Foamed polymeric lightweight concrete for road construction and method for its production
By using benzalkonium chloride, tetraoctylammonium bromide, isomeric decaol ether compound additives and early strength reinforcing composite foaming agent in foamed lightweight concrete, the problem of uneven dispersion of dry soil and cement was solved, achieving uniform strength distribution and structural stability of lightweight concrete, and improving the quality and economic benefits of road construction.
Patent Information
- Application Number
- CN202610634396.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-09
- Publication Date
- 2026-07-10
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of road construction materials, and in particular to a foamed polymer lightweight concrete for road construction and its preparation method. Background Technology
[0002] With the continuous acceleration of the development of comprehensive national strength, the traffic volume on expressways has also been increasing. The demand for traffic has far exceeded the original construction expectations, and the traffic capacity of expressways has been declining year by year, failing to meet the needs of development. Upgrading and renovating existing expressways has become an important way to improve the functionality of expressways and meet traffic capacity requirements. Foamed lightweight soil is a new type of material developed in recent years. It mainly uses cement-based binders and admixtures as the main binders, adding additives and water to form a slurry. This slurry is then mixed with a certain proportion of small, stable air bubbles to form a fluid, which is then poured and cured on-site to create a lightweight concrete material containing a large number of tiny, independent, and uniformly distributed air bubbles. This material has advantages such as light weight, good fluidity, high strength, stable performance, strong uprightness, and low environmental impact. In 1986, foamed lightweight soil was first used as road fill in the Ichino Ward of the Hachinohe Line on the Tohoku Highway in Japan, reducing the load, shortening the construction period, and effectively controlling road landslides. In 1988, 27,000 m³ of foamed lightweight soil was poured as a roadbed in the Dorkland area of London, England, reducing the superstructure load, effectively controlling road settlement, and minimizing the impact on surrounding buildings. In 2010, as foamed lightweight soil technology matured, Japan applied the material to the runway of Tokyo Airport, which shortened the construction period and reduced settlement.
[0003] However, because dry soil is used as filler in foamed lightweight soil, it has higher hygroscopicity compared to sand and gravel used in traditional concrete. Moreover, dry soil has higher viscosity during the mixing process with water, making it difficult to evenly disperse dry soil and cement. As a result, lightweight concrete using dry soil as filler is prone to uneven strength distribution due to uneven distribution of filler and cementitious materials. Under continuous pouring, local weak areas are likely to appear, causing the constructed road structure to be prone to damage in these weak areas and failing to meet usage requirements. Therefore, there is still room for improvement. Summary of the Invention
[0004] In order to make the strength distribution of foamed polymer lightweight concrete more uniform and reduce the defects of local weak areas, this application provides a foamed polymer lightweight concrete for road construction and its preparation method.
[0005] In a first aspect, this application provides a foamed polymer lightweight concrete for road construction, employing the following technical solution: A foamed polymer lightweight concrete for road construction is formed by curing and solidifying a foamed polymer lightweight concrete mix for road construction. The foamed polymer lightweight concrete mix for road construction comprises the following components in parts by weight: 249-251 parts cement; 443-447 parts water; 380-390 parts dry soil; 310-320 parts of foaming agent; 18-21 parts of auxiliary agents; The auxiliary agent is a compound of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether.
[0006] By adopting the above technical solution and adding an additive composed of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether, the cement and dry soil can be fully and evenly mixed, and the dispersibility is greatly improved. This results in a uniform strength distribution of the cured lightweight concrete, making it less prone to local weak points and reducing the risk of local structural damage. At the same time, benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether also help the foaming agent to be evenly dispersed in the mixture, resulting in a more uniform distribution of air bubbles after curing, and thus a more uniform strength distribution of the lightweight concrete.
[0007] Preferably, the mass ratio of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether in the auxiliary agent is 6-7:5-6:7-8.
[0008] By adopting the above technical solution and specifically selecting the mass ratio of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether, the effect of improving the dispersion uniformity of each component is better, resulting in a more uniform strength distribution of lightweight concrete. Furthermore, after benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether are compounded in a special ratio, the strength of lightweight concrete can be further improved, and the resulting engineering structure is more durable.
[0009] Preferably, the cement is ordinary Portland cement.
[0010] By adopting the above technical solutions and using ordinary silicate cement, the resulting lightweight concrete structures exhibit better durability and more stable quality.
