A production method of high-conductivity and high-heat-dissipation copper slot wire
By adding trace alloying elements such as Ag, Cr, Sr, Sc, Ge, and Zr to copper channel wires, and combining processes such as ultrasonic dispersion-mechanical ball milling, directional microwave strong field and electrical pulse treatment, the problems of decreased conductivity and heat dissipation performance and insufficient mechanical strength of copper channel wires under high current conditions have been solved. This has enabled the production of copper channel wires with high conductivity and high heat dissipation, which are suitable for use in high-end equipment.
Patent Information
- Application Number
- CN202610646798.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-12
- Publication Date
- 2026-07-03
AI Technical Summary
Existing copper cable trays suffer from excessive temperature rise due to Joule heat buildup under high current operating conditions, resulting in decreased conductivity and heat dissipation, insufficient mechanical strength, and problems such as long production cycles, high energy consumption, and poor performance consistency in the manufacturing process.
Using high-purity electrolytic copper as the base material, and adding trace alloying elements such as Ag, Cr, Sr, Sc, Ge, and Zr, a high-conductivity and high-heat-dissipation copper channel wire is formed through a process of ultrasonic dispersion-mechanical ball milling, vacuum hot pressing, directional microwave strong field and electric pulse treatment, hot extrusion forming, cold rolling finishing and gradient heat treatment.
It achieves synergistic optimization of the conductivity, heat dissipation and fatigue resistance of copper channel wire, improves the uniformity and stability of material structure, is suitable for the use requirements of high-end equipment, and has a simple process that can be mass-produced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper channel wire technology, and in particular to a method for producing high-conductivity, high-heat-dissipation copper channel wire. Background Technology
[0002] As power electronic equipment develops towards higher power and higher integration, the conductivity and heat dissipation performance of copper trunking, as a high-current-carrying conductor, have become key factors restricting the reliability of equipment operation. Under long-term high-current operation, existing busbar trunking and copper trunking products experience excessive temperature rise due to Joule heat accumulation, leading not only to increased energy loss but also to safety hazards such as insulation aging and increased contact resistance. Therefore, developing copper trunking with both high conductivity and high heat dissipation efficiency has become an urgent industry need.
[0003] Current copper channel wire production primarily uses pure copper or conventional copper alloys as raw materials, processed through conventional processes such as smelting, rolling, drawing, and forming. While pure copper possesses good electrical and thermal conductivity, it suffers from low mechanical strength, insufficient fatigue resistance, and is prone to grain growth under high-temperature conditions, leading to a decline in electrical and heat dissipation performance, making it difficult to meet the long-term operating requirements of high-end equipment. Conventional copper alloys improve mechanical strength by adding alloying elements, but the introduction of these elements disrupts the lattice integrity of the copper matrix, increasing electron scattering and resulting in a significant decrease in electrical and thermal conductivity. This creates a contradiction between "increased strength and decreased electrical and heat dissipation performance," failing to achieve synergistic optimization of electrical conductivity, heat dissipation, and mechanical properties. Furthermore, existing copper channel wire production processes also suffer from various technical shortcomings, including long production cycles, high energy consumption, inadequate ingot purification, and poor product performance consistency.
[0004] Therefore, developing a copper channel wire production method with good conductivity, good heat dissipation, sufficient fatigue resistance, stable process, and scalable production has become an urgent technical problem to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a production method for high-conductivity and high-heat-dissipation copper channel wires. Through precise alloy composition design, efficient ingot purification treatment, suitable forming process and gradient heat treatment process, the conductivity, heat dissipation and fatigue life of copper channel wires are synergistically optimized, while improving the consistency and stability of the products, meeting the needs of high-end equipment, and the process is simple, can be mass-produced, and conforms to the development trend of the industry.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is: a method for producing high-conductivity, high-heat-dissipation copper trench wire, comprising the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 850~950℃, hot pressing pressure 20~30MPa, heat preservation for 2~3h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0007] Preferably, the purity of the high-purity electrolytic copper in step S1 is ≥99.9995%.
[0008] Preferably, the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 40~60kHz, power 150~200W, dispersion time 20~30min; mechanical ball milling ball-to-material ratio (10~15):1, rotation speed 300~400r / min, ball milling time 1~2h; the temperature of the mixed powder is controlled to ≤150℃ during the dispersion process.
[0009] Preferably, the copper-alloy element solid composite powder in step S1 comprises the following components by weight percentage: Ag 0.13-0.25%, Cr 0.05-0.1%, Sr 0.01-0.03%, Sc 0.08-0.12%, Ge 0.03-0.05%, Zr 0.1-0.15%, with the balance being electrolytic copper and other unavoidable impurities.
[0010] Preferably, the high-purity argon gas has a purity of ≥99.999% and a flow rate of 0.3~0.5L / min.
