of grade B (20℃) is not less than 100J, and the longitudinal impact energy value of grade C (0℃) is not less than 80J.
[0023] Specifically, the roles and proportions of each element are as follows: Carbon (C): Carbon is the most basic element in steel. Through its combination with other elements, it plays a significant role in improving the strength of steel. In order to meet the requirements of high strength level, and considering the high strength requirements of the product, the lower limit is set at 0.15 wt%; considering the difficulty of controlling the steelmaking process and the adverse effects on the plasticity of the material caused by excessive carbon content, the upper limit is set at 0.20 wt%.
[0024] Silicon (Si): It exists in steel in solid solution form and has a strong solid solution strengthening effect, which can significantly strengthen ferrite. To obtain high strength, the lower limit is set at 0.20 wt%; however, when Si is higher than 0.55%, the toughness and plasticity of steel decrease significantly, and the upper limit is set at 0.40 wt%.
[0025] Manganese (Mn): Effectively inhibits the transformation of ferrite to pearlite, greatly improving the low-temperature toughness of the material. It can also lower the phase transformation temperature, which is beneficial for the transformation of austenite under low-temperature conditions. However, excessive manganese content can cause segregation defects inside the cast billet; therefore, the Mn content should be controlled between 1.20 and 1.60 wt%.
[0026] Phosphorus (P): It is prone to segregation in steel, which greatly reduces the plasticity and toughness of steel and has a certain impact on the surface quality of steel. Considering the difficulty of removing P in the steelmaking process, the upper limit is set at 0.025 wt%.
[0027] Sulfur (S): It has a significant impact on the toughness of steel. It is easy to accumulate and segregate within and at the grain boundaries. In particular, it readily forms MnS inclusions with manganese, making the matrix structure of the material prone to the boundary origin of cracks. Considering the difficulty of desulfurization in the steelmaking process, the upper limit is set at 0.015 wt%.
[0028] Niobium (Nb): A strong carbide-forming element, Nb (C, N) dispersions formed with C and N are distributed in the steel matrix, playing a role in precipitation strengthening and improving toughness. The addition of Nb can inhibit austenite recrystallization during rolling, expanding the austenite non-recrystallization temperature range. The cumulative deformation under subsequent low-temperature, high-pressure conditions can elongate austenite grains, forming numerous deformation bands and dislocations at grain boundaries. These provide nucleation sites during subsequent phase transformations, refining the grains. Considering the selectability of niobium content and the adverse effects of excessively high niobium content on billet quality, an upper limit of 0.030 wt% is set. Furthermore, to enhance precipitation strengthening, niobium and vanadium can be added simultaneously, and the alloying effect of niobium content is equivalent to adding twice the amount of vanadium.
[0029] Vanadium (V): Vanadium is one of the most important microalloying elements in steel, exhibiting significant grain refinement strengthening, precipitation strengthening, and sedimentation strengthening effects. Vanadium readily forms carbonitrides with nitrogen, effectively preventing excessive grain growth, promoting the transformation of austenite to ferrite, facilitating the precipitation of soft and tough phases, and improving the low-temperature toughness of the material. Furthermore, during the post-rolling cooling process, the precipitation of carbonitrides plays a certain strengthening role. Considering the strengthening effect of vanadium, a lower limit of 0.020 wt% is set. However, due to limitations in the actual rolling process control, excessively high vanadium content cannot effectively precipitate VN particles, thus having no significant impact on the actual mechanical properties of the steel. Moreover, excessive vanadium alloying elements would lead to a dramatic increase in production costs; therefore, an upper limit of 0.100 wt% is set.
[0030] For different flange thicknesses, to ensure strength, for Q355 grade products, the vanadium alloy addition range is 0.020%~0.050% for flange thicknesses of 20mm~60mm and 0.050%~0.080% for flange thicknesses of 60mm~80mm; for Q390~Q420 grade products, the vanadium alloy addition range is 0.030%~0.060% for flange thicknesses of 20mm~60mm and 0.060%~0.100% for flange thicknesses of 60mm~80mm.