[0011] Preferably, the moisture content of the dry soil is ≤5%.
[0012] By adopting the above technical solutions and controlling the moisture content of the dry soil, the proportions of each component can be better guaranteed, resulting in higher quality lightweight concrete.
[0013] Preferably, the foaming agent is an early-strength reinforced composite foaming agent.
[0014] By adopting the above technical solution and using an early-strength reinforced composite foaming agent, the early strength of lightweight concrete is effectively improved, making the foam group less prone to collapse and better ensuring the structural stability of lightweight concrete.
[0015] Secondly, this application provides a method for preparing foamed polymer lightweight concrete for road construction, employing the following technical solution: A construction method for the above-mentioned foamed polymer lightweight concrete used in road construction includes the following steps: Step 1), mix dry soil, water and additives evenly to obtain premix; Step 2) Add cement and foaming agent to the premix, mix evenly, and obtain foamed polymer lightweight concrete mix for road construction; Step 3) Pour the foamed polymer lightweight concrete mix for road construction into the mold, cure, and demold to obtain the foamed polymer lightweight concrete for road construction.
[0016] By adopting the above technical solution, the components of the lightweight concrete are evenly dispersed, the strength distribution is relatively uniform and the strength is high, which can well meet the needs of road construction, effectively reduce costs while ensuring project quality.
[0017] Preferably, in step 1), dry soil, water, and additives are added to a mixing device and mixed for 1-2 hours to obtain a premix.
[0018] By adopting the above technical solution, the dry soil, water and additives are mixed for 1-2 hours, so that the modification effect of the additives on the dry soil is more sufficient, thereby effectively improving the dispersion uniformity of cement and dry soil, better improving the distribution uniformity of the strength of lightweight concrete, and reducing the risk of local damage to lightweight concrete.
[0019] Thirdly, this application provides an application of foamed polymer lightweight concrete for road construction, employing the following technical solution: An application of the above-mentioned foamed polymer lightweight concrete for road construction, wherein the foamed polymer lightweight concrete for road construction is used to prepare roadbeds or embankments.
[0020] By adopting the above technical solutions, the resulting roadbeds and embankments can well meet the requirements of road engineering standards and significantly reduce costs, thus possessing considerable economic value.
[0021] In summary, this application has the following beneficial effects: 1. Because this application adds an additive composed of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether, the cement and dry soil can be fully and evenly mixed, and the dispersibility is greatly improved. This results in a uniform strength distribution of the cured lightweight concrete, making it less prone to local weak points and reducing the risk of local structural damage. At the same time, benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether also help the foaming agent to be evenly dispersed in the mixture, resulting in a more uniform distribution of air bubbles after curing, and thus a more uniform strength distribution of the lightweight concrete.
[0022] 2. In this application, it is preferred to improve the dispersion uniformity of each component by specifically selecting the mass ratio of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether, which makes the strength distribution of lightweight concrete more uniform. Furthermore, after benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether are compounded in a special ratio, the strength of lightweight concrete can be further improved, and the resulting engineering structure is more durable. Detailed Implementation
[0023] The present application will be further described in detail below with reference to the embodiments.
[0024] Example 1
[0025] A foamed polymer lightweight concrete for road construction, the construction method includes the following steps: Step 1): Add 380 kg of dry soil, 443 kg of water, 6 kg of benzalkonium chloride, 5 kg of tetraoctylammonium bromide, and 7 kg of isomeric decaol ether into a mixer and stir at 100 r / min for 1-2 h to obtain a premix.
[0026] Step 2): Add 249 kg of cement and 310 kg of foaming agent to the premix, stir at 100 r / min for 5-10 min to obtain foamed polymer lightweight concrete mix for road construction.
[0027] Step 3) Pour the foamed polymer lightweight concrete mix for road construction into the mold, allow it to cure statically for 24 hours, then water it for 48 hours, demold it, and allow it to cure statically for 28 days to obtain the foamed polymer lightweight concrete for road construction.
[0028] The dry soil is ordinary loess with a moisture content of ≤5%.
[0029] Benzalkonium chloride was purchased from Shandong Guohua Chemical Co., Ltd., CAS No.: 8001-54-5, purity 99%.
[0030] Tetraoctylammonium bromide was purchased from Tiancheng Chemical (Jiangsu) Co., Ltd., CAS No.: 14866-33-2, purity 99%.