[0011] Preferably, the parameters for the directional focusing microwave strong field processing in step S3 are: microwave frequency 2.45~5.8GHz, microwave power 500~800W, focusing spot diameter 5~10mm, processing time 8~15min, and the ingot temperature is controlled not to exceed 300℃ during the processing.
[0012] Preferably, the parameters for the electrical pulse treatment in step S4 are: pulse voltage 800~1200V, pulse frequency 50~100Hz, pulse width 50~100μs, and treatment time 10~20min, with the ingot temperature maintained at 200~300℃ during the treatment.
[0013] Preferably, the hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 690~730℃, an extrusion speed of 8~12mm / s, an extrusion ratio of (8~12):1, and the extrusion die cavity is an arc-shaped transition groove. The cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling.
[0014] Preferably, the ingot preheating temperature in step S5 is 700~750℃ and the holding time is 30~40min; the extrusion die is preheated in stages, first held at 200~250℃ for 8-12min, and then held at 350~400℃ for 13-16min.
[0015] Preferably, the nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 12~18μm; the cooling rate is controlled at 15~20℃ / min.
[0016] Preferably, the total rolling rate of the cold rolling finishing in step S6 is 40-50%, the rolling rate of each pass is controlled at 8-12%, and the interval between adjacent passes is 5-10 minutes; after each pass of rolling, gentle grinding and cleaning are performed, and finally, precision straightening is performed.
[0017] Preferably, the cold rolling temperature of the cold rolling finishing in step S6 is 20~25℃, and it is completed in 4~5 passes with an interval of 5~10 minutes between adjacent passes.
[0018] Preferably, the gradient aging heat treatment in step S7 specifically involves: sequentially holding at 420~440℃ for 3.5~4.5h, holding at 320~350℃ for 1~1.5h, holding at 220~250℃ for 2~3h, and finally cooling to room temperature at a rate of 2~3℃ / min.
[0019] Preferably, the gradient alloy layer in step S8 is deposited by ion beam sputtering, with a thickness of 50-60 nm, and is a silver-copper-La gradient alloy layer. The gradient distribution is as follows: the outermost layer alloy composition is 85 wt% Ag, 0.5 wt% La, and 14.5 wt% Cu by weight percentage; the innermost layer alloy composition is 5 wt% Ag, 0.1 wt% La, and 94.9 wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85 wt% to 5 wt%, the La content decreases uniformly from 0.5 wt% to 0.1 wt%, and the copper content increases uniformly from 14.5 wt% to 94.9 wt%.
[0020] Another object of the present invention is to provide a high-conductivity, high-heat-dissipation copper channel wire produced by the aforementioned high-conductivity, high-heat-dissipation copper channel wire production method.
[0021] Due to the application of the above technical solution, the present invention has the following beneficial effects: (1) The method for producing high conductivity and high heat dissipation copper channel wire disclosed in this invention, wherein the copper-alloy element solid composite powder comprises the following components by weight percentage: Ag 0.13-0.25%, Cr 0.05-0.1%, Sr 0.01-0.03%, Sc 0.08-0.12%, Ge 0.03-0.05%, Zr 0.1-0.15%, with the balance being electrolytic copper and other unavoidable impurities. A precise blend of six elements (Ag-Cr-Sr-Sc-Ge-Zr) was employed, with each element working synergistically and complementing each other to overcome the performance limitations of existing conventional copper alloys doped with single or binary elements. Ag enhances conductivity and interfacial wettability; Cr refines grains and improves high-temperature creep resistance; Sr purifies the grain boundaries of the copper matrix and inhibits impurity segregation; Sc significantly refines as-cast grains and weakens grain boundary resistance; Ge regulates lattice defects and reduces electron scattering loss; and Zr forms a nano-dispersed phase that locks grain boundaries and improves thermal stability. Within a defined ratio range, the six elements produce a non-additive synergistic effect, simultaneously achieving ultra-fine grains, improved grain boundary purity, enhanced high-temperature structural stability, significantly optimized creep and aging resistance, and markedly improved fatigue resistance without significantly sacrificing the high conductivity of the copper matrix. This comprehensive performance improvement is unpredictable and cannot be derived from conventional ratios.