[0031] Preferably, for Q355 grade products, the vanadium alloy addition is 0.030% for a flange thickness of 20~60mm and 0.060% for a flange thickness of 60~80mm; for Q390~Q420 grade products, the vanadium alloy addition is 0.050% for a flange thickness of 20~60mm and 0.080% for a flange thickness of 60~80mm.
[0032] Aluminum (Al): A strong oxidizing element that can be used for deoxidation in steelmaking. In addition, aluminum can precipitate in combination with nitrogen, which can refine austenite grains; the lower limit is set at 0.010 wt%. However, excessive aluminum content significantly reduces the plasticity and toughness of the material, and it can easily cause brittle formation in continuously cast irregular billets, leading to leaks and affecting production safety; the upper limit is set at 0.025 wt%.
[0033] As attached Figure 2 As shown, the present invention also designs a method for producing wide-flange hot-rolled H-beams with a thickness of 20-80mm, applicable to the aforementioned wide-flange hot-rolled H-beams with a thickness of 20-80mm, comprising the following steps: S1) Hot metal pretreatment, converter smelting, argon blowing refining, LF refining.
[0034] Preferably, in S1), the LF refining process is followed by RH refining or VD refining.
[0035] S2) Casting of irregularly shaped billets.
[0036] For ultra-wide hot-rolled H-beams, there is a certain correspondence between the length and width of the original special-shaped billet, as well as the thickness of the web and the flange.
[0037] For finished hot-rolled H-beams with a height H to width B ratio in the range of 1.0 to 2.0, considering the control of the H-beam's external dimensions and a certain compression ratio, a billet width to web thickness ratio of 3.8 to 4.0 and a billet height to flange thickness ratio of 6.5 to 7.0 are selected; or a billet width to web thickness ratio of 3.5 to 3.8 and a billet height to flange thickness ratio of 7.0 to 7.5 are selected.
[0038] The specifications of the irregularly shaped billets selected in this embodiment are shown in Table 1 below.
[0039] Table 1 Specifications of irregularly shaped billets S3) Heating of billet.
[0040] After the blank is selected, the irregular blank is heated.
[0041] Specifically, the shaped billet is heated in the furnace at a temperature of 1220℃~1280℃ for 120 min~180 min, with a soaking temperature of 35 min~55 min, ensuring that the austenite grain size is not lower than grade 8.5. At the same time, excessive heating time is prevented to avoid austenite grain growth, which would adversely affect the original microstructure of subsequent rolling. The billet temperature after descaling is ensured to be not lower than 1150℃ before being sent to the billet mill for rolling.
[0042] In this embodiment, the wide-flange hot-rolled H-beam products produced using the production method described in this invention include Q355 grade products and Q390~Q420 grade products.
[0043] Among them, the Q355 grade products include Examples 1 to 8 and Comparative Examples 1 to 11, which are produced using the above 8 special-shaped billet specifications, and their chemical compositions are shown in Table 2 below.
[0044] Table 2 Chemical composition of Examples 1-8 and Comparative Examples 1-11 (Q355 grade) The Q390~Q420 grade products include Examples 9~15 and Comparative Examples 12~23, which are produced using the above 8 special-shaped billet specifications, and their chemical compositions are shown in Table 3 below.
[0045] Table 3 Chemical composition (Q390~Q420 grade) of Examples 9-15 and Comparative Examples 12-23 S4) Rolling of billets.
[0046] Before rolling on the billet mill, high-pressure water descaling should be performed (high-pressure water descaling is a technology that removes iron oxide scale from the surface of hot-rolled steel billets by high-pressure water jets, mainly used to improve the surface quality of steel). Descaling must ensure that the billet surface is clean and free of residual iron oxide scale.
[0047] Specifically, the initial rolling temperature is 1120℃~1160℃, and the final rolling temperature is not lower than 1050℃, ensuring that the temperature before the initial rolling section is higher than the temperature at which austenite is fully recrystallized.
