Carbon-based hydrophobic thin films, methods of making and applications
By depositing carbon fumes generated from the incomplete combustion of carbon-containing organic combustibles onto the substrate surface, a micro-nano structured carbon-based hydrophobic film is formed. This solves the problems of low preparation efficiency and poor substrate compatibility in existing technologies, and realizes efficient and low-cost preparation and widespread application of hydrophobic films.
Patent Information
- Application Number
- CN202610380763.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-26
- Publication Date
- 2026-06-23
AI Technical Summary
Existing technologies for preparing hydrophobic thin films are inefficient, have poor compatibility with substrate materials, are complex to prepare, and are costly, making them difficult to apply on a large scale.
Carbon-containing organic combustibles such as cooking oil and candles are used to generate carbon smoke through incomplete combustion. Carbon-based hydrophobic films are deposited on the surface of substrate materials, and combined with micro-nano structures to form hydrophobic properties. This simplifies the preparation process and is applicable to a variety of substrate materials.
It achieves efficient and low-cost preparation of hydrophobic thin films, applicable to substrates such as metals, ceramics, glass, and plastics, with short deposition time, excellent hydrophobic properties, and wide substrate compatibility.
Smart Images

Figure CN122256948A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of material surface modification technology, specifically relating to carbon-based hydrophobic films. This invention also relates to the preparation method and application of carbon-based hydrophobic films. Background Technology
[0002] In recent years, researchers have developed various methods for preparing superhydrophobic surfaces, such as metal etching, sol-gel methods, chemical vapor deposition, electrodeposition, and phase inversion. However, these methods often require complex equipment, expensive reagents, or harsh reaction conditions, which limits their widespread application in practice.
[0003] Patent CN108102610B, published on June 1, 2018, entitled "A Superhydrophobic Thin Film and Its Preparation Method," discloses a method for preparing a superhydrophobic thin film. The method involves obtaining carbon nanoparticle deposits by burning vegetable oil, then mixing them with sodium stearate, followed by ultrasonication, drying, and heat treatment to ultimately obtain a thin film with good hydrophobic properties and acid and alkali resistance. This method utilizes natural raw materials and employs a green and environmentally friendly process, demonstrating the application potential of carbon-based materials in the field of superhydrophobicity.
[0004] However, the yield and morphology of the carbon nanoparticle deposits in this patent are greatly affected by the combustion conditions, and the preparation process still has certain controllability and repeatability issues. In addition, although the introduction of sodium stearate helps to reduce surface energy, its composite process with carbon nanoparticle deposits still requires multiple steps of ultrasonic and heat treatment, making the process relatively complex; moreover, this method is inefficient, and the preparation of a single superhydrophobic film takes a long time, ranging from 140 minutes to 37 hours. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing carbon-based hydrophobic films, which solves the problem of low efficiency in the preparation of hydrophobic films in the prior art.
[0006] A second objective of this invention is to provide a carbon-based hydrophobic film prepared by the above-described method for preparing carbon-based hydrophobic films.
[0007] A third objective of this invention is to provide applications of the aforementioned carbon-based hydrophobic films.
[0008] The first technical solution adopted in this invention is a method for preparing carbon-based hydrophobic thin films, specifically implemented according to the following steps:
[0009] Step 1: Pre-treat the substrate material; Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated substrate material; Step 4: Post-process the carbon-based hydrophobic film deposited on the surface of the substrate material.
[0010] The first technical solution of the present invention is further characterized by: Step 1 is as follows: Step 1.1: Select different cleaning methods according to the material of the substrate and clean the substrate material. Step 1.2: Place the cleaned substrate material in a ventilated area to air dry naturally or use forced ventilation to dry, removing the liquid phase medium from the surface of the substrate material.
[0011] The cleaning method for step 1.1 is as follows: If the substrate material is metal or plastic, rinse with clean water for 20-40 seconds, and then clean with an alcohol solution with a volume concentration of not less than 70%; if the substrate material is ceramic or glass, soak in a sodium linear alkylbenzene sulfonate aqueous solution with a volume concentration of 1% to 10% for 5-8 minutes, rinse with clean water for 20-40 seconds, and finally clean with an alcohol solution with a volume concentration of not less than 70%.
[0012] Step 2 is as follows: Step 2.1: Place the carbon-containing organic combustible material into the container; Step 2.2: Fix the pretreated base material on top of the carbon-containing organic combustible material, so that the vertical distance between the bottom surface of the base material and the carbon-containing organic combustible material is 2cm to 10cm.