[0022] (2) The production method of high conductivity and high heat dissipation copper trench wire disclosed in this invention forms a synergistic coupling effect of directional microwave strong field and electric pulse treatment. Unlike the conventional methods of single heat treatment or single field treatment, the directional microwave strong field relies on directional dielectric to accurately activate the grain boundary and phase interface of copper alloy, gently eliminate the micro-segregation of elements and weaken the interface scattering loss. The electric pulse uses pulse energy to disturb the lattice configuration, drive the uniform precipitation of alloy elements and further bridge the micro lattice defects. The coupling of the two fields is not a simple superposition of effects, but a synergistic gain effect. It can achieve grain refinement and uniform dispersion of alloy elements in the low temperature range, and can also greatly optimize the charge transport path, reduce the interface contact resistance and lattice electron scattering. At the same time, it can stabilize the matrix structure, suppress grain coarsening and element re-segregation during subsequent processing and service. While ensuring that the high conductivity of the copper matrix does not decay, it can simultaneously and significantly improve the material structure uniformity, mechanical stability, heat resistance and aging resistance and fatigue resistance.
[0023] (4) The production method of high conductivity and high heat dissipation copper trench wire disclosed in this invention adopts an ultrasonic dispersion-mechanical ball milling synergistic process, which is different from the conventional dispersion methods of single ultrasonic dispersion or single mechanical ball milling. The two form a synergistic and complementary effect, which is not a simple superposition: ultrasonic dispersion accurately disperses the micro agglomerates of trace alloying elements by means of high frequency oscillation, while avoiding the damage of alloying element particles caused by the single action of mechanical ball milling. Mechanical ball milling relies on shearing and impact to uniformly embed the dispersed alloying element particles into the copper powder matrix, and simultaneously refines the copper powder particle size and optimizes the powder mixing uniformity. The synergistic process solves the problems of insufficient dispersion depth and poor heat dissipation of single ultrasonic dispersion. This method overcomes the challenges of secondary agglomeration of gold elements and the drawbacks of uneven dispersion, powder oxidation, and lattice defects caused by single mechanical ball milling. Without surface modification or the introduction of any conductive interference substances, it achieves efficient, uniform, and stable dispersion of trace alloying elements in copper powder. This significantly improves the density of subsequent vacuum hot pressing and the interfacial bonding force between the alloying elements and the copper matrix, laying a solid foundation for the high conductivity, high heat dissipation, and excellent fatigue resistance of copper channel wires. It achieves dispersion effects and performance improvements that cannot be predicted by existing single dispersion processes or derived through conventional process combinations. Moreover, the process is simple, cost-controllable, and more suitable for industrial mass production needs.
[0024] (5) The production method of high conductivity and high heat dissipation copper channel wire disclosed in this invention adopts ultrasonic dispersion-mechanical ball milling synergistic process in the raw material pretreatment stage to achieve uniform and stable dispersion of trace alloying elements in copper powder without surface modification, laying the foundation for subsequent processes; vacuum hot pressing further densifies the matrix and consolidates the element dispersion effect; directional microwave strong field and electric pulse treatment are coupled sequentially to accurately optimize interface bonding, refine grains and reduce charge transmission loss; hot extrusion and cold rolling finishing fix the dispersion structure and ensure dimensional accuracy; gradient heat treatment and gradient alloy layer deposition synergistically improve the comprehensive performance and surface protection capability of the material. Each step is not simply superimposed, but cooperates with each other and progresses layer by layer. Under the core premise of ensuring high conductivity of copper channel wire, the uniformity of alloying element dispersion, matrix densification, mechanical stability, heat resistance, aging resistance and oxidation resistance are simultaneously improved, and fatigue resistance is significantly improved. This solves the technical pain points of uneven dispersion, poor interface bonding and difficulty in achieving performance balance in the prior art. Moreover, the process is mature and controllable and suitable for industrial mass production. Detailed Implementation
[0025] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.
[0026] Example 1 A method for producing a high-conductivity, high-heat-dissipation copper trench wire includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 850℃, hot pressing pressure 20MPa, heat preservation for 2h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0027] The purity of the high-purity electrolytic copper in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 40kHz, power 150W, dispersion time 20min; mechanical ball milling ball-to-material ratio 10:1, rotation speed 300r / min, ball milling time 1h; the temperature of the mixed powder is controlled ≤150℃ during dispersion; the copper-alloy element solid composite powder in step S1 includes the following components by weight percentage: Ag 0.13%, Cr 0.05%, Sr 0.01%, Sc 0.08%, Ge 0.03%, Zr 0.1%, with the balance being electrolytic copper and other unavoidable impurities; the purity of the high-purity argon gas is ≥99.999%, and the flow rate is 0.3L / min.
[0028] The parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 2.45 GHz, microwave power 500 W, focused spot diameter 5 mm, and treatment time 8 min. During the treatment, the ingot temperature is controlled to not exceed 300 °C. The parameters for the electrical pulse treatment in step S4 are: pulse voltage 800 V, pulse frequency 50 Hz, pulse width 50 μs, and treatment time 10 min. During the treatment, the ingot temperature is controlled to be maintained at 200 °C. The hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 690 °C, an extrusion speed of 8 mm / s, and an extrusion ratio of 8:1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling. The ingot preheating temperature in step S5 is 700 °C, and the holding time is 30 min. The extrusion die is preheated in stages, first held at 200 °C for 8 min, and then held at 350 °C for 13 min.