[0048] If a billet with a width-to-web thickness ratio of 3.8 to 4.0 and a height-to-flange thickness ratio of 6.5 to 7.0 is selected, the entire billet-making stage will achieve a cross-sectional compression ratio of no less than 20%.
[0049] If the ratio of billet width to web thickness is 3.5 to 3.8 and the ratio of billet height to flange thickness is 7.0 to 7.5, the entire billet opening stage will achieve a cross-sectional compression ratio of no less than 30%.
[0050] The reduction action of the initial rolling process refines the original austenite grains, promotes the formation of grain boundaries in the fine austenite structure, increases the grain boundary orientation difference of the original structure, and facilitates the subsequent transformation of austenite into ferrite and pearlite.
[0051] S5) Universal precision rolling.
[0052] The initial rolling temperature does not exceed 1050℃. This process mainly ensures large deformation during continuous rolling, achieving compression changes in the flange thickness of the irregularly shaped billet, and ensuring synchronous deformation of the flange and web throughout the finishing rolling stage. This guarantees both product performance and the dimensional specifications of the wide-flange hot-rolled H-beams. The process design for universal finishing rolling is as follows for different products.
[0053] If a billet with a width-to-web thickness ratio of 3.8~4.0 and a height-to-flange thickness ratio of 6.5~7.0 is selected, then different universal rolling passes will be designed for products with different flange thicknesses. Specifically: For products with a diameter of 20-40mm, the universal rolling process shall consist of no fewer than 9 passes. The first 20% of universal rolling passes shall use low-speed, light-reduction rolling, with a cumulative flange reduction not exceeding 25% and a rolling speed not exceeding 3.0 m / s. The first 20% to 70% of universal rolling passes shall use high-speed, high-reduction rolling, with a rolling temperature not exceeding 970℃, a rolling speed not less than 3.5 m / s, a cumulative flange reduction not less than 50%, and a single-pass reduction rate for both flanges and the web not exceeding 10%. The last 20% of universal rolling passes shall use light-reduction rolling, with a cumulative flange reduction not exceeding 20%.
[0054] For products with a diameter of 40-60mm, the universal rolling process shall consist of no fewer than 7 passes. The first 20% of universal rolling passes shall use low-speed, light-reduction rolling, with a cumulative flange reduction not exceeding 25% and a rolling speed not exceeding 3.0 m / s. The first 20% to 70% of universal rolling passes shall use high-speed, high-reduction rolling, with a rolling temperature not exceeding 970℃, a rolling speed not less than 3.5 m / s, a cumulative flange reduction not less than 50%, and a single-pass reduction rate for both flanges and the web not exceeding 10%. The last 20% of universal rolling passes shall use light-reduction rolling, with a cumulative flange reduction not less than 15%.
[0055] For products with a diameter of 60-80mm, the universal rolling process shall be no less than 5 passes. The first 20% of universal rolling passes shall use low-speed, light-reduction rolling, with a cumulative flange reduction not exceeding 20% and a rolling speed not exceeding 3.0 m / s. The first 20% to 70% of universal rolling passes shall use high-speed, high-reduction rolling, with a rolling temperature not exceeding 970℃, a rolling speed not less than 3.5 m / s, a cumulative flange reduction not less than 40%, and a single-pass reduction rate for both flanges and web not exceeding 10%. The last 20% of universal rolling passes shall use light-reduction rolling, with a cumulative flange reduction not less than 10%.
[0056] In this embodiment, the rolling process of the universal rolling passes of Examples 1 to 8 is shown in Table 4.
[0057] Table 4 Rolling process for universal rolling passes (Q355 grade) in Examples 1-8 In this embodiment, the rolling process for the universal rolling passes of Comparative Examples 1 to 11 is shown in Table 5.
[0058] Table 5 Rolling process for universal rolling passes of comparative examples 1-11 (Q355 grade) In this embodiment, the rolling process for the universal rolling passes of Examples 9 to 15 is shown in Table 6.
[0059] Table 6 Rolling process for universal rolling passes (Q390~Q420 grade) in Examples 9~15 In this embodiment, the rolling process for the 12-23 universal rolling passes of comparative examples is shown in Table 7.