[0013] The carbon-containing organic combustible material is any combination of one or more materials selected from edible oil, candles, wood chips, paraffin wax, diesel oil, kerosene, and turpentine; the container is a container that can withstand temperatures above 1000℃.
[0014] Step 3 specifically involves: Step 3.1: Ignite the carbon-containing organic combustibles in the container, and adjust the flame size to keep the carbon-containing organic combustibles in a state of incomplete combustion; Step 3.2: Allow the carbon-containing organic combustibles to undergo incomplete combustion to produce carbon-containing smoke that continuously deposits on the surface of the substrate material for 3 seconds to 15 minutes. Step 3.3: During the deposition process, adjust the position of the substrate material or container to ensure uniform deposition in all areas of the substrate material surface.
[0015] The incomplete combustion state in step 3.1 is as follows: carbon-containing organic combustibles produce obvious black smoke, but no violent flame eruption.
[0016] Step 4 is as follows: Step 4.1 After deposition, extinguish the carbon-containing organic combustibles and allow the substrate material to cool naturally to room temperature in its original position; Step 4.2: Wipe the surface of the substrate material with a dry, clean cotton cloth to remove dust and loosely bonded carbon particles that adhered during the deposition process.
[0017] The second technical solution adopted in this invention is a carbon-based hydrophobic film prepared by the above-mentioned method for preparing carbon-based hydrophobic films.
[0018] The third technical solution adopted in this invention is the application of carbon-based hydrophobic films in the field of waterproofing electronic products.
[0019] The beneficial effects of this invention are: 1. The raw materials are readily available and inexpensive. The carbon source is common carbon-containing organic combustibles such as candles, cooking oil, and diesel. No special precursors or targets are required, making them easy to obtain and suitable for large-scale popularization. 2. It has low material limitations and is applicable to a wide range of substrates. It can be prepared on the surface of a variety of common materials such as metals, ceramics, glass, and plastics. It has no strict requirements on the conductivity and shape of the substrate and can be used on both planar and curved substrates, thus solving the problem of poor substrate compatibility in existing technologies. 3. High preparation efficiency, with a deposition time of only 3s to 15min and a short complete process cycle. The shortest preparation time for a carbon-based hydrophobic film is only 25min, which can quickly obtain hydrophobic effect. Attached Figure Description
[0020] Figure 1 This is a bar chart showing the water droplet contact angle and sliding angle of carbon-based hydrophobic films with different deposition times using aluminum alloy as the substrate material. Figure 2 This is a scanning electron microscope top view of the carbon-based hydrophobic film of Example 1; Figure 3 This is a scanning electron microscope top view of the carbon-based hydrophobic film of Example 2; Figure 4 This is a scanning electron microscope top view of the carbon-based hydrophobic film of Example 3; Figure 5 This is a scanning electron microscope top view of the carbon-based hydrophobic film of Example 4; Figure 6 This is a scanning electron microscope top view of the carbon-based hydrophobic film of Example 5; Figure 7 This is a scanning electron microscope side view of the carbon-based hydrophobic film of Example 1; Figure 8 This is a scanning electron microscope side view of the carbon-based hydrophobic film of Example 2; Figure 9 This is a scanning electron microscope side view of the carbon-based hydrophobic film of Example 3; Figure 10 This is a scanning electron microscope side view of the carbon-based hydrophobic film of Example 4; Figure 11 This is a scanning electron microscope side view of the carbon-based hydrophobic film of Example 5. Detailed Implementation
[0021] The following detailed description is provided in conjunction with the accompanying drawings and specific embodiments.
[0022] This invention provides a method for preparing carbon-based hydrophobic films.
[0023] Step 1: Pre-treat the substrate material; Step 1.1: Select different cleaning methods according to the material of the substrate and clean the substrate material. If the substrate material is metal or plastic, rinse with water for 20-40 seconds, then clean with an alcohol solution with a volume concentration of not less than 70%. If the substrate material is ceramic or glass, soak in a 1%-10% sodium linear alkylbenzene sulfonate aqueous solution for 5-8 minutes, then rinse with water for 20-40 seconds, and finally clean with an alcohol solution with a volume concentration of not less than 70%.