[0029] The nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 12μm; the cooling rate is controlled at 15℃ / min; the total rolling rate of the cold rolling finishing in step S6 is 40%, the rolling rate of each pass is controlled at 8%, and the interval between adjacent passes is 5min; after each pass of rolling, gentle grinding and cleaning are performed, and finally, precision straightening is performed; the cold rolling temperature of the cold rolling finishing in step S6 is 20℃, and it is completed in 4 passes with an interval of 5min between adjacent passes.
[0030] The gradient aging heat treatment in step S7 specifically involves sequentially holding at 420℃ for 3.5 hours, 320℃ for 1 hour, and 220℃ for 2 hours, and finally cooling to room temperature at a rate of 2℃ / min. The gradient alloy layer in step S8 is deposited by ion beam sputtering with a thickness of 50 nm. It is a silver-copper-La gradient alloy layer with the following gradient distribution: the outermost layer alloy composition is 85wt% Ag, 0.5wt% La, and 14.5wt% Cu by weight percentage; the innermost layer alloy composition is 5wt% Ag, 0.1wt% La, and 94.9wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85wt% to 5wt%, the La content decreases uniformly from 0.5wt% to 0.1wt%, and the copper content increases uniformly from 14.5wt% to 94.9wt%.
[0031] Example 2 A method for producing a high-conductivity, high-heat-dissipation copper trench wire includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 870℃, hot pressing pressure 23MPa, heat preservation for 2.3h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0032] The purity of the high-purity electrolytic copper mentioned in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 45kHz, power 160W, dispersion time 23min; mechanical ball milling ball-to-material ratio 12:1, rotation speed 330r / min, ball milling time 1.2h; the temperature of the mixed powder is controlled ≤150℃ during dispersion; the copper-alloy element solid composite powder mentioned in step S1 includes the following components by weight percentage: Ag 0.16%, Cr 0.06%, Sr 0.015%, Sc 0.09%, Ge 0.035%, Zr 0.12%, with the balance being electrolytic copper and other unavoidable impurities; the purity of the high-purity argon gas is ≥99.999%, and the flow rate is 0.35L / min; the parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 3GHz, microwave power 600W, focusing spot diameter 6mm, and treatment time 10min, with the ingot temperature controlled not to exceed 300℃ during the treatment process.
[0033] The parameters for the electrical pulse treatment in step S4 are: pulse voltage 900V, pulse frequency 60Hz, pulse width 60μs, and treatment time 13min. During the treatment, the ingot temperature is maintained at 230℃. The hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 700℃, an extrusion speed of 9mm / s, and an extrusion ratio of 9:1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling. The ingot preheating temperature in step S5 is 710℃, and the holding time is 33min. The extrusion die is preheated in stages, first held at 220℃ for 9min, and then held at 360℃ for 14min. The nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 14μm. The cooling rate is controlled at 16℃ / min.
[0034] The total rolling rate of the cold rolling finishing in step S6 is 43%, with the rolling rate of each pass controlled at 9%, and an interval of 6 minutes between adjacent passes; after each pass of rolling, gentle grinding and cleaning are performed, and finally precision straightening is performed; the cold rolling temperature of the cold rolling finishing in step S6 is 21℃, and it is completed in 4 passes with an interval of 6 minutes between adjacent passes; the gradient aging heat treatment in step S7 is specifically as follows: sequentially holding at 425℃ for 3.8h, holding at 330℃ for 1.2h, and holding at 230℃ for 2.3h, and finally cooling to room temperature at a rate of 2.3℃ / min.
[0035] The gradient alloy layer described in step S8 is deposited by ion beam sputtering, with a thickness of 53 nm. It is a silver-copper-La gradient alloy layer, and the gradient distribution is as follows: the outermost layer alloy composition is 85 wt% Ag, 0.5 wt% La, and 14.5 wt% Cu by weight percentage; the innermost layer alloy composition is 5 wt% Ag, 0.1 wt% La, and 94.9 wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85 wt% to 5 wt%, the La content decreases uniformly from 0.5 wt% to 0.1 wt%, and the copper content increases uniformly from 14.5 wt% to 94.9 wt%.