[0060] Table 7 Rolling process for universal rolling passes of comparative examples 11-23 (Q390-Q420 grade) S6) Controlled cooling after rolling.
[0061] Based on the product's steel grade and thickness effect, the rolled parts after universal precision rolling are subjected to controlled cooling treatment.
[0062] For finished products with a thickness of 60mm or more and a steel grade higher than Q390, a controlled cooling process after rolling is adopted; for other rolled products, a controlled air cooling process after rolling is adopted.
[0063] Specifically, the post-rolling controlled cooling process includes: the cooling time at the same position of the rolled piece does not exceed 15 seconds, and the surface temperature of the rolled piece after cooling does not exceed 700℃.
[0064] S7) Air cooling.
[0065] After rolling, the rolled piece is transported to the cooling bed by the transport roller conveyor and air-cooled to room temperature.
[0066] S8) Fixed-length straightening.
[0067] The finished products on the cooling bed are cut into multiple lengths or fixed lengths, with the fixed length range being 12~24m. The cut products are then transported to the straightening machine to straighten their shape.
[0068] The production method also includes step S9) bundling: bundling and packaging the finished products of fixed length and storing them in the warehouse for shipment.
[0069] In this embodiment, Examples 1-8 and Comparative Examples 1-11 were constructed as a comparative group to analyze the mechanical properties of the finished products. The specific comparative pairings are shown in Table 8 below. The mechanical properties of Examples 1-8 are shown in Table 9. The mechanical properties of Comparative Examples 1-11 are shown in Table 10.
[0070] Table 8 Comparison pairing of Examples 1-8 with Comparative Examples 1-11 (Q355 grade) Table 9 Mechanical properties of Examples 1-8 (Q355 grade) As can be seen from Table 9, the hot-rolled H-beams in Examples 1-8 have a flange thickness of 20-75 mm, a yield strength of 370 MPa-388 MPa, a tensile strength of 508 MPa-535 MPa, an elongation of 23.0%-26.0%, a longitudinal impact energy value of 135 J-173 J at 20°C (not less than 100 J), and a transverse impact energy value of 99 J-120 J at 0°C (not less than 80 J), meeting the usage requirements of domestic and international underground engineering and building structure industries.
[0071] Table 10 Mechanical properties of comparative examples 1-11 (Q355 grade) As can be seen from Table 10, the hot-rolled H-beams in Comparative Examples 1 to 11 have flange thicknesses of 20 to 75 mm, yield strengths of 325 MPa to 438 MPa, tensile strengths of 489 MPa to 642 MPa, elongation of 20.0% to 25.0%, longitudinal impact energy values at 20°C of 98 J to 162 J (some are below the 100 J requirement), and transverse impact energy values at 0°C of 75 J to 132 J (some are below the 80 J requirement), which do not meet the usage requirements of domestic and international underground engineering and building structure industries.
[0072] In this embodiment, Examples 9-15 and Comparative Examples 12-23 were constructed as a comparative group to analyze the mechanical properties of the finished products. The specific comparative pairings are shown in Table 11 below. The mechanical properties of Examples 9-15 are shown in Table 12. The mechanical properties of Comparative Examples 12-23 are shown in Table 13.
[0073] Table 11 Comparison pairing of Examples 9-15 with Comparative Examples 12-23 (Q390-Q420 levels) Table 12 Mechanical properties of Examples 9-15 (Q390-Q420 grade) As can be seen from Table 12, the hot-rolled H-beams in Examples 9-15 have a flange thickness of 25-75 mm, a yield strength of 422 MPa-450 MPa, a tensile strength of 638 MPa-652 MPa, an elongation of 23.5%-26.0%, a longitudinal impact energy value of 138 J-168 J at 20°C (not less than 100 J), and a transverse impact energy value of 98 J-120 J at 0°C (not less than 80 J), meeting the usage requirements of domestic and international underground engineering and building structure industries.