[0024] Step 1.2: Place the cleaned substrate material in a ventilated area to air dry naturally or use forced ventilation to dry, removing the liquid phase medium from the surface of the substrate material.
[0025] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the carbon-containing organic combustible material into the container; Step 2.2: Fix the pretreated base material on top of the carbon-containing organic combustible material, so that the vertical distance between the bottom surface of the base material and the carbon-containing organic combustible material is 2cm to 10cm.
[0026] Among them, the carbon-containing organic combustibles are any combination of one or more materials selected from edible oil, candles, wood chips, paraffin wax, diesel oil, kerosene, and turpentine; the high-temperature resistant containers are containers that can withstand temperatures above 1000℃.
[0027] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated substrate material; Step 3.1: Ignite the carbon-containing organic combustibles in the container, and adjust the flame size to keep the carbon-containing organic combustibles in a state of incomplete combustion; The incomplete combustion state is characterized by the production of obvious black smoke from carbonaceous organic combustibles without violent flame eruption; Step 3.2: Allow the carbon-containing organic combustibles to undergo incomplete combustion to produce carbon-containing smoke that continuously deposits on the surface of the substrate material for 3 seconds to 15 minutes. Step 3.3: During the deposition process, adjust the position of the substrate material or container to ensure uniform deposition in all areas of the substrate material surface; Step 4: Post-process the carbon-based hydrophobic film deposited on the surface of the substrate material.
[0028] Step 4.1 After deposition, extinguish the carbon-containing organic combustibles and allow the substrate material to cool naturally to room temperature in its original position; Step 4.2: Wipe the surface of the substrate material with a dry, clean, soft cloth to remove dust and loosely bonded carbon particles that adhered during the deposition process.
[0029] This invention also provides a carbon-based hydrophobic film prepared by the above method; This invention also provides the application of carbon-based hydrophobic films in the field of waterproofing electronic products.
[0030] The core basis of the present invention's method for preparing carbon-based hydrophobic films via fumigation is as follows: Carbon-containing organic combustibles: Any one or more of the following can be mixed in any proportion: cooking oil, candles, wood chips, paraffin wax, diesel oil, kerosene, and turpentine. The common characteristics of this type of combustible are high carbon content, easy production of nano-sized carbon particles when incompletely burned, mild combustion process, no need for high temperature and high pressure environment, and readily available materials, thus lowering the threshold for use. Substrate type: Covers common materials such as metals, ceramics, glass, and plastics. This selection is based on meeting the application requirements in different scenarios and avoiding the limitations of substrate materials in existing technologies. Deposition distance: 2cm to 10cm. A distance of less than 2cm will cause the local temperature of the substrate to be too high, which may damage the substrate (such as deformation of plastic substrates). Also, carbon deposition is too fast and it is easy to form a thick film with a rough and uneven surface, which will affect the hydrophobic effect. A distance of more than 10cm will reduce the number of carbon particles reaching the substrate surface, resulting in low deposition efficiency and difficulty in forming a continuous hydrophobic film. Deposition time: 3s to 15min. A time of less than 3s will result in insufficient carbon deposition, discontinuous film, and failure to achieve hydrophobic function. A time of more than 15min will result in an excessively thick film, which is prone to cracking and peeling, and there is no additional improvement in hydrophobic performance, resulting in waste of resources.
[0031] The function, principle, and advantages of each step in the method of this invention are as follows: Step 1 removes impurities such as oil, dust, and moisture from the substrate surface to prevent these impurities from affecting the bonding force between the carbon particles and the substrate, ensuring a firm film adhesion. The principle is to remove physically adsorbed impurities through cleaning and to prevent uneven carbon particle deposition caused by moisture. The advantage is that the operation is simple, requiring only regular rinsing with water, wiping with alcohol, and natural drying or low-temperature drying.
[0032] Step 2 aims to create a stable deposition environment, ensuring that the carbon-containing smoke generated by the combustion of the carbon source can be deposited directionally on the substrate surface. The principle is to utilize thermal convection, where carbon particles generated by the incomplete combustion of combustibles move upward with the smoke and adhere to the substrate surface.