[0036] Example 3 A method for producing a high-conductivity, high-heat-dissipation copper trench wire includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 900℃, hot pressing pressure 25MPa, heat preservation for 2.5h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0037] The purity of the high-purity electrolytic copper in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 50kHz, power 180W, dispersion time 25min; mechanical ball milling ball-to-material ratio 13:1, rotation speed 350r / min, ball milling time 1.5h; the temperature of the mixed powder is controlled ≤150℃ during dispersion; the copper-alloy element solid composite powder in step S1 includes the following components by weight percentage: Ag 0.2%, Cr 0.08%, Sr 0.02%, Sc 0.1%, Ge 0.04%, Zr 0.13%, with the balance being electrolytic copper and other unavoidable impurities; the purity of the high-purity argon gas is ≥99.999%, and the flow rate is 0.4L / min.
[0038] The parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 4GHz, microwave power 650W, focused spot diameter 7mm, and treatment time 11min. During the treatment, the ingot temperature is controlled to not exceed 300℃. The parameters for the electrical pulse treatment in step S4 are: pulse voltage 1000V, pulse frequency 80Hz, pulse width 80μs, and treatment time 15min. During the treatment, the ingot temperature is controlled to be maintained at 250℃.
[0039] The hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 710℃, an extrusion speed of 10mm / s, and an extrusion ratio of 10:1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling. The ingot preheating temperature in step S5 is 730℃, and the holding time is 35min. The extrusion die is preheated in stages, first held at 230℃ for 10min, and then held at 380℃ for 14.5min. The nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 15μm. The cooling rate is controlled at 18℃ / min.
[0040] The total rolling rate of the cold rolling finishing in step S6 is 45%, with the rolling rate of each pass controlled at 10% and an interval of 8 minutes between adjacent passes; after each pass of rolling, gentle grinding and cleaning are performed, and finally, precision straightening is performed; the cold rolling temperature of the cold rolling finishing in step S6 is 23℃, and it is completed in 4 passes with an interval of 8 minutes between adjacent passes; the gradient aging heat treatment in step S7 is specifically as follows: sequentially holding at 430℃ for 4 hours, holding at 335℃ for 1.3 hours, and holding at 235℃ for 2.5 hours, and finally cooling to room temperature at a rate of 2.5℃ / min.
[0041] The gradient alloy layer described in step S8 is deposited by ion beam sputtering, with a thickness of 50-60 nm. It is a silver-copper-La gradient alloy layer, and the gradient distribution is as follows: the outermost layer alloy composition is 85 wt% Ag, 0.5 wt% La, and 14.5 wt% Cu by weight percentage; the innermost layer alloy composition is 5 wt% Ag, 0.1 wt% La, and 94.9 wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85 wt% to 5 wt%, the La content decreases uniformly from 0.5 wt% to 0.1 wt%, and the copper content increases uniformly from 14.5 wt% to 94.9 wt%.
[0042] Example 4 A method for producing a high-conductivity, high-heat-dissipation copper trench wire includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 940℃, hot pressing pressure 28MPa, heat preservation for 2.8h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0043] The purity of the high-purity electrolytic copper in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 55kHz, power 190W, dispersion time 28min; mechanical ball milling ball-to-material ratio 14:1, rotation speed 380r / min, ball milling time 1.8h; the temperature of the mixed powder is controlled ≤150℃ during dispersion; the copper-alloy element solid composite powder in step S1 includes the following components by weight percentage: Ag 0.23%, Cr 0.09%, Sr 0.025%, Sc 0.11%, Ge 0.045%, Zr 0.14%, with the balance being electrolytic copper and other unavoidable impurities; the purity of the high-purity argon gas is ≥99.999%, and the flow rate is 0.45L / min.
[0044] The parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 5GHz, microwave power 750W, focused spot diameter 9mm, and treatment time 14min. During the treatment, the ingot temperature is controlled to not exceed 300℃. The parameters for the electrical pulse treatment in step S4 are: pulse voltage 1100V, pulse frequency 90Hz, pulse width 90μs, and treatment time 18min. During the treatment, the ingot temperature is controlled to be maintained at 280℃.
[0045] The hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 720℃, an extrusion speed of 11mm / s, and an extrusion ratio of 11:1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling. The ingot preheating temperature in step S5 is 740℃, and the holding time is 38min. The extrusion die is preheated in stages, first held at 240℃ for 11min, and then held at 390℃ for 15.5min. The nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 17μm. The cooling rate is controlled at 19℃ / min.
[0046] The total rolling rate of the cold rolling finishing in step S6 is 48%, with the rolling rate of each pass controlled at 11% and an interval of 9 minutes between adjacent passes. After each pass of rolling, gentle grinding and cleaning are performed, followed by precision straightening. The cold rolling temperature of the cold rolling finishing in step S6 is 24℃, and it is completed in 5 passes with an interval of 9 minutes between adjacent passes. The gradient aging heat treatment in step S7 is specifically as follows: sequentially holding at 435℃ for 4.3h, 345℃ for 1.4h, and 245℃ for 2.8h, and finally cooling to room temperature at a rate of 2.8℃ / min.