[0074] Table 13 Mechanical properties of comparative examples 12-23 (Q390-Q420 grade) As can be seen from Table 13, the hot-rolled H-beams in Comparative Examples 12-23 have a flange thickness of 25-75 mm, a yield strength of 358 MPa-450 MPa, a tensile strength of 522 MPa-668 MPa, an elongation of 23.5%-25.0%, and a longitudinal impact energy value of 124 J-168 J at 20℃, which is not lower than the requirement of 100 J; the transverse impact energy value at 0℃ is 79 J-120 J, some of which are lower than the requirement of 80 J, and do not meet the usage requirements of the domestic and international underground engineering and building structure industries.
[0075] This production method also includes step S9) bundling: bundling and packaging the finished products of fixed length and storing them in the warehouse for shipment.
[0076] This invention relates to a method for producing wide-flange hot-rolled H-beams with a thickness of 20-80mm. The method utilizes a process of initial rolling + universal finishing rolling + controlled cooling after rolling to obtain hot-rolled H-beams with a flange thickness of 20-80mm and a flange width of 400-500mm. The yield strength meets the requirements of Q355-Q420, and the impact performance meets the requirements of Class B (20℃) longitudinal impact energy value not less than 100J and Class C (0℃) longitudinal impact energy value not less than 80J, satisfying the usage requirements of domestic and international underground engineering and building structure industries.
[0077] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A wide-flange hot-rolled H-beam with a thickness of 20-80 mm, comprising Fe and trace residual elements, characterized in that: It also includes 0.15–0.20 parts carbon, 0.20–0.40 parts silicon, 1.20–1.60 parts manganese, 0–0.025 parts phosphorus, 0–0.015 parts sulfur, 0–0.030 parts niobium, 0.020–0.100 parts vanadium, and 0.010–0.025 parts aluminum, in parts by weight. The specifications of the wide-flange hot-rolled H-beams range from 20mm to 80mm in flange thickness, 400mm to 1000mm in web height, 400mm to 500mm in flange width, and a web height / flange width ratio of 1.0 to 2.
0. The strength grade of the wide-flange hot-rolled H-beams meets the requirements of Q355~Q420, and the impact performance meets the requirements of B~C.
2. The 20-80mm thick wide-flange hot-rolled H-beam according to claim 1, characterized in that: For Q355-level products, with a flange thickness of 20~60mm, the vanadium alloy addition range is 0.020%~0.050%; with a flange thickness of 60~80mm, the vanadium alloy addition range is 0.050%~0.080%. For Q390~Q420 grade products, with a flange thickness of 20~60mm, the vanadium alloy addition range is 0.030%~0.060%, and with a flange thickness of 60~80mm, the vanadium alloy addition range is 0.060%~0.100%.
3. The 20-80mm thick wide-flange hot-rolled H-beam according to claim 2, characterized in that: For Q355-level products, the vanadium alloy addition is 0.030% for 20~60mm flange thickness and 0.060% for 60~80mm flange thickness. For Q390~Q420 grade products, the vanadium alloy addition is 0.050% for 20~60mm flange thickness and 0.080% for 60~80mm flange thickness.
4. A method for producing wide-flange hot-rolled H-beams with a thickness of 20-80 mm, applicable to the wide-flange hot-rolled H-beams with a thickness of 20-80 mm as described in any one of claims 1-4, characterized in that, Includes the following steps: S1) Hot metal pretreatment, converter smelting, argon blowing refining, LF refining; S2) Casting of irregularly shaped billets; S3) Billet heating; S4) Billet rolling; The initial rolling temperature is 1120℃~1160℃, and the final rolling temperature is not lower than 1050℃, ensuring that the temperature before the initial rolling section is higher than the complete recrystallization temperature of austenite. S5) Universal precision rolling; The initial rolling temperature shall not exceed 1050℃, and different universal rolling passes shall be designed for products with different flange thicknesses; details are as follows: For products with a diameter of 20-40mm, the universal rolling process should be no less than 9 passes. For products with a diameter of 40-60mm, the universal rolling process should be completed in no fewer than 7 passes. For products with a diameter of 60-80mm, the universal rolling process should be carried out in no less than 5 passes. S6) For finished products with a thickness of 60mm or more and a steel grade higher than Q390, the post-rolling controlled cooling process is adopted; for other rolled parts, the post-rolling air cooling process control in step S7) is adopted. S7) Air cooling after rolling; S8) Fixed-length straightening.