[0033] Step 3 is the core step, which involves depositing carbon particles from carbon-containing fumes onto the substrate surface to form a carbon-based thin film with a micro-nano rough structure. The principle is that when carbon-containing organic combustibles undergo incomplete combustion, carbon nanoparticles, graphite-like carbon, and other substances are produced, which accumulate on the substrate surface to form a thin film with a micro-nano-level uneven structure. The carbon material itself has low surface energy, and combined with the micro-nano rough structure, hydrophobic properties are achieved according to the Cassie-Baxter model. The advantage is that, unlike the vacuum evaporation and sputtering physical processes of PVD (Physical Vapor Deposition) technology, this step does not require a vacuum environment, high temperature and pressure, or high energy input. Carbon deposition can be completed simply through the natural combustion of combustibles. The process is extremely simple, and the deposition process is gentle and will not damage the substrate.
[0034] Step 4 removes floating dust and loosely attached carbon particles from the film surface, ensuring a clean and smooth surface and improving hydrophobic stability. The principle is to remove loosely attached impurities through physical wiping, avoiding affecting the integrity of the film surface structure. The advantage is that it is easy to operate, requires no chemical reagents or complex processing, and the natural cooling process can further enhance the adhesion between the film and the substrate.
[0035] This invention uses carbon-containing organic combustibles as a carbon source to prepare carbon-based hydrophobic films through fumigation deposition, breaking through the limitations of existing technologies that rely on special carbon sources (such as targets or special precursors), and realizing a preparation mode of "everyday materials + simple process". This invention constructs a simple deposition device that requires no vacuum environment or precision equipment, with a simple process flow, convenient operation, and significantly improved practicality; This invention broadens the scope of applicable substrate materials, enabling preparation on the surfaces of various common materials such as metals, ceramics, glass, and plastics, without being limited by the shape of the substrate. It solves the defects of existing technologies, such as large material limitations and poor substrate compatibility.
[0036] The core principle of this invention is "carbon particle deposition + micro / nano structure construction + low surface energy synergy", which is explained in detail below: The principle of carbon source combustion and carbon particle generation: When carbon-containing organic combustibles (such as cooking oil) undergo incomplete combustion, hydrocarbons undergo cracking reactions to generate nanoscale carbon particles (including amorphous carbon, carbon nanospheres, etc.), while a small amount of carbon monoxide, hydrogen and other gases are produced at the same time. The carbon particles move upward with the hot gas flow (smoke) to provide a carbon source for thin film deposition; this process does not require additional energy input, simplifying the carbon source conversion steps.
[0037] The principle of carbon-based thin film formation: Carbon particles adhere to the substrate surface through van der Waals forces, physical adsorption, and other processes. As the deposition time increases, the carbon particles gradually accumulate to form a continuous thin film. Due to the nanoscale size of the carbon particles themselves and their random distribution during the accumulation process, a micro-nano-scale rough structure is naturally formed on the surface of the thin film. This structure is one of the keys to achieving hydrophobic properties.
[0038] The principle behind hydrophobic properties: Carbon materials themselves have low surface energy (approximately 25 mJ / m²). 2 ~30mJ / m 2 Combined with the micro-nano rough structure of the film surface, according to the Cassie-Baxter wetting model, water droplets cannot spread on the film surface and only contact the surface protrusions, forming a "gas-liquid-solid" three-phase contact state, thus exhibiting excellent hydrophobic properties (contact angle ≥120°); while the untreated substrate surface is usually hydrophilic or weakly hydrophobic (contact angle ≤70°).
[0039] Example 1 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the aluminum alloy substrate material; First rinse with clean water for 20 seconds, then clean with a 75% alcohol solution. After cleaning, place the aluminum alloy plate in a ventilated area to air dry naturally for 10 minutes until it is completely dry.
[0040] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the candle in a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pre-treated aluminum alloy plate horizontally above the candle, so that the vertical distance between the bottom of the aluminum alloy plate and the top of the candle is 2cm.
[0041] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated aluminum alloy plate; Step 3.1: Ignite the candle in the high-temperature resistant container, adjust the flame size so that the candle produces obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continuously deposit on the lower surface of the aluminum alloy plate for 3 seconds; Step 3.3: During the deposition process, adjust the position of the candle to ensure uniform deposition in all areas of the bottom surface of the aluminum alloy plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the aluminum alloy plate.
[0042] Step 4.1: After deposition is complete, extinguish the candle and allow the aluminum alloy plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the aluminum alloy plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0043] Example 2 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the aluminum alloy substrate material; First rinse with clean water for 40 seconds, then clean with a 75% alcohol solution. Place the cleaned aluminum alloy sheet in a ventilated area to air dry naturally for 30 minutes.