[0047] The gradient alloy layer described in step S8 is deposited by ion beam sputtering, with a thickness of 58 nm. It is a silver-copper-La gradient alloy layer, and the gradient distribution is as follows: the outermost layer alloy composition is 85 wt% Ag, 0.5 wt% La, and 14.5 wt% Cu by weight percentage; the innermost layer alloy composition is 5 wt% Ag, 0.1 wt% La, and 94.9 wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85 wt% to 5 wt%, the La content decreases uniformly from 0.5 wt% to 0.1 wt%, and the copper content increases uniformly from 14.5 wt% to 94.9 wt%.
[0048] Example 5 A method for producing a high-conductivity, high-heat-dissipation copper trench wire includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the matrix raw material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr; after the electrolytic copper undergoes three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm; the trace alloying elements undergo grinding and mixing pretreatment, and are ground to a particle size ≤30μm; then the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process; the mixing and dispersion process is carried out entirely under a high-purity argon protective atmosphere; Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 950℃, hot pressing pressure 30MPa, heat preservation for 3h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
[0049] The purity of the high-purity electrolytic copper in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 60kHz, power 200W, dispersion time 30min; mechanical ball milling ball-to-material ratio 15:1, rotation speed 400r / min, ball milling time 2h; the temperature of the mixed powder is controlled ≤150℃ during dispersion; the copper-alloy element solid composite powder in step S1 includes the following components by weight percentage: Ag 0.25%, Cr 0.1%, Sr 0.03%, Sc 0.12%, Ge 0.05%, Zr 0.15%, with the balance being electrolytic copper and other unavoidable impurities; the purity of the high-purity argon gas is ≥99.999%, and the flow rate is 0.5L / min.
[0050] The parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 5.8 GHz, microwave power 800 W, focused spot diameter 10 mm, and treatment time 15 min. During the treatment, the ingot temperature is controlled to not exceed 300 °C. The parameters for the electrical pulse treatment in step S4 are: pulse voltage 1200 V, pulse frequency 100 Hz, pulse width 100 μs, and treatment time 20 min. During the treatment, the ingot temperature is controlled to be maintained at 300 °C. The hot extrusion molding in step S5 adopts a forward extrusion process with an extrusion temperature of 730 °C, an extrusion speed of 12 mm / s, and an extrusion ratio of 12:1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling.
[0051] In step S5, the ingot preheating temperature is 750℃ and the holding time is 40min; the extrusion die is preheated in sections, first held at 250℃ for 12min, and then held at 400℃ for 16min; the nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 18μm; the cooling rate is controlled at 20℃ / min; in step S6, the total rolling rate of the cold rolling finishing is 50%, the rolling rate of each pass is controlled at 12%, and the interval between adjacent passes is 10min; after each pass of rolling, gentle grinding and cleaning are performed, and finally, precision straightening is performed; the cold rolling temperature of the cold rolling finishing in step S6 is 25℃, and it is completed in 5 passes with an interval of 10min between adjacent passes.
[0052] The gradient aging heat treatment in step S7 specifically involves sequentially holding at 440℃ for 4.5h, 350℃ for 1.5h, and 250℃ for 3h, and finally cooling to room temperature at a rate of 3℃ / min. The gradient alloy layer in step S8 is deposited by ion beam sputtering with a thickness of 60nm. It is a silver-copper-La gradient alloy layer with the following gradient distribution: the outermost layer has an alloy composition of 85wt% Ag, 0.5wt% La, and 14.5wt% Cu by weight percentage; the innermost layer has an alloy composition of 5wt% Ag, 0.1wt% La, and 94.9wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85wt% to 5wt%, the La content decreases uniformly from 0.5wt% to 0.1wt%, and the copper content increases uniformly from 14.5wt% to 94.9wt%.
[0053] Comparative Example 1 A method for producing a high-conductivity, high-heat-dissipation copper trench wire is basically the same as that in Example 5, except that directional microwave strong field treatment is used instead of electrical pulse treatment, the treatment time is 20 minutes, and other parameters are the same as those in step S3 for directional microwave strong field treatment.
[0054] Comparative Example 2 A method for producing a high-conductivity, high-heat-dissipation copper trench wire is basically the same as that in Example 5, except that ordinary microwave treatment is used instead of directional microwave strong field treatment. The microwave frequency is 2.45 GHz, the power is 800 W, and the processing time is 15 min.
[0055] Comparative Example 3 A method for producing a high-conductivity, high-heat-dissipation copper trench wire is basically the same as that in Example 5, except that a common alloy layer is used instead of a gradient alloy layer; the thickness is 60nm, and the composition by weight percentage is 85wt% Ag, 0.5wt% La, and 14.5wt% Cu.