5. The method for producing 20-80mm thick wide-flange hot-rolled H-beams according to claim 4, characterized in that: In S2), the ratio of the width to the web thickness of the selected irregular billet is 3.8 to 4.0, and the ratio of the billet height to the flange thickness is 6.5 to 7.0; or the ratio of the width to the web thickness of the selected irregular billet is 3.5 to 3.8, and the ratio of the billet height to the flange thickness is 7.0 to 7.
5.
6. The method for producing 20-80mm thick wide-flange hot-rolled H-beams according to claim 5, characterized in that: In S3), the heating temperature in the furnace is 1220℃~1280℃, and the furnace time is 120 min~180 min, of which the temperature of the soaking zone is 35 min~55 min, to ensure that the austenite grain size grade is not lower than 8.
5.
7. The method for producing 20-80mm thick wide-flange hot-rolled H-beams according to claim 6, characterized in that: In S4), if a billet with a width-to-web thickness ratio of 3.8 to 4.0 and a height-to-flange thickness ratio of 6.5 to 7.0 is selected, the entire billet opening stage will achieve a cross-sectional compression ratio of no less than 20%. If the ratio of billet width to web thickness is 3.5 to 3.8 and the ratio of billet height to flange thickness is 7.0 to 7.5, the entire billet opening stage will achieve a cross-sectional compression ratio of no less than 30%.
8. The method for producing 20-80mm thick wide-flange hot-rolled H-beams according to claim 4, characterized in that: In S5), for products with a diameter of 20-40mm, low-speed, light-reduction rolling is used in the first 20% of universal rolling passes, with a cumulative flange reduction of no more than 25% and a rolling speed of no more than 3.0m / s; high-speed, high-reduction rolling is used in the first 20% to 70% of universal rolling passes, with a rolling temperature of no more than 970℃, a rolling speed of no less than 3.5m / s, a cumulative flange reduction of no less than 50%, and a single-pass reduction rate of flange reduction and web reduction of no more than 10%; light-reduction rolling is used in the last 20% of universal rolling passes, with a cumulative flange reduction of no more than 20%. For products with a diameter of 40-60mm, the first 20% of universal rolling passes shall use low-speed, light-reduction rolling, with a cumulative flange reduction not exceeding 25% and a rolling speed not exceeding 3.0m / s; the first 20% to 70% of universal rolling passes shall use high-speed, high-reduction rolling, with a rolling temperature not exceeding 970℃, a rolling speed not less than 3.5m / s, a cumulative flange reduction not less than 50%, and a single-pass reduction rate for both flanges and web not exceeding 10%; the last 20% of universal rolling passes shall use light-reduction rolling, with a cumulative flange reduction not less than 15%. For products with a diameter of 60-80mm, low-speed, light-reduction rolling is used in the first 20% of universal rolling passes, with the cumulative reduction of the flanges not exceeding 20% and the rolling speed not exceeding 3.0m / s; high-speed, high-reduction rolling is used in the first 20% to 70% of universal rolling passes, with the rolling temperature not exceeding 970℃, the rolling speed not less than 3.5m / s, the cumulative reduction of the flanges not less than 40%, and the single-pass reduction rate of the flanges and web not exceeding 10%; light-reduction rolling is used in the last 20% of universal rolling passes, with the cumulative reduction of the flanges not less than 10%.
9. The method for producing 20-80mm thick wide-flange hot-rolled H-beams according to claim 8, characterized in that: In S6), the post-rolling controlled cooling process includes: the cooling time at the same rolling position does not exceed 15s, and the surface temperature of the rolled piece after cooling does not exceed 700℃.
Citation Information
Patent Citations
A wide-flange heavy hot-rolled H-beam, its production method and application
CN113604740B