[0044] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the candle in a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pre-treated aluminum alloy plate horizontally above the candle, so that the vertical distance between the bottom of the aluminum alloy plate and the top of the candle is 2cm.
[0045] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated aluminum alloy plate; Step 3.1: Ignite the candle in the high-temperature resistant container, adjust the flame size so that the candle produces obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continuously deposit on the lower surface of the aluminum alloy plate for 5 seconds; Step 3.3: During the deposition process, adjust the position of the candle to ensure uniform deposition in all areas of the bottom surface of the aluminum alloy plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the aluminum alloy plate.
[0046] Step 4.1: After deposition is complete, extinguish the candle and allow the aluminum alloy plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the aluminum alloy plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0047] Example 3 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the aluminum alloy substrate material; First rinse with clean water for 30 seconds, then clean with a 75% alcohol solution. Place the cleaned aluminum alloy sheet in a ventilated area to air dry naturally for 20 minutes.
[0048] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the candle in a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pre-treated aluminum alloy plate horizontally above the candle, so that the vertical distance between the bottom of the aluminum alloy plate and the top of the candle is 2cm.
[0049] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated aluminum alloy plate; Step 3.1: Ignite the candle in the high-temperature resistant container, adjust the flame size so that the candle produces obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continuously deposit on the lower surface of the aluminum alloy plate for 10 seconds; Step 3.3: During the deposition process, adjust the position of the candle to ensure uniform deposition in all areas of the bottom surface of the aluminum alloy plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the aluminum alloy plate.
[0050] Step 4.1: After deposition is complete, extinguish the candle and allow the aluminum alloy plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the aluminum alloy plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0051] Example 4 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the aluminum alloy substrate material; First rinse with clean water for 25 seconds, then clean with a 95% alcohol solution. After cleaning, use a hairdryer to dry the aluminum alloy sheet using natural airflow.
[0052] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the candle in a graphite container that can withstand temperatures up to 1000°C; Step 2.2: Fix the pre-treated aluminum alloy plate horizontally above the candle, so that the vertical distance between the bottom of the aluminum alloy plate and the top of the candle is 2cm.
[0053] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated aluminum alloy plate; Step 3.1: Ignite the candle in the high-temperature resistant container, adjust the flame size so that the candle produces obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continuously deposit on the lower surface of the aluminum alloy plate for 20 seconds; Step 3.3: During the deposition process, adjust the position of the candle to ensure uniform deposition in all areas of the bottom surface of the aluminum alloy plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the aluminum alloy plate.
[0054] Step 4.1: After deposition is complete, extinguish the candle and allow the aluminum alloy plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the aluminum alloy plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0055] Example 5 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the aluminum alloy substrate material; First rinse with clean water for 35 seconds, then clean with a 75% alcohol solution. Place the cleaned aluminum alloy sheet in a ventilated area to air dry for 15 minutes.
[0056] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the candle in a graphite container that can withstand temperatures up to 1000°C; Step 2.2: Fix the pre-treated aluminum alloy plate horizontally above the candle, so that the vertical distance between the bottom of the aluminum alloy plate and the top of the candle is 2cm.
[0057] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated aluminum alloy plate; Step 3.1: Ignite the candle in the high-temperature resistant container, adjust the flame size so that the candle produces obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continuously deposit on the lower surface of the aluminum alloy plate for 40 seconds; Step 3.3: During the deposition process, adjust the position of the candle to ensure uniform deposition in all areas of the bottom surface of the aluminum alloy plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the aluminum alloy plate.
[0058] Step 4.1: After deposition is complete, extinguish the candle and allow the aluminum alloy plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the aluminum alloy plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0059] Example 6 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the glass substrate material; First, soak in a 1% (v / v) sodium linear alkylbenzene sulfonate aqueous solution for 5 minutes, then rinse with clean water for 30 seconds, and finally clean with a 70% (v / v) alcohol solution. Place the cleaned glass plate in a ventilated area to air dry for 25 minutes.
[0060] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the paraffin wax into a graphite container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pretreated glass plate horizontally above the paraffin wax, so that the vertical distance between the bottom of the glass plate and the top of the paraffin wax is 2cm.