[0056] Comparative Example 4 A method for producing a high-conductivity, high-heat-dissipation copper channel wire is basically the same as that in Example 5, except that an equal amount of Cu is used instead of Ge.
[0057] To further illustrate the unexpected positive technical effects achieved by the high conductivity and high heat dissipation copper trench wires manufactured in the embodiments of the present invention, relevant performance tests were conducted on the high conductivity and high heat dissipation copper trench wires of Example 5 and Comparative Examples 1-4. The test results are shown in Table 1, and the test methods are as follows: (1) Conductivity test: Referring to GB / T 32791-2016 "Eddy current test method for conductivity of copper and copper alloys" and GB / T 3048.2-2021 "Test method for electrical properties of wires and cables - Part 2: Resistance measurement", a Keysight 34420A micro-ohmmeter was used to measure the resistivity of the sample at room temperature (25℃) and humidity 50%RH. The conductivity was then calculated based on the resistivity (based on the conductivity of standard pure copper at 100% IACS). Five test points were selected for each sample (three evenly distributed points at both ends and the middle), and the average value was taken as the final test result.
[0058] (2) Thermal conductivity test: The test was conducted in accordance with the national standard GB / T 22588-2008 "Measuring thermal diffusivity or thermal conductivity by flash method". The sample was cut into a circular piece with a diameter of 10 mm and a thickness of 2 mm, and the surface was polished to a smooth finish. The sample was placed in a laser flash thermal conductivity meter, the test temperature was set to 25℃, and nitrogen protection was used. Each sample was tested 3 times, and the average value was taken as the final thermal conductivity, in W / (m·K). (3) Fatigue life test: Refer to the fatigue test of JISZ 2273-1978, and count the number of repetitions until the test piece breaks when the load stress is 500MPa; the diameter of the test piece is 0.5mm; each case uses 3 pieces to carry out the above test, and calculate the average number of repetitions until the groove breaks.
[0059] As can be seen from the test results in Table 1, the copper channel wire prepared in Example 5 of this invention has a conductivity of 98.6% IACS, a thermal conductivity of 365.3 W / (m·K), and a fatigue life of 1.72 × 10⁻⁶. 7Secondly, all three performance indicators are significantly better than those of Comparative Example 1 (without electrical pulse treatment), Comparative Example 2 (with ordinary microwave treatment), Comparative Example 3 (with ordinary homogeneous alloy layer), and Comparative Example 4 (with Ge element replacement). Due to defects in the preparation process, surface structure, and alloy composition, the uniformity of grain structure, grain boundary cleanliness, and interface matching of each comparative example deteriorated, and the electrical conductivity, thermal conductivity, and fatigue resistance all decreased to varying degrees. This fully demonstrates that the present invention, by using directional microwave strong field and electrical pulse composite treatment, optimizing the microalloy formula, and setting a silver-copper-La gradient alloy layer, can synergistically improve the electrical conductivity, heat dissipation performance, and fatigue service life of copper trench wires. Compared with pure copper, it significantly extends the fatigue life while maintaining high electrical conductivity and heat dissipation performance.
[0060] Table 1 Performance test results of high conductivity and high heat dissipation copper trench wire
[0061] The above embodiments are only for illustrating the technical concept and features of the present invention. Their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be used to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for producing a high-conductivity, high-heat-dissipation copper channel wire, characterized in that, Includes the following steps: Step S1, Pretreatment: High-purity electrolytic copper is selected as the base material, and trace alloying elements are added; the trace alloying elements include Ag, Cr, Sr, Sc, Ge, and Zr. After electrolytic copper undergoes a three-stage purification and drying pretreatment, it is ground into copper powder with a particle size ≤50μm. Trace alloying elements are ground and mixed pretreatment, and ground to a particle size ≤30μm. Subsequently, the copper powder and trace alloying element powder are mixed evenly, and a copper-alloying element solid composite powder is prepared by ultrasonic dispersion-mechanical ball milling synergistic process. The mixing and dispersion process is carried out in a high-purity argon protective atmosphere throughout. Step S2, Vacuum Hot Pressing and Ingot Preparation: The dispersed copper-alloy element solid composite powder is placed in a vacuum hot press furnace, and a solid composite process is adopted, controlling the vacuum degree to ≤1×10. -5 Pa, hot pressing temperature 850~950℃, hot pressing pressure 20~30MPa, heat preservation for 2~3h; after the ingot is prepared, its surface is ground and polished. Step S3, Directional Microwave Intensity Field Treatment: Place the polished copper alloy ingot into the directional microwave intensity field treatment equipment, introduce high-purity argon gas as a protective gas, and perform directional focused microwave intensity field treatment. Step S4, Electrical pulse treatment: The copper alloy ingot after directional microwave strong field treatment is transferred into the electrical pulse treatment equipment, and high-purity argon gas is continuously introduced as a protective gas to maintain a continuous protective atmosphere for electrical pulse treatment. Step S5, Hot Extrusion Molding: The copper alloy ingot after electrical pulse treatment and the extrusion die are preheated and then hot extruded. Step S6, Cold Rolling Finishing: Perform multiple cold rolling finishing passes on the cooled billet; Step S7, Gradient heat treatment: Place the copper channel wire semi-finished product into an atmosphere-protected heat treatment furnace, introduce high-purity argon gas for protection, and adopt a four-stage gradient aging heat treatment. Step S8, Surface Treatment: Perform a double-layer treatment on the heat-treated copper channel line, including bottom cleaning and gradient alloy layer deposition.
2. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The purity of the high-purity electrolytic copper mentioned in step S1 is ≥99.9995%; the ultrasonic dispersion-mechanical ball milling synergistic process parameters in step S1 are as follows: ultrasonic dispersion frequency 40~60kHz, power 150~200W, dispersion time 20~30min; mechanical ball milling ball-to-material ratio (10~15):1, rotation speed 300~400r / min, ball milling time 1~2h; the temperature of the mixed powder is controlled ≤150℃ during the dispersion process.
3. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The copper-alloy element solid composite powder mentioned in step S1 comprises the following components by weight percentage: Ag 0.13-0.25%, Cr 0.05-0.1%, Sr 0.01-0.03%, Sc 0.08-0.12%, Ge 0.03-0.05%, Zr 0.1-0.15%, with the balance being electrolytic copper and other unavoidable impurities; the high-purity argon gas has a purity ≥99.999% and a flow rate of 0.3~0.5L / min.
4. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The parameters for the directional focusing microwave strong field treatment in step S3 are: microwave frequency 2.45~5.8GHz, microwave power 500~800W, focused spot diameter 5~10mm, and treatment time 8~15min. During the treatment, the ingot temperature is controlled to not exceed 300℃. The parameters for the electrical pulse treatment in step S4 are: pulse voltage 800~1200V, pulse frequency 50~100Hz, pulse width 50~100μs, and treatment time 10~20min. During the treatment, the ingot temperature is controlled to be maintained at 200~300℃.
5. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The hot extrusion molding described in step S5 adopts a forward extrusion process with an extrusion temperature of 690~730℃, an extrusion speed of 8~12mm / s, and an extrusion ratio of (8~12):
1. The extrusion die cavity is an arc-shaped transition groove, and the cavity surface is sprayed with nano-graphite lubricant. After extrusion, it is cooled to room temperature by air cooling. The ingot preheating temperature described in step S5 is 700~750℃, and the holding time is 30~40min. The extrusion die is preheated in stages, first held at 200~250℃ for 8-12min, and then held at 350~400℃ for 13-16min.
6. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 5, characterized in that, The nano-graphite lubricant has a particle size ≤50nm and a coating thickness of 12~18μm; the cooling rate is controlled at 15~20℃ / min.
7. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The total rolling rate of the cold rolling finishing in step S6 is 40-50%, the rolling rate of each pass is controlled at 8-12%, and the interval between adjacent passes is 5-10 minutes; after each pass of rolling, gentle grinding and cleaning are performed, and finally precision straightening is performed; the cold rolling temperature of the cold rolling finishing in step S6 is 20-25℃, and it is completed in 4-5 passes with an interval of 5-10 minutes between adjacent passes.
8. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The gradient aging heat treatment described in step S7 is as follows: sequentially holding at 420~440℃ for 3.5~4.5h, at 320~350℃ for 1~1.5h, at 220~250℃ for 2~3h, and finally cooling to room temperature at a rate of 2~3℃ / min.
9. The method for producing high-conductivity, high-heat-dissipation copper channel wire according to claim 1, characterized in that, The gradient alloy layer described in step S8 is deposited by ion beam sputtering, with a thickness of 50-60 nm. It is a silver-copper-La gradient alloy layer, and the gradient distribution is as follows: the outermost layer alloy composition is 85 wt% Ag, 0.5 wt% La, and 14.5 wt% Cu by weight percentage; the innermost layer alloy composition is 5 wt% Ag, 0.1 wt% La, and 94.9 wt% Cu by weight percentage; from the surface to the substrate, the silver content decreases uniformly from 85 wt% to 5 wt%, the La content decreases uniformly from 0.5 wt% to 0.1 wt%, and the copper content increases uniformly from 14.5 wt% to 94.9 wt%.
10. A high-conductivity, high-heat-dissipation copper channel wire produced by the production method of the high-conductivity, high-heat-dissipation copper channel wire according to any one of claims 1-9.