[0031] The isomeric deca-ol ether was purchased from Haian Petrochemical Plant in Jiangsu Province, CAS No.: 61827-42-7, purity 99%.
[0032] The cement was purchased from Guangdong Shengrui Technology Co., Ltd., model: SRJ001, ordinary Portland cement, PO42.5 cement.
[0033] The foaming agent was purchased from Guangdong Shengrui Technology Co., Ltd., model: M32.
[0034] Example 2
[0035] A foamed polymer lightweight concrete for road construction, the construction method includes the following steps: Step 1): Add 388 kg of dry soil, 445 kg of water, 6.5 kg of benzalkonium chloride, 5.5 kg of tetraoctylammonium bromide, and 7.5 kg of isomeric decaol ether into a mixer and stir at 100 r / min for 1-2 hours to obtain a premix.
[0036] Step 2) Add 250kg of cement and 316kg of foaming agent to the premix, stir at 100r / min for 5-10min to obtain foamed polymer lightweight concrete mix for road construction.
[0037] Step 3) Pour the foamed polymer lightweight concrete mix for road construction into the mold, allow it to cure statically for 24 hours, then water it for 48 hours, demold it, and allow it to cure statically for 28 days to obtain the foamed polymer lightweight concrete for road construction.
[0038] The dry soil is ordinary loess with a moisture content of ≤5%.
[0039] Benzalkonium chloride was purchased from Shandong Guohua Chemical Co., Ltd., CAS No.: 8001-54-5, purity 99%.
[0040] Tetraoctylammonium bromide was purchased from Tiancheng Chemical (Jiangsu) Co., Ltd., CAS No.: 14866-33-2, purity 99%.
[0041] The isomeric deca-ol ether was purchased from Haian Petrochemical Plant in Jiangsu Province, CAS No.: 61827-42-7, purity 99%.
[0042] The cement was purchased from Guangdong Shengrui Technology Co., Ltd., model: SRJ001, ordinary Portland cement, PO42.5 cement.
[0043] The foaming agent was purchased from Guangdong Shengrui Technology Co., Ltd., model: M32.
[0044] Example 3
[0045] A foamed polymer lightweight concrete for road construction, the construction method includes the following steps: Step 1): Add 390 kg of dry soil, 447 kg of water, 7 kg of benzalkonium chloride, 6 kg of tetraoctylammonium bromide, and 8 kg of isomeric decaol ether into a mixer and stir at 100 r / min for 1-2 h to obtain a premix.
[0046] Step 2) Add 251kg of cement and 320kg of foaming agent to the premix, stir at 100r / min for 5-10min to obtain foamed polymer lightweight concrete mix for road construction.
[0047] Step 3) Pour the foamed polymer lightweight concrete mix for road construction into the mold, allow it to cure statically for 24 hours, then water it for 48 hours, demold it, and allow it to cure statically for 28 days to obtain the foamed polymer lightweight concrete for road construction.
[0048] The dry soil is ordinary loess with a moisture content of ≤5%.
[0049] Benzalkonium chloride was purchased from Shandong Guohua Chemical Co., Ltd., CAS No.: 8001-54-5, purity 99%.
[0050] Tetraoctylammonium bromide was purchased from Tiancheng Chemical (Jiangsu) Co., Ltd., CAS No.: 14866-33-2, purity 99%.
[0051] The isomeric deca-ol ether was purchased from Haian Petrochemical Plant in Jiangsu Province, CAS No.: 61827-42-7, purity 99%.
[0052] The cement was purchased from Guangdong Shengrui Technology Co., Ltd., model: SRJ001, ordinary Portland cement, PO42.5 cement.
[0053] The foaming agent was purchased from Guangdong Shengrui Technology Co., Ltd., model: M32.
[0054] Comparative Example 1 A foamed polymer lightweight concrete for road construction, differing from Example 2 only in that: Hexadecyltrimethylammonium bromide was used to replace benzalkonium chloride in an equal amount.
[0055] Hexadecyltrimethylammonium bromide was purchased from Wuhan Prof Biotechnology Co., Ltd.
[0056] Comparative Example 2 A foamed polymer lightweight concrete for road construction, differing from Example 2 only in that: Tetraoctylammonium bromide was replaced in equal amounts with dodecylmethyl tertiary amine.
[0057] The didodecylmethyl tertiary amine was purchased from Kunshan Aichao Biotechnology Co., Ltd.