[0061] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated glass plate; Step 3.1: Ignite the paraffin wax in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the candle to continue to accumulate on the lower surface of the glass plate for 3 minutes; Step 3.3: During the deposition process, adjust the position of the glass plate to ensure uniform deposition in all areas of the bottom surface of the glass plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the glass plate.
[0062] Step 4.1: After deposition is complete, extinguish the paraffin wax and allow the glass plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom of the glass plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0063] Example 7 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the plastic board substrate material; First, rinse the plastic surface with clean water for 30 seconds, then clean it with a 70% alcohol solution. Place the cleaned plastic sheet in a ventilated area to air dry for 23 minutes.
[0064] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the diesel fuel into a graphite container that can withstand temperatures up to 1000°C; Step 2.2: Fix the pre-treated plastic plate horizontally above the diesel fuel, so that the vertical distance between the bottom of the plastic plate and the top of the candle is 3cm.
[0065] Step 3: Deposit a carbon-based hydrophobic film onto the surface of the pretreated plastic sheet; Step 3.1: Ignite the diesel fuel in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain incomplete combustion. Step 3.2: Allow the black smoke produced by the incomplete combustion of diesel fuel to continuously deposit on the lower surface of the plastic plate for 5 seconds; Step 3.3: During the deposition process, adjust the position of the plastic plate to ensure uniform deposition in all areas of the bottom surface of the plastic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the plastic plate.
[0066] Step 4.1: After the deposition is complete, extinguish the diesel fuel and allow the plastic plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom of the plastic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0067] Example 8 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 10% (v / v) detergent solution for 8 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 18 minutes.
[0068] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the cooking oil into a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pre-treated ceramic plate horizontally above the cooking oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the cooking oil is 10cm.
[0069] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the cooking oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of cooking oil to continuously deposit on the lower surface of the ceramic plate for 15 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0070] Step 4.1: After the deposition is complete, turn off the cooking oil and allow the ceramic plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0071] Example 9 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0072] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the kerosene into a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pretreated ceramic plate horizontally above the kerosene, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the kerosene is 6cm.
[0073] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the kerosene in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of kerosene to continuously deposit on the lower surface of the ceramic plate for 8 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0074] Step 4.1: After deposition is complete, extinguish the kerosene and allow the ceramic plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0075] Example 10 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 6% (v / v) detergent solution for 6 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 30 minutes.
[0076] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the pine wood chips into a ceramic container that can withstand temperatures up to 1000℃; Step 2.2: Fix the pretreated ceramic plate horizontally above the wood chips, so that the vertical distance between the bottom surface of the ceramic plate and the surface of the wood chips is 7cm.
[0077] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the wood chips inside the high-temperature resistant container, adjust the flame size to produce obvious black smoke from the wood chips, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke from the incomplete combustion of wood chips to continuously deposit on the lower surface of the ceramic plate for 10 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0078] Step 4.1: After deposition is complete, extinguish the wood chips and allow the ceramic plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0079] Example 11 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0080] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place the turpentine oil into a ceramic container that can withstand temperatures up to 1000°C; Step 2.2: Fix the pretreated ceramic plate horizontally above the turpentine, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the turpentine is 6cm.
[0081] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the turpentine in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain the incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of turpentine to continuously deposit on the lower surface of the ceramic plate for 5 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0082] Step 4.1: After deposition is complete, extinguish the turpentine and allow the ceramic plate to cool naturally to room temperature in its original position. Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0083] Example 12 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 6 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0084] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Put kerosene and diesel oil into a ceramic container that can withstand 1000℃ in a 1:1 ratio; Step 2.2: Fix the pretreated ceramic plate horizontally above the mixed oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the mixed oil is 6cm.
[0085] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the mixed oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the mixed oil to continuously deposit on the lower surface of the ceramic plate for 9 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0086] Step 4.1: After deposition is complete, extinguish the mixed oil and allow the ceramic plate to cool naturally to room temperature in its original position; Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0087] Example 13 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0088] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place kerosene, diesel oil, and cooking oil in a 1:2:1 ratio into a ceramic container that can withstand 1000℃. Step 2.2: Fix the pretreated ceramic plate horizontally above the mixed oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the mixed oil is 6cm.
[0089] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the mixed oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the mixed oil to continuously deposit on the lower surface of the ceramic plate for 8 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0090] Step 4.1: After deposition is complete, extinguish the mixed oil and allow the ceramic plate to cool naturally to room temperature in its original position; Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0091] Example 14 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0092] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place turpentine, kerosene, diesel, and cooking oil in a ceramic container that can withstand 1000℃ in a ratio of 1:2:1:2; Step 2.2: Fix the pretreated ceramic plate horizontally above the mixed oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the mixed oil is 6cm.
[0093] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the mixed oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the mixed oil to continuously deposit on the lower surface of the ceramic plate for 9 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0094] Step 4.1: After deposition is complete, extinguish the mixed oil and allow the ceramic plate to cool naturally to room temperature in its original position; Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0095] Example 15 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0096] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place wood chips, paraffin wax, kerosene, diesel oil, and cooking oil in a weight ratio of 1:2:1:2:1 into a ceramic container that can withstand 1000℃. Step 2.2: Fix the pretreated ceramic plate horizontally above the mixed oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the mixed oil is 4cm.
[0097] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the mixed oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the mixed oil to continuously deposit on the lower surface of the ceramic plate for 6 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0098] Step 4.1: After deposition is complete, extinguish the mixed oil and allow the ceramic plate to cool naturally to room temperature in its original position; Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0099] Example 16 The method for preparing the carbon-based hydrophobic thin film provided in this embodiment specifically includes the following steps: Step 1: Pre-treat the ceramic substrate material; First, soak in a 5% (v / v) detergent solution for 7 minutes, then rinse with clean water for 30 seconds, and finally clean with a 75% (v / v) alcohol solution. Place the cleaned ceramic slab in a ventilated area to air dry for 26 minutes.
[0100] Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 2.1: Place wood chips, paraffin wax, kerosene, diesel oil, cooking oil, and turpentine in a weight ratio of 1:1:1:2:1:2:1 into a ceramic container that can withstand 1000℃. Step 2.2: Fix the pretreated ceramic plate horizontally above the mixed oil, so that the vertical distance between the bottom surface of the ceramic plate and the horizontal surface of the mixed oil is 4.5cm.
[0101] Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated ceramic plate; Step 3.1: Ignite the mixed oil in the high-temperature resistant container, adjust the flame size to produce obvious black smoke, and maintain an incomplete combustion state; Step 3.2: Allow the black smoke produced by the incomplete combustion of the mixed oil to continuously deposit on the lower surface of the ceramic plate for 6 minutes; Step 3.3: During the deposition process, adjust the position of the ceramic plate to ensure uniform deposition in all areas of the bottom surface of the ceramic plate; Step 4: Post-process the carbon-based hydrophobic film deposited on the bottom surface of the ceramic plate.
[0102] Step 4.1: After deposition is complete, extinguish the mixed oil and allow the ceramic plate to cool naturally to room temperature in its original position; Step 4.2: Wipe the bottom surface of the ceramic plate with a dry, clean cotton cloth to remove the floating dust and loosely bonded carbon particles that adhered during the deposition process.
[0103] The carbon-based hydrophobic films prepared in Examples 1-16 were tested. The hydrophobic properties of the films were measured using a contact angle meter, and the data are shown in Table 1. Table 1 - Hydrophobic properties of carbon-based hydrophobic films in Examples 1-16
[0104] As can be seen from Table 1, the contact angle between the carbon-based hydrophobic film prepared by this method and water droplets is 147°~164°, and the contact angle is greater than 120°, which shows excellent hydrophobic properties.
[0105] Wetting analysis was performed on the carbon-based hydrophobic films prepared in Examples 1-5, and the results are shown below. Figure 1 As shown, all carbon-based hydrophobic film surfaces exhibited high water repellency, with high contact angles ranging from 147° to 160° and low slip angles ranging from 21° to 6°. However, superhydrophobic properties only occurred on surfaces with contact angles exceeding 150° and slip angles less than 10°, i.e., deposition times of 3 seconds and 5 seconds. The smooth aluminum surface coated with candle soot exhibited a relatively high contact angle of 160° within 5 seconds, while the slip angle was only 5°. Compared to the 3-second deposition sample, the nano-network coating showed higher adhesion stability. It can be concluded that with increasing deposition time, the contact angle decreases while the slip angle increases.
[0106] The carbon-based hydrophobic films prepared in Examples 1-5 were observed using scanning electron microscopy (SEM). The top view of the SEM images is shown below. Figures 2-6 It can be seen that with increasing deposition time, the coating porosity slightly decreases, the network becomes more compact, and the nanoparticle size slightly increases. The nanoparticle size ranges from 40 nm to 70 nm between deposition times of 3 to 40 seconds. Figure 1 It can be concluded that the increase in nanoparticle size and their aggregation leads to a decrease in surface porosity, which in turn leads to a decrease in contact angle and an increase in slip angle.