[0058] Comparative Example 3 A foamed polymer lightweight concrete for road construction, differing from Example 2 only in that: Stearamide dimethylamine was used to replace the isomeric decaol ether in equal amounts.
[0059] Stearamide dimethylamine was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.
[0060] Comparative Example 4 A foamed polymer lightweight concrete for road construction, differing from Example 2 only in that: Hexadecyltrimethylammonium bromide was used to replace benzalkonium chloride in equal amounts, didodecylmethyl tertiary amine was used to replace tetraoctylammonium bromide in equal amounts, and stearamide dimethylamine was used to replace isomeric decaol ether in equal amounts.
[0061] Hexadecyltrimethylammonium bromide was purchased from Wuhan Prof Biotechnology Co., Ltd.
[0062] The didodecylmethyl tertiary amine was purchased from Kunshan Aichao Biotechnology Co., Ltd.
[0063] Stearamide dimethylamine was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.
[0064] Experiment 1 According to the requirements of GBT50080-2016 "Standard for Test Methods of Performance of Ordinary Concrete Mixtures", test samples were prepared for the foamed polymer lightweight concrete mixes used for road construction in each embodiment and comparative example. The same batch of mixes was used for all foamed polymer lightweight concrete mixes used for road construction in each embodiment and comparative example. 100 test samples were prepared for each embodiment and comparative example.
[0065] The 28-day compressive strength of the test sample was tested according to GBT50080-2016 "Standard for Test Methods of Performance of Ordinary Concrete Mixture". The average value and coefficient of variation of the 28-day compressive strength of each example and comparative example were calculated based on 100 experimental data from each example and comparative example.
[0066] The detailed experimental data for Experiment 1 are shown in Table 1.
[0067] Table 1
[0068] According to the data in Table 1, the average compressive strength of each embodiment is higher than that of the comparative examples. This shows that the addition of additives such as benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether can improve the strength of lightweight concrete to a certain extent. At the same time, the coefficient of variation of the compressive strength of each embodiment is significantly lower than that of the comparative examples. This indicates that the strength distribution of the comparative examples is uneven, which easily leads to local weak areas and thus the pavement structure is prone to local damage, resulting in an increased frequency of pavement maintenance. In contrast, the strength distribution of each embodiment is more uniform, and the overall average strength fully meets the pavement structure construction standards. The pavement structure produced is less prone to local weak areas, thus making the pavement structure less susceptible to damage, significantly reducing the frequency of maintenance, and having higher economic value.
[0069] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A foamed polymer lightweight concrete for road construction, characterized in that: It is made from foamed polymer lightweight concrete mix used in road construction, which is then cured and solidified. The foamed polymer lightweight concrete mix for road construction comprises the following components in parts by weight: 249-251 parts cement; 443-447 parts water; 380-390 parts dry soil; 310-320 parts of foaming agent; 18-21 parts of auxiliary agents; The auxiliary agent is a compound of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether.
2. The foamed polymer lightweight concrete for road construction according to claim 1, characterized in that: In the aforementioned additives, the mass ratio of benzalkonium chloride, tetraoctylammonium bromide, and isomeric decaol ether is 6-7:5-6:7-8.
3. The foamed polymer lightweight concrete for road construction according to claim 2, characterized in that: The cement is ordinary Portland cement.
4. The foamed polymer lightweight concrete for road construction according to claim 3, characterized in that: The moisture content of the dry soil is ≤5%.
5. The foamed polymer lightweight concrete for road construction according to claim 4, characterized in that: The foaming agent is an early-strength reinforced composite foaming agent.
6. A construction method for foamed polymer lightweight concrete for road construction according to any one of claims 1-5, characterized in that: Includes the following steps: Step 1), mix dry soil, water and additives evenly to obtain premix; Step 2) Add cement and foaming agent to the premix, mix evenly, and obtain foamed polymer lightweight concrete mix for road construction; Step 3) Pour the foamed polymer lightweight concrete mix for road construction into the mold, cure, and demold to obtain the foamed polymer lightweight concrete for road construction.
7. A construction method for foamed polymer lightweight concrete for road construction according to claim 6, characterized in that: In step 1), dry soil, water, and additives are added to a mixing device and mixed for 1-2 hours to obtain a premix.
8. An application of the foamed polymer lightweight concrete for road construction according to claims 1-5, characterized in that: The foamed polymer lightweight concrete used in road construction is used to prepare roadbeds or embankments.