[0107] The carbon-based hydrophobic films prepared in Examples 1-5 were observed using scanning electron microscopy (SEM). Side views of the SEM images are shown below. Figures 7-11 The thicknesses of the deposited nanoparticle networks (see D1 in the figure) were 8 μm, 12 μm, 18 μm, 37 μm, and 67 μm, respectively, with deposition times of 3, 5, 10, 20, and 40 seconds. Analysis showed that for every additional second of deposition time, the growth of the porous candle soot nanonetwork increased linearly by approximately 2 to 3 μm.
Claims
1. A method for preparing a carbon-based hydrophobic thin film, characterized in that, The specific steps are as follows: Step 1: Pre-treat the substrate material; Step 2: Construct a device platform for preparing carbon-based hydrophobic thin films; Step 3: Deposit a carbon-based hydrophobic film on the surface of the pretreated substrate material; Step 4: Post-process the carbon-based hydrophobic film deposited on the surface of the substrate material.
2. The method for preparing a carbon-based hydrophobic thin film according to claim 1, characterized in that, Step 1 specifically involves: Step 1.1: Select different cleaning methods according to the material of the substrate and clean the substrate material. Step 1.2: Force-dry the cleaned substrate material by blowing air to dry the surface of the substrate material.
3. The method for preparing a carbon-based hydrophobic thin film according to claim 2, characterized in that, The cleaning method described in step 1.1 is as follows: If the substrate material is metal or plastic, rinse with clean water for 20-40 seconds, and then clean with an alcohol solution with a volume concentration of not less than 70%; if the substrate material is ceramic or glass, soak in a sodium linear alkylbenzene sulfonate aqueous solution with a volume concentration of 1% to 10% for 5-8 minutes, rinse with clean water for 20-40 seconds, and finally clean with an alcohol solution with a volume concentration of not less than 70%.
4. The method for preparing a carbon-based hydrophobic thin film according to claim 1, characterized in that, Step 2 specifically involves: Step 2.1: Place the carbon-containing organic combustible material into the container; Step 2.2: Fix the pretreated base material on top of the carbon-containing organic combustible material, so that the vertical distance between the bottom surface of the base material and the carbon-containing organic combustible material is 2cm to 10cm.
5. The method for preparing a carbon-based hydrophobic thin film according to claim 4, characterized in that, The carbon-containing organic combustible material is any combination of one or more materials selected from edible oil, candles, wood chips, paraffin wax, diesel oil, kerosene, and turpentine; the container is a container that can withstand temperatures above 1000℃.
6. The method for preparing a carbon-based hydrophobic thin film according to claim 1, characterized in that, Step 3 specifically involves: Step 3.1: Ignite the carbon-containing organic combustibles in the container, and adjust the flame size to keep the carbon-containing organic combustibles in a state of incomplete combustion; Step 3.2: Allow the carbon-containing organic combustibles to undergo incomplete combustion to produce carbon-containing smoke that continuously deposits on the surface of the substrate material for 3 seconds to 15 minutes. Step 3.3: During the deposition process, adjust the position of the substrate material or container to ensure uniform deposition in all areas of the substrate material surface.
7. The method for preparing a carbon-based hydrophobic thin film according to claim 6, characterized in that, The incomplete combustion state described in step 3.1 is as follows: carbon-containing organic combustibles produce obvious black smoke, but there is no violent flame eruption.
8. The method for preparing a carbon-based hydrophobic thin film according to claim 1, characterized in that, Step 4 specifically involves: Step 4.1 After deposition, extinguish the carbon-containing organic combustibles and allow the substrate material to cool naturally to room temperature in its original position; Step 4.2: Wipe the surface of the substrate material with a dry, clean cotton cloth to remove dust and loosely bonded carbon particles that adhered during the deposition process.
9. A carbon-based hydrophobic thin film, characterized in that, The carbon-based hydrophobic film was prepared using the method described in any one of claims 1-8.
10. The application of the carbon-based hydrophobic film according to claim 9 in the field of waterproofing electronic products.
Citation Information
Patent Citations
A superhydrophobic thin film and its preparation method
CN108102610B